Conductive substrate coating for lithium ion battery and preparation method of conductive substrate coating
Through the combination of graphene modified polyurethane and methacrylic silane coupling agent, the thermal runaway problem of lithium-ion battery conductive coating under extreme conditions is solved, the adhesive performance and compatibility of the coating are improved, and the battery is extended life.
Patent Information
- Application Number
- CN202411038273.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-07-31
AI Technical Summary
Existing lithium-ion battery conductive coatings are prone to thermal runaway under extreme conditions such as high temperature, overcharging, and overdischarge, leading to dispersion and compatibility of conductive agents, and performance defects such as battery short circuits.
Graphene modified polyurethane is used as the binder and methacrylic silane coupling agent is used as the compatible agent. The bonding performance of the coating and the compatibility of inorganic fillers are improved through compounding technology to form a stable crosslinking structure.
It significantly improves the bonding performance and compatibility of the conductive coating of lithium-ion batteries, avoids thermal expansion and fall off of the coating, extends the cycle life of the battery, and enhances the stability of the battery.
Smart Images

Figure BDA0004971700240000091 
Figure BDA0004971700240000101
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of lithium ion battery conductive coatings, and in particular to a conductive base coating for lithium ion batteries and a preparation method thereof. Background Art
[0002] Lithium-ion batteries are generally batteries that use lithium alloy metal oxides as positive electrode materials, graphite as negative electrode materials, and non-aqueous electrolytes. They are secondary batteries (rechargeable batteries) that mainly rely on the movement of lithium ions between the positive and negative electrodes to perform charging and discharging. Due to this excellent charging and discharging capability, they are widely used in consumer electronics, electric vehicles and transportation, energy storage, aerospace, medical equipment, military and security fields, etc.
[0003] Existing lithium-ion batteries have been significantly improved in terms of energy density, memory effect, self-discharge, cycle life, etc., but the conductive coating on the surface of the battery still has certain defects in performance. For example, the invention patent with application number CN201410238020.2 provides a conductive coating and its preparation method, a lithium-ion battery positive electrode sheet and its preparation method, and a lithium-ion battery. By preparing a resin containing a carboxylic acid group as a binder, the resin containing a carboxylic acid group can produce a carboxylic acid ammonium salt structure with strong hydrophilicity during the neutralization process with ammonia water, which improves the adhesion and reduces the internal resistance of the electrode. However, there is a serious and unresolved problem of the dispersion of the conductive agent in this technology. For example, the patent with application number 202310988730.6 discloses a conductive coating for lithium-ion batteries and its preparation method. In this technical solution, four acrylic resins are used for compounding to improve the bonding ability of the coating, but the compatibility problem between inorganic fillers and binders in the conductive base coating of lithium-ion batteries is still not solved. Lithium-ion batteries are prone to thermal runaway under extreme conditions such as high temperature, overcharging, and over-discharging, which reduces the compatibility of the binder and inorganic filler in the coating, causes thermal expansion and shedding of the surface coating of the conductive coating, accelerates coating aging, and causes battery short circuits.
[0004] Based on this, there is an urgent need for a lithium-ion battery conductive base coating with good compatibility and adhesion to avoid damage to the lithium-ion battery caused by defects in the coating performance. Summary of the invention
[0005] The purpose of the present invention is to provide a conductive base coating for lithium ion batteries with good bonding performance and a preparation method thereof.
[0006] In order to achieve the above-mentioned purpose, the present invention provides the following technical scheme: a conductive base coating for lithium-ion batteries, comprising at least the following components in parts by mass: 45-60 parts of a binder, 15-30 parts of a conductive inorganic filler, 180-240 parts of an organic solvent, 1.5-3 parts of a dispersant, and 0.6-2.8 parts of a compatibilizer, wherein the binder comprises at least polyurethane, and the compatibilizer is a methacrylate silane coupling agent.
[0007] As a preferred technical solution, the polyurethane is graphene-modified polyurethane.
[0008] As a preferred technical solution, the method for modifying polyurethane with graphene comprises at least the following steps:
[0009] (1) adding graphene to a solvent and mixing them uniformly to obtain a dispersion A;
[0010] (3) adding polyurethane to dispersion A and mixing evenly to obtain dispersion B;
[0011] (3) Sodium dodecylbenzene sulfonate and methacrylate silane coupling agent are added to the dispersion B and mixed evenly to obtain the dispersion.
