Preparation method of Pt alloy catalyst with core-shell structure
By loading transition metal nanoparticles on a carbon support and forming a core-shell structure Pt alloy catalyst, the problems of complex and high cost of catalyst preparation process in the prior art are solved, and low-cost, environmentally friendly catalyst preparation and high oxygen are achieved Reducing activity.
Patent Information
- Application Number
- CN202411291545.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-14
- Publication Date
- 2024-11-15
AI Technical Summary
The preparation process of existing hydrogen fuel cell catalysts is complex and costly, and the waste liquid and waste gas generated during batch preparation pollute the environment, increasing energy consumption.
Using the preparation method of core-shell structure Pt alloy catalyst, the core-shell structure Pt alloy catalyst is prepared by supporting transition metal nanoparticles on a carbon support and forming a platinum shell under heat treatment conditions. The replacement reaction is used to generate metal composite nanoparticles, and a core-shell structure Pt alloy catalyst is prepared. .
It has achieved low cost, simple process, low equipment technical requirements, suitable for industrial production, and environmentally friendly. The catalyst has high oxygen reduction activity and good hydrogen adsorption characteristics.
Smart Images

Figure CN118970071A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of electrochemical catalysts, and in particular to a method for preparing a core-shell structured Pt alloy catalyst. Background Art
[0002] As one of the main hydrogen energy application scenarios, hydrogen fuel cells are attracting more and more attention, but various hydrogen energy is still not popularized. One of the main reasons is that the cost of fuel cell stacks remains high, and in the BOM cost of the stack, the catalyst is one of the decisive factors.
[0003] In order to reduce the cost of catalysts in the fuel cell stack, the current mainstream approach is to increase the activity of the catalyst in the fuel cell stack and reduce the amount of Pt. This method is effective. After years of technological development, the amount of Pt on the membrane electrode has been reduced to 0.2 mg / cm 2 However, the existing preparation process has high requirements, the process is complicated, and the expensive chemicals and reagents used make the preparation cost of the catalyst increase instead of decrease. At the same time, the waste liquid and waste gas generated in the batch preparation process not only increase the cost of the catalyst, but also pollute the environment and increase energy consumption. Summary of the invention
[0004] In view of the deficiencies in the prior art, the present invention aims to provide a method for preparing a core-shell structured Pt alloy catalyst.
[0005] In order to achieve the above object, the present invention adopts the following technical solution:
[0006] A method for preparing a core-shell structured Pt alloy catalyst comprises the following steps:
[0007] S1, adding transition metal nanoparticles and carbon carrier into a solvent, stirring and mixing to obtain a mixed solution;
[0008] S2, drying the mixed solution obtained in step S1 to obtain a solid sample;
[0009] S3, heat treating the solid sample obtained in step S2 under a protective atmosphere;
[0010] S4, dispersing the solid sample after the heat treatment in step S3 in a solution saturated with an inert gas, adding a platinum precursor dropwise under magnetic stirring conditions, stirring and filtering after the reaction is complete, and drying the filtered solid;
[0011] S5, heat-treating the solid obtained by drying in step S4 again under a protective atmosphere;
[0012] S6. The solid after the heat treatment in step S5 is acid-washed with H2SO4 solution, and then filtered and washed to obtain a core-shell structure Pt alloy catalyst.
[0013] Furthermore, in step S1, the transition metal nanoparticles are one or more of cobalt nitrate, cobalt chloride, cobalt sulfate, nickel nitrate, nickel chloride, and nickel sulfate; the mass ratio of the carbon carrier to the transition metal nanoparticles is 1:2-10; and the solvent is one or more of water, ethanol, methanol, isopropanol, and ethylene glycol.
[0014] Furthermore, in step S1, ultrasonic dispersion is used to uniformly mix the transition metal nanoparticles and the carbon carrier with the solvent.
[0015] Furthermore, in step S2, the drying treatment is carried out by one or more methods selected from the group consisting of room temperature shade drying, vacuum drying, rotary evaporation drying, and freeze drying.
[0016] Furthermore, in step S3, the protective atmosphere is high-purity hydrogen, hydrogen-argon mixed gas or hydrogen-nitrogen mixed gas, and the volume concentration of the hydrogen is 1%-100%; the temperature of the heat treatment is 400°C-700°C, and the time of the heat treatment is the reaction time of 0.5h-12h.
[0017] Furthermore, the heat treatments in steps S3 and S5 are both performed in a tube furnace.
