High-strength high-temperature-resistant lithium ion battery diaphragm and preparation method thereof
By using polyimide, nanoalumina and graphene nanosheets to prepare high-strength high-temperature resistant lithium-ion battery separators, the problems of insufficient thermal stability and mechanical strength of traditional separators are solved, and better electrolyte wetting and safety are achieved performance.
Patent Information
- Application Number
- CN202411323179.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-23
- Publication Date
- 2024-11-15
AI Technical Summary
The thermal stability and mechanical strength of traditional lithium-ion battery separators may cause battery short circuits, fires or explosions in high temperature environments, and poor electrolyte wetting properties affect battery performance.
Polyimide, nano-alumina and graphene nanosheets are used as raw materials to prepare high-strength, high-temperature, high-temperature resistant lithium-ion battery separators through solution preparation and heat treatment to improve the mechanical strength of the separators and the electrolyte wetting properties.
It significantly improves the mechanical strength and high temperature resistance of the diaphragm, ensures the uniform wetting of the electrolyte, reduces the internal impedance of the battery, and enhances safety performance and cycle life.
Smart Images

Figure BDA0005054592450000041
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of battery materials, and in particular to the preparation of a lithium-ion battery separator, and in particular to a high-strength and high-temperature-resistant lithium-ion battery separator and a preparation method thereof. Background Art
[0002] As the global demand for clean energy continues to grow, lithium-ion batteries, as an efficient and environmentally friendly energy storage device, have been widely used in many fields such as electric vehicles, portable electronic devices, and energy storage systems. In the structure of lithium-ion batteries, although the diaphragm does not directly participate in the electrochemical reaction, its performance has a crucial impact on the overall performance of the battery, especially safety and cycle life.
[0003] Traditional lithium-ion battery separators are usually made of polyolefin materials, such as polyethylene (PE) and polypropylene (PP). These materials have certain chemical stability and insulation properties, and can meet the basic needs of lithium-ion batteries to a certain extent. However, with the rapid development of lithium-ion battery technology and the continuous expansion of application scenarios, the limitations of polyolefin separators are becoming increasingly prominent.
[0004] On the one hand, the melting point of polyolefin separators is relatively low, usually between 130-170°C. When the battery is charged and discharged at high power or working in a high temperature environment, the polyolefin separator is prone to thermal shrinkage or even melting, resulting in direct contact between the positive and negative electrodes, causing internal short circuits in the battery, and in severe cases, may cause battery fires, explosions and other safety accidents. In recent years, safety issues caused by insufficient thermal stability of lithium-ion battery separators have been reported from time to time, which has brought huge challenges to the widespread application of lithium-ion batteries.
[0005] On the other hand, the mechanical strength of polyolefin separators is limited, and it is difficult to withstand the stress caused by volume changes caused by the insertion and extraction of lithium ions during the battery charging and discharging process. During long-term use, the separator is prone to rupture, wrinkles, and lithium dendrites piercing the separator, which affects the battery's cycle performance and service life.
[0006] In addition, in order to improve the energy density and charge and discharge rate of lithium-ion batteries, the separator needs to have good electrolyte wettability to promote the rapid transfer of lithium ions between the positive and negative electrodes. However, the surface energy of polyolefin separators is low and their affinity for electrolytes is poor, resulting in uneven penetration and distribution of electrolytes in the separator, increasing the internal resistance of the battery and reducing the performance of the battery.
[0007] In summary, the development of a new type of lithium-ion battery separator with high strength, high temperature resistance and good electrolyte wettability has become a key issue that needs to be solved in the current lithium-ion battery field. This will not only help improve the safety performance of lithium-ion batteries and promote the further development of lithium-ion battery technology, but also lay a solid foundation for its application in a wider range of fields. Summary of the invention
[0008] The present invention provides a high-strength, high-temperature-resistant lithium-ion battery separator and a preparation method thereof, aiming to solve the problems existing in the above-mentioned background technology.
[0009] In order to achieve the above technical objectives, the present invention mainly adopts the following technical solutions:
[0010] In a first aspect, the present invention discloses a high-strength and high-temperature resistant lithium-ion battery separator, which comprises the following raw materials in parts by weight: 10-15 parts of polyimide, 1-2 parts of nano-ceramic material and 0.5-1 part of graphene nanosheets.
[0011] In a preferred embodiment of the present invention, the nano-ceramic material is nano-alumina.