[0012] As a preferred technical solution, the raw materials for preparing the polyurethane include polyether carbonate polyol, isocyanate prepolymer and polyisocyanate, the polyether carbonate polyol has a functionality of 2 to 4, a hydroxyl value of 50-60 mgKOH / g, a mass percentage of CO2 of 5 to 35%, and a mass ratio between the isocyanate prepolymer and the polyisocyanate of 1 to 3:1.
[0013] As a preferred technical solution, the isocyanate prepolymer and polyisocyanate are obtained by modifying hollow glass microspheres and silicon dioxide, and the mass ratio of the hollow glass microspheres to silicon dioxide is 2 to 5:1.
[0014] As a preferred technical solution, the NCO content of the polyisocyanate is 10-20%.
[0015] As a preferred technical solution, the method for preparing the polyurethane comprises at least the following steps:
[0016] (1) preparing component A: adding 15 to 50 parts of polyether carbonate polyol and 5 to 10 parts of chain extender by weight, and stirring to obtain component A;
[0017] (2) preparing component B: adding 30 to 70 parts of isocyanate prepolymer, 6 to 28 parts of polyisocyanate, 5 to 25 parts of hollow glass microspheres, 0.1 to 2 parts of fumed silica, and 0.1 to 0.5 parts of dehydrating agent by weight, stirring evenly, and then discharging the material to obtain component B; wherein the isocyanate prepolymer is prepared by reacting polyether carbonate polyol and polyisocyanate in a mass ratio of 1:0.5 to 2;
[0018] (3) Component A and component B are uniformly mixed in a volume ratio of 1:0.8-1.5 to obtain polyurethane.
[0019] As a preferred technical solution, the conductive inorganic filler is a mixture of modified graphite fiber and modified graphene, the mass ratio of the modified graphite fiber to the modified graphene is 1-3:10-15, and the modified graphite fiber and modified graphene are obtained by modifying graphite fiber and graphene with an organosilicon coupling agent.
[0020] As a preferred technical solution, the solvent in the method for modifying polyurethane with graphene is at least one of dimethyl sulfoxide, N-methylpyrrolidone and N-methylpyridine.
[0021] As a preferred technical solution, in the method for modifying polyurethane with graphene, the solvent is a mixture of dimethyl sulfoxide and N-methylpyrrolidone, and the mass ratio between the dimethyl sulfoxide and N-methylpyrrolidone is 3:1.
[0022] As a preferred technical solution, the conductive inorganic filler is a mixture of graphite fiber and graphene, and the mass ratio of the graphite fiber to the graphene is 1-3:10-15.
[0023] As a preferred technical solution, the dispersant is selected from at least one of sodium lignin sulfonate, sodium fatty alcohol polyoxyethylene ether sulfate, sodium polyacrylate and potassium polyacrylate.
[0024] As a preferred technical solution, the organic solvent is at least one of dimethylformamide, acetone and ethyl acetate.
[0025] As a preferred technical solution, the organic solvent is a mixture of dimethylformamide, acetone and ethyl acetate, and the mass ratio of dimethylformamide, acetone and ethyl acetate is 1-2:1-2:3-5.
[0026] A method for preparing the above-mentioned conductive base coating for lithium ion batteries comprises at least the following steps:
[0027] (1) After weighing the binder and the organic solvent, mix them and stir them evenly;
[0028] (2) Adding the conductive inorganic filler, dispersant and compatibilizer to the mixture prepared in step (1), and performing ultrasonication and stirring until a uniform mixture is obtained.
[0029] Beneficial Effects
[0030] The present invention provides a conductive base coating for lithium ion batteries and a preparation method thereof. The present invention compounds multiple components to synergistically enhance the performance. The conductive performance of the coating can be improved by using graphene-modified polyurethane. The inventors have found that in the system of the present invention, polyurethane is used as a binder and a methacrylate silane coupling agent is used as a compatibilizer. The carboxyl group in the methacrylate silane forms a stable chemical bond with the amino and hydroxyl functional groups of the polyurethane, and the methacrylate silane can form a cross-linked structure with graphite fibers and graphene inorganic fillers in the polyurethane, thereby further enhancing the bonding performance of the coating and improving the compatibility with the inorganic filler. DETAILED DESCRIPTION
[0031] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0032] Example 1
[0033] A conductive base coating for a lithium ion battery in this embodiment includes the following components in parts by mass: 45 parts of a binder, 15 parts of a conductive inorganic filler, 180 parts of an organic solvent, 1.5 parts of a dispersant, and 0.6 parts of a compatibilizer, wherein the binder is graphene-modified polyurethane, the compatibilizer is a methacrylate silane coupling agent, the conductive inorganic filler is a mixture of organic silicon coupling agent-modified graphite fiber and organic silicon coupling agent-modified graphene, the mass ratio between the graphite fiber and the graphene is 1:14, the dispersant is sodium lignin sulfonate, and the organic solvent is a mixture of dimethylformamide, acetone and ethyl acetate, and the mass ratio between the dimethylformamide, acetone and ethyl acetate is 1:1:5.