[0018] Furthermore, in step S4, the inert gas is one or more of nitrogen, argon, and helium; the solution is one or more of water, ethanol, methanol, isopropanol, and ethylene glycol; the platinum precursor includes one or more of chloroplatinic acid, potassium chloroplatinate, sodium chloroplatinate, potassium chloroplatinite, sodium chloroplatinite, platinum acetylacetonate, and platinum nitrate, the molar ratio of platinum to transition metal nanoparticles is 1:0.1-2, the reaction temperature is 10°C-80°C, and the reaction time is 30min-180min.
[0019] Further, in step S5, the protective atmosphere is nitrogen, argon or a hydrogen-argon mixture, and the hydrogen-argon mixture is a 5% H2 / Ar mixture or 10% H2 / Ar; the heat treatment temperature is 400°C-800°C, and the heat treatment time is 1h-6h.
[0020] Further, in step S6, the solid after the heat treatment in step S5 is acid washed with 0.5 mol / L H2SO4 solution at 70°C for 2h-6h.
[0021] The beneficial effect of the present invention is that the method of the present invention first loads the transition metal nanoparticles on the carbon carrier by solid phase reduction, then mixes the sample loaded with the transition metal with the platinum salt, and utilizes the substitution reaction to replace a layer of platinum shell on the surface of the transition metal nanoparticles to form metal composite nanoparticles according to the different activities of the metals, and then adjusts the crystal structure of the composite nanoparticles under heat treatment conditions to prepare a Pt alloy catalyst with a core-shell structure. The method has the characteristics of low cost, simple process, low equipment and technical requirements, conducive to industrialized scale-up production, and green. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 This is a transmission electron microscope image of the core-shell structure Co@Pt / C alloy catalyst obtained in Example 1 of the present invention;
[0023] Figure 2 The XRD diffraction pattern of the core-shell structure Co@Pt / C alloy catalyst obtained in Example 1 of the present invention;
[0024] Figure 3 This is the ECSA diagram of the core-shell structure Co@Pt / C alloy catalyst obtained in Example 1 of the present invention;
[0025] Figure 4 This is the LSV diagram of the core-shell structure Co@Pt / C alloy catalyst obtained in Example 1 of the present invention;
[0026] Figure 5 This is a transmission electron microscopy image of the core-shell structure Co@Pt / C alloy catalyst obtained in Example 2 of the present invention;
[0027] Figure 6 This is the XRD diffraction pattern of the core-shell structure Co@Pt / C alloy catalyst obtained in Example 2 of the present invention. DETAILED DESCRIPTION
[0028] The present invention will be further described below in conjunction with the accompanying drawings. It should be noted that this embodiment is based on the technical solution and provides a detailed implementation method and specific operation process, but the protection scope of the present invention is not limited to this embodiment.
[0029] Example 1
[0030] This embodiment provides a method for preparing a core-shell structured Pt alloy catalyst, the specific process is as follows:
[0031] S1. According to the mass ratio of carbon support to transition metal salt of 1:4.3, 1790.2 mg of transition metal salt cobalt nitrate was added to 200 mL of ethanol, stirred for 10 min, then 418.7 mg of carbon powder was added and ultrasonicated for 40 min to obtain a mixed solution;
[0032] S2, placing the mixed solution in a room temperature environment to dry in the shade, and after forming a solid, drying it in a vacuum drying oven at 50°C;
[0033] S3, placing the dried sample in a tubular furnace, replacing the gas with Ar gas three times, and then replacing it with 5% H2 / Ar mixed gas, heating up at a rate of 5°C / min, sintering the sample at a heat treatment temperature of 550°C and a heat treatment time of 2h, and cooling the sample to room temperature with the furnace after sintering to obtain a solid sample after heat treatment;
[0034] S4, take 82 mg of the solid sample obtained in step S3, disperse it in a pure water solution saturated with N2 gas, add a pure water solution saturated with N2 gas containing 69.7 mg of potassium chloroplatinite according to a molar ratio of platinum to cobalt nitrate of 1:2, react at 30°C for 30 minutes, filter and dry after the reaction is completed;
[0035] S5, placing the sample dried in step S4 in a tubular furnace and replacing the gas with Ar gas three times, and then replacing it with 5% H2 / Ar mixed gas, heating up at a rate of 5°C / min, sintering the sample at a heat treatment temperature of 600°C and a heat treatment time of 2h, and cooling the sample to room temperature with the furnace after sintering to obtain a heat-treated sample;
[0036] S6. The sample after the heat treatment in step S5 is acid-washed with 0.5M H2SO4 solution at 70°C for 2h, then filtered and washed, and dried to obtain the final core-shell structure Pt alloy catalyst.