[0012] Furthermore, the average particle size of the nano-alumina is 50-200 nm.
[0013] In a preferred embodiment of the present invention, the diameter of the graphene nanosheet is 1-10 μm.
[0014] In a preferred embodiment of the present invention, the thickness of the diaphragm is 10-50 μm.
[0015] In a second aspect, the present invention discloses a method for preparing a high-strength and high-temperature resistant lithium-ion battery separator as described in the first aspect, comprising the following steps:
[0016] (1) Solution preparation: dissolving polyimide powder in an organic solvent and stirring at a constant temperature for a set time to obtain a polyimide solution; then adding nano-ceramic material and graphene nanosheets to the polyimide solution and mixing them evenly, and then ultrasonically treating them for a set time to obtain a uniform mixed solution;
[0017] (2) Thin film preparation: The mixed solution is formed into a film on a flat and clean substrate by a casting method or a doctor blade method, and then vacuum dried to remove the solvent to obtain a dried thin film;
[0018] (3) Heat treatment: The dried film is heat treated under nitrogen or argon protection to further cross-link the polyimide molecular chains to obtain a high-strength, high-temperature resistant lithium-ion battery separator.
[0019] In a preferred embodiment of the present invention, in step (1), the organic solvent is N-methylpyrrolidone NMP, the mass fraction of the obtained polyimide solution is 10-30%, the stirring temperature is 30-50°C, the stirring time is 1-4h, the ultrasonic treatment time is 1-3h, and the ultrasonic temperature is 20-30°C.
[0020] In a preferred embodiment of the present invention, in step (2), when the film is formed by the casting method, the casting speed is 5-15 mm / s; when the film is formed by the blade coating method, the blade coating speed is 10-20 mm / s, the vacuum drying temperature is 40-100°C, and the drying time is 2-8h.
[0021] In a preferred embodiment of the present invention, in step (3), the heat treatment temperature is 200-300°C, and the heat treatment time is 1-5h.
[0022] Compared with the prior art, the present invention has the following beneficial effects:
[0023] The invention provides a high-strength and high-temperature-resistant lithium-ion battery separator and a preparation method thereof. The addition of nano-alumina and graphene nanosheets significantly improves the mechanical strength and high-temperature resistance of the separator. Through the optimized preparation process, the separator has a uniform structure and good electrolyte wettability. DETAILED DESCRIPTION
[0024] In order to further illustrate the technical means adopted by the present invention and the effects achieved, the following will be combined with specific embodiments to describe in detail the specific implementation methods, characteristics and effects of the present invention according to a method for preparing a high-strength and high-temperature resistant lithium-ion battery separator proposed by the present invention. It should be noted in the following embodiments that the present invention is not limited to the following embodiments. In the absence of conflict, the embodiments disclosed in the present invention and the features therein can be combined with each other. Unless otherwise specified, the raw materials described in the embodiments of the present invention are conventional raw materials available on the market, the equipment used are equipment commonly used in the field, and the reaction conditions are normal conditions; the identification of the product is identification by conventional methods.
[0025] The preparation method of the high-strength and high-temperature resistant lithium-ion battery separator provided by the present invention comprises the following specific steps:
[0026] (1) Solution preparation: First, select polyimide powder with high purity and stable performance. Slowly add the polyimide powder into N-methylpyrrolidone (NMP) solvent, and stir it at a certain speed and temperature in a constant temperature stirrer to ensure that the polyimide is fully dissolved to form a uniform and transparent solution. The mass fraction of the solution is controlled at 10-50%. Then, slowly add the pre-treated nano-alumina and graphene nanosheets into the above polyimide solution. Use ultrasonic treatment equipment to ultrasonically treat the mixed solution for 1-3 hours, so that the nano-alumina and graphene nanosheets are evenly dispersed in the polyimide solution to obtain a stable mixed solution.
[0027] (2) Film preparation: The mixed solution is formed into a film on a flat and clean substrate by casting or doctor blade. In the casting method, the flow rate of the solution and the height of the doctor blade are controlled to ensure that the thickness of the formed film is uniform. In the doctor blade method, attention should be paid to the angle and pressure of the doctor blade to ensure the flatness of the film. After the film is formed, the substrate is placed in a constant temperature drying oven and dried under appropriate temperature conditions to completely remove the solvent and initially solidify the film.
