Rubidium-doped zirconium lithium halide solid electrolyte and preparation method thereof
By doping rubidium ions in the chloride solid electrolyte to form large pore diameter channels, the lithium ion conductivity is improved, and the problems of low conductivity and high cost of existing electrolyte materials are solved, and low-cost and high-performance rubidium doped zirconium halide are achieved. Preparation of lithium solid electrolytes, suitable for all-solid lithium-ion batteries.
Patent Information
- Application Number
- CN202411164830.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-23
- Publication Date
- 2024-11-15
AI Technical Summary
The existing chloride solid electrolyte materials have low conductivity, high cost and poor stability, making it difficult to meet the needs of improving the performance of all-solid lithium-ion batteries.
By doping rubidium ions, large-pore lithium ion channels are formed, which weakens the Coulomb repulsion between Zr4+ and Li+ and improves the conductivity of lithium ion. The chemical formula of Li2+3xRbxZr1-xX6 is adopted, combining anhydrous lithium halide, zirconium halide and rubidium halide and rubidium halide. The high-purity material is ground and annealed under an inert gas atmosphere to prepare rubidium-doped zirconium halide solid electrolyte.
It significantly improves the conductivity at room temperature, reduces production costs, has low cost and excellent performance, has low annealing temperature, and has better ionic conductivity than oxide and sulfide electrolytes.
Smart Images

Figure CN118970156A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of solid electrolyte materials, and in particular to a rubidium-doped lithium zirconium halide solid electrolyte and a preparation method thereof. Background Art
[0002] The energy density of traditional liquid lithium-ion batteries has encountered bottlenecks, and liquid electrolytes have the characteristics of high chemical reactivity, easy oxidation, and easy combustion, which are prone to safety hazards. The electrolyte of solid-state batteries is solid, which can greatly improve battery safety and energy density compared to traditional electrolytes. It is regarded as the next generation of battery technology that breaks through the bottleneck of lithium-ion batteries. The most critical link in the development of solid-state batteries is to develop and prepare solid-state electrolytes with excellent performance to promote the performance improvement of all-solid-state batteries. Compared with other solid-state electrolyte materials, halide solid electrolyte materials have high ionic conductivity, good deformability, good interface compatibility with the positive electrode and good oxidation stability, etc., and are expected to become the main electrolyte material for the new generation of solid-state batteries.
[0003] The paper “A cost-effective and humidity-tolerant chloride solid electrolyte for lithium batteries” reports a low-cost chloride solid electrolyte material Li2ZrCl6, which is several orders of magnitude cheaper than the most advanced chloride solid electrolyte ($11.6 / kg) and has an ideal room temperature conductivity (0.81 mS·cm –1 ), is an ideal solid electrolyte material.
[0004] The conductivity of solid electrolytes not only determines the ion transmission efficiency, but also indirectly affects the energy density of all-solid-state batteries. The conductivity of the current chloride electrolyte material Li2ZrCl6 is only 0.81 mS·cm –1 , there is still room for further improvement.
[0005] The patent application with publication number CN116315050A discloses a solid electrolyte material with the general chemical formula of Li a+a+2b Zr 1-a-b M a N b X6, M is selected from one or two of Eu and Gd, N is selected from one or more of Co, Cu, Zn, Mg and Cd, a+b is 0.1-0.5, and a / b is 1-6. The solid electrolyte obtained by this chemical formula has improved ion conductivity, but its element composition is complex, the cost is high and the stability is poor.
[0006] Therefore, it is necessary to provide an improved rubidium-doped lithium zirconium halide solid electrolyte and a preparation method thereof to solve the above problems. Summary of the invention
[0007] The purpose of the present invention is to provide a rubidium-doped lithium zirconium halide solid electrolyte and a preparation method thereof, by doping rubidium ions, a large-aperture lithium ion channel is formed to promote the conduction of lithium ions; it can also weaken the Zr 4+ With Li + The Coulomb repulsion between them helps the dissociation of lithium ions and improves the lithium ion conductivity.
[0008] To achieve the above object, the present invention provides a rubidium-doped lithium zirconium halide solid electrolyte, the chemical formula of which is Li 2+3x R x Zr 1-x X6, 0<x≤0.5, X is one or more of F, Cl, Br, I elements.
[0009] Furthermore, 0<x≤0.4.
[0010] Furthermore, 0.1≤x≤0.2. X is preferably Cl.
[0011] For example, x is a specific numerical value such as 0.10, 0.12, 0.15, 0.18 or 0.20.