[0037] Figure 1 This is a transmission electron microscopy image of the core-shell structure Co@Pt / C alloy catalyst obtained in this example; Figure 2 The XRD diffraction pattern of the core-shell structure Co@Pt / C alloy catalyst obtained in Example 1; Figure 3 This is the ECSA diagram of the core-shell structure Co@Pt / C alloy catalyst obtained in this example; Figure 4 This is the LSV diagram of the core-shell structure Co@Pt / C alloy catalyst obtained in this example.
[0038] from Figure 1-4 It can be seen that the core-shell structured Co@Pt / C alloy catalyst has a relatively uniform particle size of about 3-5 nm, and the crystal structure is an ordered PtCo alloy structure. Through electrochemical characterization, it has obvious hydrogen adsorption and desorption characteristics of Pt alloy, and the ORR half-wave potential is about 0.9 V, with high oxygen reduction activity.
[0039] Example 2
[0040] This embodiment provides a method for preparing a core-shell structured Pt alloy catalyst, the specific process is as follows:
[0041] S1: 895.1 mg of cobalt nitrate was added to 120 mL of ethanol at a mass ratio of carbon support to transition metal salt of 1:4.3, stirred for 10 min, then added 209.4 mg of carbon powder and ultrasonicated for 30 min;
[0042] S2, placing the mixed solution in a room temperature environment to dry in the shade, and after forming a solid, drying it in a vacuum drying oven at 50°C;
[0043] S3, placing the dried sample in a tube furnace, replacing the gas with Ar gas three times, and then replacing it with 5% H2 / Ar mixed gas, heating up at a rate of 5°C / min, sintering the sample at a heat treatment temperature of 500°C and a heat treatment time of 3h, and cooling the sample to room temperature with the furnace after sintering to obtain a heat-treated sample;
[0044] S4, take 82 mg of the sample after heat treatment in step S3, disperse it in a pure water solution saturated with N2 gas, add a pure water solution saturated with N2 gas containing 69.7 mg of potassium chloroplatinite according to a molar ratio of platinum to cobalt nitrate of 1:2, react at 30°C for 30 minutes, filter and dry after the reaction is completed;
[0045] S5. The dried sample is placed in a tubular furnace and replaced with Ar gas three times, and then replaced with 5% H2 / Ar mixed gas, the heating rate is 5°C / min, the sample is sintered at a heat treatment temperature of 650°C and a heat treatment time of 2h. After sintering, the sample is cooled to room temperature with the furnace to obtain a heat-treated sample;
[0046] S6. The sample after the heat treatment in step S5 is acid-washed with 0.5M H2SO4 solution at 70°C for 2h, then filtered and washed, and dried to obtain the final core-shell structure Pt alloy catalyst.
[0047] Figure 5 This is a transmission electron microscopy image of the core-shell structure Co@Pt / C alloy catalyst obtained in this example; Figure 6 This is the XRD diffraction pattern of the core-shell structure Co@Pt / C alloy catalyst obtained in this example.
[0048] from Figure 5-6 It can be seen that with the increase of the heat treatment temperature in step S5, the particle size of the Co@Pt / C alloy becomes significantly larger, and the characteristic diffraction peak of its XRD is significantly enhanced, and the crystallinity is better.
[0049] Example 3
[0050] This embodiment provides a method for preparing a core-shell structured Pt alloy catalyst, the specific process is as follows:
[0051] S1. According to the mass ratio of carbon support to transition metal salt of 1:4.3, 1790.2 mg of nickel nitrate was added to 200 mL of ethanol, stirred for 10 min, then 418.7 mg of carbon powder was added and ultrasonicated for 40 min;
[0052] S2, placing the mixed solution in a room temperature environment to dry in the shade, and after forming a solid, drying it in a vacuum drying oven at 50°C;
[0053] S3, placing the sample dried in step S2 in a tube furnace, replacing the gas with Ar gas three times, and then replacing it with 5% H2 / Ar mixed gas, heating up at a rate of 5°C / min, sintering the sample at a heat treatment temperature of 500°C and a heat treatment time of 3h, and cooling the sample to room temperature with the furnace after sintering to obtain a heat-treated sample;
[0054] S4, take 85 mg of the sample obtained by heat treatment in step S3, disperse it in a pure water solution saturated with N2 gas, add a pure water solution saturated with N2 gas containing 105 mg of potassium chloroplatinite according to a molar ratio of platinum to nickel nitrate of 1:1.5, react at 30°C for 30 minutes, filter and dry after the reaction is completed;
[0055] S5. The dried sample is placed in a tubular furnace and replaced with Ar gas three times, and then replaced with 5% H2 / Ar mixed gas. The heating rate is 5°C / min. The sample is sintered at a heat treatment temperature of 600°C and a heat treatment time of 2h. After sintering, the sample is cooled to room temperature with the furnace to obtain a heat-treated sample.