[0028] (3) Heat treatment: The dried film is placed in a high-temperature furnace and heat treated under the protection of an inert gas such as nitrogen or argon. The heat treatment temperature is controlled at 200-300°C and the treatment time is 1-5 hours. During this process, the polyimide molecular chains are further cross-linked to form a more stable structure, thereby improving the performance of the diaphragm.
[0029] The film thickness test, tensile strength test, and thermal shrinkage test of the embodiments of the present invention and the comparative examples were tested, and the test methods are as follows:
[0030] Thickness test: Use a Mahr thickness gauge or micrometer to measure the thickness of the film material. The thickness of the film material can be directly read according to the indication of the Mahr thickness gauge or micrometer.
[0031] Tensile strength test: Use a universal mechanical testing machine to test the tensile properties of the diaphragm. Before the test, cut the sample film into a set width b and record the average thickness d of the film. Then stretch the sample at a certain speed until the sample breaks, and record the maximum tensile force F when the sample breaks. Then, according to the width b and thickness d of the sample, as well as the maximum tensile force F (unit: N) value, use the following formula to calculate the tensile strength σ (unit: MPa) of the film:
[0032]
[0033] Heat shrinkage test: After laying the sample film flat, use a cutting board (300*100) to cut out the sample to be tested, and measure the length h1 of the cut sample. Set the oven temperature to 200℃, and keep it warm for 1 hour after reaching the temperature. Put the sample in the oven and keep it warm for 1 hour. After cooling for 10 minutes, measure the length h2 of the sample.
[0034] Diaphragm thermal shrinkage = (h1-h2) / h1*100%.
[0035] The following is an explanation through specific embodiments.
[0036] Example 1
[0037] A method for preparing a high-strength, high-temperature-resistant lithium-ion battery separator, the steps of which are as follows:
[0038] (1) Membrane solution preparation:
[0039] 10 g of polyimide powder was dissolved in 40 g of NMP, and the mixture was stirred at 300 rpm for 3 hours in a constant temperature stirrer at 40° C. to prepare a polyimide solution with a mass fraction of 20%; 1 g of nano-alumina with an average particle size of 100 nm and 0.5 g of graphene nanosheets with a sheet size of 5 μm were ultrasonically treated at a frequency of 30 kHz for 20 minutes in an ultrasonic disperser, and then slowly added to the polyimide solution, and then stirred at 300 rpm for 1.5 hours at 40° C., and then ultrasonically treated at 25° C. for 2 hours to obtain a uniform mixed solution;
[0040] (2) Film preparation:
[0041] The mixed solution was formed into a film on a flat glass plate by a casting method, the casting speed was controlled to be 10 mm / s, and then vacuum dried at 50° C. to remove the solvent;
[0042] (3) Heat treatment:
[0043] The dried film was heat-treated at 300° C. for 2 hours under nitrogen protection to further cross-link the polyimide molecular chains to obtain a high-strength and high-temperature resistant lithium-ion battery separator.
[0044] The performance test of the diaphragm prepared in Example 1 of the present invention showed that the thickness of the diaphragm was 20 μm, the tensile strength was 200 MPa, the thermal shrinkage rate was less than 2% (200° C., 1 h), and the electrolyte wettability was good.
[0045] Example 2
[0046] A method for preparing a high-strength, high-temperature-resistant lithium-ion battery separator, the steps of which are as follows:
[0047] (1) Solution preparation:
[0048] 15 g of polyimide powder was dissolved in 55 g of NMP, and the mixture was stirred at 350 rpm for 3.5 hours in a constant temperature stirrer at 45° C. to prepare a polyimide solution with a mass fraction of 20%; 2 g of nano-alumina with an average particle size of 150 nm and 1 g of graphene nanosheets with a sheet size of 8 μm were ultrasonically treated at a frequency of 35 kHz for 25 minutes in an ultrasonic disperser, and then slowly added to the polyimide solution, and then stirred at 350 rpm for 1.5 hours at 45° C., and then ultrasonically treated at 25° C. for 2 hours to obtain a uniform mixed solution;
[0049] (2) Film preparation:
[0050] The mixed solution was coated on a stainless steel plate by a doctor blade method at a speed of 15 mm / s, and then vacuum dried at 50°C to remove the solvent.
[0051] (3) Heat treatment:
[0052] The dried film was heat-treated at 300° C. for 2 hours under argon protection to further cross-link the polyimide molecular chains to obtain a high-strength and high-temperature resistant lithium-ion battery separator.