[0012] The doping of rubidium ions can increase the + The concentration of rubidium ions is also increased, and because the atomic radius of rubidium ions is large, doping causes the zirconium halide lithium lattice distortion, thereby forming a large-aperture lithium ion channel to promote the conduction of lithium ions. Rubidium ion doping can also weaken the Zr 4+ With Li + The Coulomb repulsion between the two helps the lithium ions to dissociate and improve the lithium ion conductivity. In addition, the doping of rubidium ions also causes metal site disorder, reduces the site order, and can also improve the conductivity of lithium zirconium halide. The present invention can significantly improve the conductivity at room temperature by regulating the doping ratio of rubidium ions.
[0013] The present invention also provides a method for preparing the rubidium-doped lithium zirconium halide solid electrolyte described in any one of the above items, comprising: mixing anhydrous lithium halide, anhydrous zirconium halide and anhydrous rubidium halide according to Li 2+3x R x Zr 1-x The chemical ratio of X6 is weighed, then ground and mixed under an inert gas atmosphere, ball milled, and finally annealed at 200-400°C to obtain rubidium-doped lithium zirconium halide.
[0014] Furthermore, the annealing time is 4 to 12 hours.
[0015] Furthermore, the ball milling speed is 300-600 rpm, and the ball milling time is 10-72 hours.
[0016] Furthermore, the ball mill uses zirconia beads, and the mass ratio of balls to materials is (15~45):1.
[0017] Furthermore, the mortar used for grinding is an agate mortar, and the grinding time is 10 to 60 minutes.
[0018] Furthermore, the inert gas is argon with a purity of ≥99.999%.
[0019] Furthermore, the purity of the anhydrous lithium halide is ≥99.9%, the purity of the anhydrous zirconium halide is ≥98%, and the purity of the anhydrous rubidium halide is ≥99.9%; the anhydrous lithium halide, anhydrous zirconium halide and anhydrous rubidium halide are all dried in an oven at 120° C. for 24 hours before use.
[0020] The beneficial effects of the present invention are as follows: 1. The rubidium-doped lithium zirconium halide solid electrolyte provided by the present invention is obtained by modifying lithium zirconium halide by doping a trace amount of rubidium to obtain a halide solid electrolyte with high ionic conductivity.
[0021] 2. The rubidium-doped lithium zirconium halide of the present invention has both low production cost and excellent comprehensive performance. The ion conductivity is significantly better than that of oxide electrolytes and is not inferior to that of sulfide electrolytes. The raw material cost is lower than that of sulfide electrolytes, and the annealing temperature is about 300°C, which is lower than the heating temperature of sulfides (400-700°C) and oxides (above 1100°C). BRIEF DESCRIPTION OF THE DRAWINGS
[0022] In order to more clearly illustrate the technical solutions in the present invention or the prior art, the following briefly introduces the drawings required for use in the embodiments or the description of the prior art. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0023] Figure 1 The following are the XRD diffraction patterns of the examples and comparative examples.
[0024] Figure 2 The electrochemical impedance spectroscopy results of the embodiments and comparative examples at 25°C are shown in FIG. DETAILED DESCRIPTION
[0025] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be clearly and completely described below in conjunction with the drawings of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0026] Example 1
[0027] A method for preparing a rubidium-doped lithium zirconium halide solid electrolyte comprises the following steps: 1) Step 1: Anhydrous lithium chloride, anhydrous zirconium chloride and anhydrous rubidium chloride are prepared according to Li 2.15 Zr 0.95 R 0.05 The Cl6 chemical ratio is weighed and ground and mixed in an inert gas atmosphere.
[0028] 2) Step 2: In an inert gas atmosphere, the ground mixed powder was placed in a ball mill jar, sealed with tape, and then ball milled on a planetary ball mill at a rotation speed of 600 rpm, a ball milling time of 72 h, and a ball-to-material ratio of 15:1.
[0029] 3) Step 3: The ball-milled powder is taken out from the ball mill under an inert gas atmosphere, and annealed at 200° C. for 6 h under argon protection to finally obtain a rubidium-doped lithium zirconium halide material.
[0030] 4) Step 4: The material was pressed into a disc using a cold isostatic pressing device at a pressure of 200 MPa for 5 minutes, and an XRD test was performed on the disc with a scanning range of 10° to 80° and a scanning rate of 5° / min.
[0031] 5) Step 5: The surface of the wafer is gold-sprayed and the ionic conductivity of the sample is detected using the AC impedance method with an amplitude of 10 mV and a frequency range of 1 MHz to 1 Hz.