[0034] In parts by mass, the method for graphene-modified polyurethane comprises the following steps:
[0035] (1) adding 3 parts of graphene to a mixed solvent consisting of 30 parts of dimethyl sulfoxide and 10 parts of N-methylpyrrolidone and mixing them uniformly to obtain a dispersion A;
[0036] (3) adding polyurethane to dispersion A and mixing evenly to obtain dispersion B;
[0037] (3) Add 0.1 parts of sodium dodecylbenzene sulfonate and 0.1 parts of methacrylate silane coupling agent to the dispersion B and mix well to obtain the dispersion.
[0038] The preparation method of the polyurethane comprises the following steps:
[0039] (1) Preparation of component A: adding 15 parts of polyether carbonate polyol and 5 parts of chain extender by weight, stirring to obtain component A, wherein the polyether carbonate polyol has a functionality of 3, a hydroxyl value of 57 mgKOH / g, a CO2 mass percentage of 9.4%, a brand of PCE-3015E, purchased from Zhejiang Huangma New Materials Co., Ltd., and the chain extender is propylene glycol;
[0040] (2) Preparation of component B: adding 30 parts by weight of isocyanate prepolymer, 6 parts of polyisocyanate, wherein the NCO content of the polyisocyanate is 13.4%, purchased from Jintao Chemical Industry, brand MDILL, 5 parts of hollow glass microspheres, 0.1 parts of fumed silica, and 0.1 parts of a desiccant, wherein the desiccant is alumina, and stirring well to obtain component B; wherein the isocyanate prepolymer is prepared by reacting a polyether carbonate polyol with a polyisocyanate in a mass ratio of 1:2;
[0041] (3) Component A and component B are mixed evenly in a volume ratio of 1:1.5 to obtain polyurethane.
[0042] The conductive inorganic filler is a mixture of modified graphite fiber and modified graphene, and the mass ratio of the modified graphite fiber to the modified graphene is 1:10;
[0043] In parts by mass, the modified graphite fiber and modified graphene are obtained by modifying graphite fiber and graphene with an organosilicon coupling agent, specifically, mixing 1 part of graphite fiber and graphene with 100 parts of a 55wt% ethanol aqueous solution and 0.1 part of an organosilicon coupling agent KH-550, stirring and reacting at 60° C. for 2 hours, filtering to obtain a solid, washing, and drying.
[0044] A method for preparing a conductive base coating for a lithium ion battery comprises the following steps:
[0045] (1) mixing graphene-modified polyurethane with a mixture of dimethylformamide, acetone and ethyl acetate, and stirring the mixture evenly;
[0046] (2) adding the modified graphite fiber and the modified graphene, sodium lignin sulfonate and methacrylate silane coupling agent to the mixture prepared in step (1), and performing ultrasonication and stirring until a uniform mixture is obtained.
[0047] Example 2
[0048] A conductive base coating for a lithium ion battery in this embodiment includes the following components in parts by mass: 60 parts of a binder, 30 parts of a conductive inorganic filler, 240 parts of an organic solvent, 3 parts of a dispersant, and 2.8 parts of a compatibilizer, wherein the binder is graphene-modified polyurethane, the compatibilizer is a methacrylate silane coupling agent, the conductive inorganic filler is a mixture of organic silicon coupling agent-modified graphite fiber and organic silicon coupling agent-modified graphene, the mass ratio between the graphite fiber and the graphene is 1:14, the dispersant is sodium lignin sulfonate, and the organic solvent is a mixture of dimethylformamide, acetone and ethyl acetate, and the mass ratio between the dimethylformamide, acetone and ethyl acetate is 1:1:5.
[0049] In parts by mass, the method for graphene-modified polyurethane comprises the following steps:
[0050] (1) adding 3 parts of graphene to a mixed solvent consisting of 30 parts of dimethyl sulfoxide and 10 parts of N-methylpyrrolidone and mixing them uniformly to obtain a dispersion A;
[0051] (3) adding polyurethane to dispersion A and mixing evenly to obtain dispersion B;
[0052] (3) Add 0.1 parts of sodium dodecylbenzene sulfonate and 0.1 parts of methacrylate silane coupling agent to the dispersion B and mix well to obtain the dispersion.