[0056] S6. The sample after the heat treatment in step S5 is acid-washed with 0.5M H2SO4 solution at 70°C for 2h, then filtered and washed, and dried to obtain the final core-shell structure Pt alloy catalyst.
[0057] For those skilled in the art, various corresponding changes and modifications can be made according to the above technical solutions and concepts, and all of these changes and modifications should be included in the protection scope of the claims of the present invention.
Claims
1. A method for preparing a core-shell structured Pt alloy catalyst, characterized in that: The steps include: S1, adding transition metal nanoparticles and carbon carrier into a solvent, stirring and mixing to obtain a mixed solution; S2, drying the mixed solution obtained in step S1 to obtain a solid sample; S3, heat treating the solid sample obtained in step S2 under a protective atmosphere; S4, dispersing the solid sample after the heat treatment in step S3 in a solution saturated with an inert gas, adding a platinum precursor dropwise under magnetic stirring conditions, stirring and filtering after the reaction is complete, and drying the filtered solid; S5, heat-treating the solid obtained by drying in step S4 again under a protective atmosphere; S6. The solid after the heat treatment in step S5 is acid-washed with H2SO4 solution, and then filtered and washed to obtain a core-shell structure Pt alloy catalyst.
2. The preparation method according to claim 1, characterized in that: In step S1, the transition metal nanoparticles are one or more of cobalt nitrate, cobalt chloride, cobalt sulfate, nickel nitrate, nickel chloride, and nickel sulfate; the mass ratio of the carbon carrier to the transition metal nanoparticles is 1:2-10; and the solvent is one or more of water, ethanol, methanol, isopropanol, and ethylene glycol.
3. The preparation method according to claim 1, characterized in that: In step S1, ultrasonic dispersion is used to uniformly mix the transition metal nanoparticles and the carbon carrier with the solvent.
4. The preparation method according to claim 1, characterized in that: In step S2, the drying treatment is carried out by one or more methods selected from the group consisting of room temperature shade drying, vacuum drying, rotary evaporation drying, and freeze drying.
5. The preparation method according to claim 1, characterized in that: In step S3, the protective atmosphere is high-purity hydrogen, hydrogen-argon mixed gas or hydrogen-nitrogen mixed gas, and the volume concentration of the hydrogen is 1%-100%; the heat treatment temperature is 400°C-700°C, and the heat treatment time is the reaction time of 0.5h-12h.
6. The preparation method according to claim 1, characterized in that: The heat treatments in steps S3 and S5 are both performed in a tube furnace.
7. The preparation method according to claim 1, characterized in that: In step S4, the inert gas is one or more of nitrogen, argon, and helium; the solution is one or more of water, ethanol, methanol, isopropanol, and ethylene glycol; the platinum precursor includes one or more of chloroplatinic acid, potassium chloroplatinate, sodium chloroplatinate, potassium chloroplatinite, sodium chloroplatinite, platinum acetylacetonate, and platinum nitrate, the molar ratio of platinum to transition metal nanoparticles is 1:0.1-2, the reaction temperature is 10°C-80°C, and the reaction time is 30min-180min.
8. The preparation method according to claim 1, characterized in that: In step S5, the protective atmosphere is nitrogen, argon or a hydrogen-argon mixture, and the hydrogen-argon mixture is a 5% H2 / Ar mixture or a 10% H2 / Ar mixture; the heat treatment temperature is 400°C-800°C, and the heat treatment time is 1h-6h.
9. The preparation method according to claim 1, characterized in that: In step S6, the solid heat-treated in step S5 is acid-washed with a 0.5 mol / L H2SO4 solution at 70°C for 2h-6h.