[0032] Example 2
[0033] The difference from Example 1 is that the chemical formula of the rubidium-doped lithium zirconium halide solid electrolyte is Li 2.30 Zr 0.90 R 0.10 The rest is the same as in Example 1 and will not be described again.
[0034] Example 3
[0035] The difference from Example 1 is that the chemical formula of the rubidium-doped lithium zirconium halide solid electrolyte is Li 2.45 Zr 0.85 R 0.15The rest is the same as in Example 1 and will not be described again.
[0036] Example 4
[0037] The difference from Example 1 is that the chemical formula of the rubidium-doped lithium zirconium halide solid electrolyte is Li 2.60 Zr 0.80 R 0.20 The rest is the same as in Example 1 and will not be described again.
[0038] Example 5
[0039] The difference from Example 1 is that the chemical formula of the rubidium-doped lithium zirconium halide solid electrolyte is Li 2.75 Zr 0.75 R 0.25 The rest is the same as in Example 1 and will not be described again.
[0040] Example 6
[0041] The difference from Example 1 is that the chemical formula of the rubidium-doped lithium zirconium halide solid electrolyte is Li 2.90 Zr 0.70 R 0.30 The rest is the same as in Example 1 and will not be described again.
[0042] Comparative Example 1
[0043] The difference from Example 1 is that the chemical formula of the rubidium-doped lithium zirconium halide solid electrolyte is Li2ZrCl6. The rest is the same as Example 1 and will not be repeated here.
[0044] Table 1 Conductivity test results of embodiments and comparative examples
[0045] The XRD diffraction patterns of the embodiments and comparative examples are shown in Figure 1 The electrochemical impedance spectroscopy results of the examples and comparative examples at 25°C are shown in Figure 2 .
[0046] from Figure 1 It can be observed that all the embodiments and comparative examples exhibit a P-3m1 crystal structure consistent with Li3YCl6, and the doping of rubidium element causes a slight shift in the characteristic peaks of the samples.
[0047] Combination Figure 2 As can be seen from Table 1, the present invention can be annealed at a relatively low temperature by doping with an appropriate amount of rubidium, and the room temperature ionic conductivity of the obtained rubidium-doped lithium zirconium halide material is significantly improved compared with lithium zirconium chloride. Therefore, the preparation method of the present invention is simple, low in cost, good in performance, and has broad application prospects.
[0048] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A rubidium-doped lithium zirconium halide solid electrolyte, characterized in that: Its chemical formula is Li 2+3x R x Zr 1-x X6, wherein 0.1≤x≤0.2, X is one or more of F, Cl, Br, and I elements.
2. A method for preparing the rubidium-doped lithium zirconium halide solid electrolyte according to claim 1, characterized in that: include: Anhydrous lithium halide, anhydrous zirconium halide and anhydrous rubidium halide are prepared by Li 2+3x R x Zr 1-x The chemical ratio of X6 is weighed, then ground and mixed under an inert gas atmosphere, ball milled, and finally annealed at 200-400°C to obtain rubidium-doped lithium zirconium halide.
3. The method for preparing the rubidium-doped lithium zirconium halide solid electrolyte according to claim 2, characterized in that: The annealing time is 4 to 12 hours.
4. The method for preparing the rubidium-doped lithium zirconium halide solid electrolyte according to claim 2, characterized in that: The ball milling speed is 300-600 rpm, and the ball milling time is 10-72 hours.
5. The method for preparing the rubidium-doped lithium zirconium halide solid electrolyte according to claim 2, characterized in that: The ball mill uses zirconia beads, and the mass ratio of the balls to the materials is (15-45):
1.
6. The method for preparing the rubidium-doped lithium zirconium halide solid electrolyte according to claim 2, characterized in that: The mortar used for the grinding is an agate mortar, and the grinding time is 10 to 60 minutes.
7. The method for preparing the rubidium-doped lithium zirconium halide solid electrolyte according to claim 2, characterized in that: The inert gas is argon with a purity of ≥99.999%.
8. The method for preparing the rubidium-doped lithium zirconium halide solid electrolyte according to claim 2, characterized in that: The purity of the anhydrous lithium halide is ≥99.9%, the purity of the anhydrous zirconium halide is ≥98%, and the purity of the anhydrous rubidium halide is ≥99.9%.
9. The method for preparing the rubidium-doped lithium zirconium halide solid electrolyte according to claim 2, characterized in that: The anhydrous lithium halide, anhydrous zirconium halide and anhydrous rubidium halide were all dried in an oven at 120° C. for 24 hours before use.