[0053] The preparation method of the polyurethane comprises the following steps:
[0054] (1) Preparation of component A: adding 15 parts of polyether carbonate polyol and 5 parts of chain extender by weight, stirring to obtain component A, wherein the polyether carbonate polyol has a functionality of 3, a hydroxyl value of 57 mgKOH / g, a CO2 mass percentage of 9.4%, a brand of PCE-3015E, purchased from Zhejiang Huangma New Materials Co., Ltd., and the chain extender is propylene glycol;
[0055] (2) Preparation of component B: adding 30 parts by weight of isocyanate prepolymer, 6 parts of polyisocyanate, wherein the NCO content of the polyisocyanate is 13.4%, purchased from Jintao Chemical Industry, brand MDILL, 5 parts of hollow glass microspheres, 0.1 parts of fumed silica, and 0.1 parts of a desiccant, wherein the desiccant is alumina, and stirring well to obtain component B; wherein the isocyanate prepolymer is prepared by reacting a polyether carbonate polyol with a polyisocyanate in a mass ratio of 1:2;
[0056] (3) Component A and component B are mixed evenly in a volume ratio of 1:1.5 to obtain polyurethane.
[0057] The conductive inorganic filler is a mixture of modified graphite fiber and modified graphene, and the mass ratio of the modified graphite fiber to the modified graphene is 1:10;
[0058] In parts by mass, the modified graphite fiber and modified graphene are obtained by modifying graphite fiber and graphene with an organosilicon coupling agent, specifically, mixing 1 part of graphite fiber and graphene with 100 parts of a 55wt% ethanol aqueous solution and 0.1 part of an organosilicon coupling agent KH-550, stirring and reacting at 60° C. for 2 hours, filtering to obtain a solid, washing, and drying.
[0059] A method for preparing a conductive base coating for a lithium ion battery comprises the following steps:
[0060] (1) mixing graphene-modified polyurethane with a mixture of dimethylformamide, acetone and ethyl acetate, and stirring the mixture evenly;
[0061] (2) adding the modified graphite fiber and the modified graphene, sodium lignin sulfonate and methacrylate silane coupling agent to the mixture prepared in step (1), and performing ultrasonication and stirring until a uniform mixture is obtained.
[0062] Comparative Example 1
[0063] The specific implementation of this comparative example is the same as that of Example 1, except that the binder is graphene-modified polyacrylate, which is purchased from Feiyue Chemical Industry with a brand number of 9003-01-4.
[0064] The method for modifying polyacrylate with graphene comprises the following steps:
[0065] (1) adding 3 parts of graphene to a mixed solvent consisting of 30 parts of dimethyl sulfoxide and 10 parts of N-methylpyrrolidone and mixing them uniformly to obtain a dispersion A;
[0066] (3) adding polyacrylate to dispersion A and mixing evenly to obtain dispersion B;
[0067] (3) Add 0.1 parts of sodium dodecylbenzene sulfonate and 0.1 parts of methacrylate silane coupling agent to the dispersion B and mix well to obtain the dispersion.
[0068] Comparative Example 2
[0069] The specific implementation of this comparative example is the same as that of Example 1, except that the binder is polyurethane.
[0070] Comparative Example 3
[0071] The specific implementation of this comparative example is the same as that of Example 1, except that no compatibilizer is contained.
[0072] Comparative Example 4
[0073] The specific implementation of this comparative example is the same as that of Example 1, except that the polyurethane is commercially available and purchased from Jining Tangyi Chemical Co., Ltd.
[0074] The specific implementation of this comparative example is the same as that of Example 1, except that the mass ratio between the graphite fiber and the graphene is 14:1.
[0075] Comparative Example 6
[0076] The specific implementation of this comparative example is the same as that of Example 1, except that the mass ratio between the modified graphite fiber and the modified graphene is 10:1.
[0077] Performance Testing
[0078] The conductive coatings prepared in Examples 1-2 and Comparative Examples 1-6 were coated on aluminum materials and cured. The samples were subjected to peel strength tests at room temperature, peel strength tests after oven treatment at 60°C for 12 hours, and peel strength tests after immersion in electrolyte at 60°C for 200 hours according to the standard GB / T2792-2014. The specific test results are shown in Table 1 below.