[0053] The performance test results of the diaphragm prepared in Example 2 of the present invention are as follows: the thickness of the diaphragm is 30 μm, the tensile strength is 250 MPa, the thermal shrinkage rate is less than 1.5% (200° C., 1 h), and the electrolyte wettability is good.
[0054] Comparative Example 1
[0055] The diaphragm was prepared using pure polyimide of the same mass as in Example 1, but without adding nano-alumina and graphene nanosheets, and the same preparation process as in Example 1 of the present invention was used.
[0056] The performance test of the diaphragm prepared in Comparative Example 1 of the present invention showed that the thickness of the diaphragm was 20 μm, the tensile strength was 110 MPa, the thermal shrinkage rate was greater than 10% (200° C., 1 h), and the electrolyte wettability was poor.
[0057] Comparative Example 2
[0058] The diaphragm was prepared using the same mass of polyimide as in Example 1, and 1.5 g of nano-alumina was added, but no graphene nanosheets were added, and the same preparation process as in Example 1 of the present invention was followed.
[0059] The performance test of the diaphragm prepared in Comparative Example 2 of the present invention showed that the thickness of the diaphragm was 25 μm, the tensile strength was 130 MPa, the thermal shrinkage rate was about 80% (200° C., 1 h), and the electrolyte wettability was average.
[0060] Comparative Example 3
[0061] The diaphragm was prepared using the same mass of polyimide as in Example 1, and 1 g of graphene nanosheets was added, but no nano-alumina was added, and the same preparation process as in Example 1 of the present invention was followed.
[0062] The performance test of the diaphragm prepared in Comparative Example 3 of the present invention showed that the thickness of the diaphragm was 25 μm, the tensile strength was 120 MPa, the thermal shrinkage rate was about 7% (200° C., 1 h), and the electrolyte wettability was good.
[0063] The specific embodiments described above further illustrate the objectives, technical solutions and beneficial effects of the present invention in detail, but do not limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A high-strength, high-temperature-resistant lithium-ion battery separator, characterized in that: The diaphragm comprises the following raw materials in parts by weight: 10-15 parts of polyimide, 1-2 parts of nano-ceramic material and 0.5-1 part of graphene nanosheet.
2. The high-strength and high-temperature-resistant lithium-ion battery separator according to claim 1, characterized in that: The nano ceramic material is nano alumina.
3. The high-strength and high-temperature-resistant lithium-ion battery separator according to claim 2, characterized in that: The average particle size of the nano-alumina is 50-200nm.
4. The high-strength and high-temperature-resistant lithium-ion battery separator according to claim 1, characterized in that: The diameter of the graphene nanosheet is 1-10 μm.
5. The high-strength and high-temperature-resistant lithium-ion battery separator according to claim 1, characterized in that: The thickness of the separator is 10-50 μm.
6. A method for preparing a high-strength, high-temperature-resistant lithium-ion battery separator according to any one of claims 1 to 5, characterized in that: The steps include: (1) Solution preparation: dissolving polyimide powder in an organic solvent and stirring at a constant temperature for a set time to obtain a polyimide solution; then adding nano-ceramic material and graphene nanosheets to the polyimide solution and mixing them evenly, and then ultrasonically treating them for a set time to obtain a uniform mixed solution; (2) Thin film preparation: The mixed solution is formed into a film on a flat and clean substrate by a casting method or a doctor blade method, and then vacuum dried to remove the solvent to obtain a dried thin film; (3) Heat treatment: The dried film is heat treated under nitrogen or argon protection to further cross-link the polyimide molecular chains to obtain a high-strength, high-temperature resistant lithium-ion battery separator.
7. The preparation method according to claim 6, characterized in that: In step (1), the organic solvent is N-methylpyrrolidone NMP, the mass fraction of the obtained polyimide solution is 10-30%, the stirring temperature is 30-50°C, the stirring time is 1-4h, the ultrasonic treatment time is 1-3h, and the ultrasonic temperature is 20-30°C.
8. The preparation method according to claim 6, characterized in that: In step (2), when the film is formed by the casting method, the casting speed is 5-15 mm / s; when the film is formed by the blade coating method, the blade coating speed is 10-20 mm / s, the vacuum drying temperature is 40-100° C., and the drying time is 2-8 h.
9. The preparation method according to claim 6, characterized in that: In step (3), the heat treatment temperature is 200-300°C, and the heat treatment time is 1-5h.