[0079] Table 1 - Conductive coating peel strength performance test
[0080]
[0081]
[0082] It can be seen from the above table that the coatings using the polyurethane adhesive and the methacrylate silane coupling agent compatibilizer in Examples 1 and 2 have better bonding properties.
[0083] The above is a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A conductive base coating for lithium ion batteries, characterized in that: The invention comprises at least the following components in parts by weight: 45-60 parts of a binder, 15-30 parts of a conductive inorganic filler, 180-240 parts of an organic solvent, 1.5-3 parts of a dispersant, and 0.6-2.8 parts of a compatibilizer. The binder comprises at least polyurethane, and the compatibilizer is a methacrylate silane coupling agent.
2. The conductive base coating for lithium ion batteries according to claim 1, characterized in that: The polyurethane is graphene-modified polyurethane.
3. The conductive base coating for lithium ion batteries according to claim 2, characterized in that: The method for modifying polyurethane with graphene comprises at least the following steps: (1) adding graphene to a solvent and mixing them uniformly to obtain a dispersion A; (3) adding polyurethane to dispersion A and mixing evenly to obtain dispersion B; (3) Sodium dodecylbenzene sulfonate and methacrylate silane coupling agent are added to the dispersion B and mixed evenly to obtain the dispersion.
4. The conductive base coating for lithium ion batteries according to claim 3, characterized in that: The raw materials for preparing the polyurethane include polyether carbonate polyol, isocyanate prepolymer and polyisocyanate. The functionality of the polyether carbonate polyol is 2-4, the hydroxyl value is 50-60 mgKOH / g, the mass percentage of CO2 is 5-35%, and the mass ratio between the isocyanate prepolymer and the polyisocyanate is 1-3:
1.
5. The conductive base coating for lithium ion batteries according to claim 4, characterized in that: The isocyanate prepolymer and the polyisocyanate are obtained by modifying hollow glass microspheres and silicon dioxide, and the mass ratio of the hollow glass microspheres to the silicon dioxide is 2-5:
1.
6. The conductive base coating for lithium ion batteries according to claim 5, characterized in that: The NCO content of the polyisocyanate is 10-20%.
7. The conductive base coating for lithium ion batteries according to claim 6, characterized in that: The preparation method of the polyurethane comprises at least the following steps: (1) preparing component A: adding 15 to 50 parts of polyether carbonate polyol and 5 to 10 parts of chain extender by weight, and stirring to obtain component A; (2) preparing component B: adding 30 to 70 parts of isocyanate prepolymer, 6 to 28 parts of polyisocyanate, 5 to 25 parts of hollow glass microspheres, 0.1 to 2 parts of fumed silica, and 0.1 to 0.5 parts of dehydrating agent by weight, stirring evenly, and then discharging the material to obtain component B; wherein the isocyanate prepolymer is prepared by reacting polyether carbonate polyol and polyisocyanate in a mass ratio of 1:0.5 to 2; (3) Component A and component B are uniformly mixed in a volume ratio of 1:0.8-1.5 to obtain polyurethane.
8. The conductive base coating for lithium ion batteries according to claim 5, characterized in that: The conductive inorganic filler is a mixture of modified graphite fiber and modified graphene, the mass ratio of the modified graphite fiber to the modified graphene is 1-3:10-15, and the modified graphite fiber and modified graphene are obtained by modifying graphite fiber and graphene with an organic silicon coupling agent.
9. The conductive base coating for lithium ion batteries according to claim 8, characterized in that: The organic solvent is a mixture of dimethylformamide, acetone and ethyl acetate, and the mass ratio of the dimethylformamide, acetone and ethyl acetate is 1-2:1-2:3-5.
10. A method for preparing the conductive base coating for lithium ion batteries according to claims 1-9, characterized in that: At least the following steps are included: (1) After weighing the binder and the organic solvent, mix them and stir them evenly; (2) Adding the conductive inorganic filler, dispersant and compatibilizer to the mixture prepared in step (1), and performing ultrasonication and stirring until a uniform mixture is obtained.
Citation Information
Patent Citations
Method for preparing graphene / waterborne polyurethane conductive composite material
CN102093700A
Graphene-containing metal surface treatment agent and preparation method of anti-corrosion coating
CN104629603A
Graphene heat-conducting coating and preparation method thereof
CN108300218A
Carbon slurry and electrode for perovskite solar cell
CN108922653A
Graphene modified polyurethane composite material and preparation method thereof
CN114395160A