Composite flame-retardant diaphragm for lithium battery and preparation method of composite flame-retardant diaphragm
By installing modified layers of polyimide, flame retardant, alumina and silica modified PVA fibers on the lithium-ion battery separator, the problem of poor thermal stability of the lithium-ion battery separator at high temperatures is solved, and excellent results are achieved The flame retardant and high temperature resistance improve the safety of the battery.
Patent Information
- Application Number
- CN202411352071.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-26
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-09-26
AI Technical Summary
The thermal stability of the lithium-ion battery is poor at high temperatures, which can easily lead to shrinkage and internal short circuits, causing fire safety accidents. The flame retardant efficiency of the existing technology is low and cannot effectively ensure battery safety.
The modified layer is provided on the surface of the polypropylene diaphragm. The modified layer is composed of polyimide, flame retardant, alumina and silica modified PVA fibers. It is formed by electrospinning technology to improve the high temperature resistance and flame retardant of the diaphragm. performance.
It significantly improves the flame retardant and high temperature resistance of lithium battery separators, delays polyimide degradation, isolates oxygen, slows down flame spread, and significantly improves the safety of the battery.
Smart Images

Figure CN118970375A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of lithium batteries, and in particular to a composite flame-retardant diaphragm for lithium batteries and a preparation method thereof. Background Art
[0002] Lithium-ion batteries have the advantages of high energy density, long life, and no memory effect. They are widely used in fields such as mobile phones, laptops, and electric vehicles. The safety issues of lithium batteries mainly stem from thermal runaway of the battery caused by its improper use, which in turn causes fire safety accidents. Analyzing from the source of thermal runaway, there are two main reasons that threaten battery safety. On the one hand, polyolefin diaphragms and carbonate electrolytes have extremely poor thermal stability and highly flammable properties. Once the battery is overheated (greater than 120°C), the diaphragm will shrink rapidly, causing the positive and negative electrodes to directly contact each other to form an internal short circuit, generating a large amount of Joule heat and triggering a domino-like chemical reaction inside the battery.
[0003] The safety of the diaphragm will have a great impact on the safety of the battery, and a high-safety diaphragm must have excellent heat resistance, no obvious shrinkage behavior at high temperatures, and preferably have flame retardant properties; however, the flame retardant efficiency of the diaphragm in related technologies is low.
[0004] Application Contents
[0005] The present application is made in view of the above-mentioned problems, and its object is to provide a composite flame-retardant separator for lithium batteries, which has excellent flame-retardant performance.
[0006] Specifically as follows, the first aspect of the present application provides a composite flame-retardant diaphragm for a lithium battery, comprising a polypropylene diaphragm body;
[0007] A modified layer is provided on either side of the polypropylene diaphragm body;
[0008] The modified layer comprises the following preparation raw materials:
[0009] Polyimide, flame retardant, alumina and silica modified PVA fiber;
[0010] The silica-modified PVA fiber comprises the following preparation raw materials:
[0011] PVA, silica sol, ammonium polyphosphate and silane polyethylene glycol carboxyl.
[0012] According to one of the technical solutions of this application, at least the following beneficial effects are achieved:
[0013] The present application forms a composite diaphragm with excellent flame retardant properties by arranging a modified layer on the surface of a polypropylene diaphragm; the raw materials for preparing the modified layer in the present application also include polyimide, flame retardant, ammonium polyphosphate and silane polyethylene glycol carboxyl groups, wherein the polyimide itself has high thermal stability and contains abundant polar groups on its surface, thereby giving the modified layer excellent high temperature resistance; the present application also utilizes silane polyethylene glycol carboxyl groups to modify ammonium polyphosphate, which can improve its dispersibility in the modified layer and facilitate the ammonium polyphosphate to be fully dispersed in the modified layer, and similarly, the silane polyethylene glycol carboxyl groups introduce carboxyl groups on the surface of ammonium polyphosphate, and the carboxyl groups interact with the amino residues on the surface of the polyimide, which can anchor the ammonium polyphosphate on the surface of the polyimide, thereby facilitating the improvement of the flame retardant properties of the polyimide.
[0014] According to some embodiments of the present application, the modified layer is disposed on both side surfaces of the polypropylene diaphragm body.
[0015] According to some embodiments of the present application, the modified layer includes the following preparation raw materials in parts by weight:
[0016] 100 parts of polyimide, 5 to 7 parts of flame retardant, 2 to 4 parts of aluminum oxide and 12 to 14 parts of silicon dioxide modified PVA fiber.
[0017] According to some embodiments of the present application, the raw materials for preparing the modified layer also include a solvent.
[0018] According to some embodiments of the present application, the silica-modified PVA fiber includes the following preparation raw materials in parts by weight:
[0019] 100 parts of PVA, 10-20 parts of silica sol, 8-15 parts of ammonium polyphosphate and 1-2 parts of silane polyethylene glycol carboxyl.
[0020] According to some embodiments of the present application, the degree of polymerization of the PVA is 15K to 18K.
[0021] According to some embodiments of the present application, the raw materials for preparing the silica-modified PVA fiber also include a solvent.
[0022] According to some embodiments of the present application, the thickness of the polypropylene diaphragm body is 5 μm to 30 μm.
[0023] According to some embodiments of the present application, the flame retardant includes DOPO-melamine.
[0024] The molecular structure of 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide (DOPO) contains biphenyl ring and phenanthrene ring structures, especially the side phosphorus group is introduced in the form of a cyclic O=PO bond, which has excellent flame retardant properties; and melamine and the molecular chain of 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide are physically entangled, and can also play a partial toughening effect.
[0025] DOPO-melamine is in the form of two-dimensional flakes with large size; ammonium polyphosphate mainly exists in the form of small particles; forming a point-surface combined flame retardant additive; at the same time, melamine can decompose as a gas source to release a large amount of gas to promote the rapid expansion of the carbon layer. The fluffy and porous structure makes a certain temperature gradient exist between the matrix and the surface of the carbon layer. The surface temperature of the diaphragm is much lower than the flame temperature, which slows down the possibility of further degradation of polyimide and release of combustible gas, and at the same time isolates the entry of external oxygen, thereby exerting a good flame retardant effect for a considerable period of time.
[0026] The expansion system composed of DOPO-melamine and ammonium polyphosphate decomposes to generate a large amount of NH3, water vapor and other gases when heated without breaking through the carbon layer barrier. There is also a synergistic effect between DOPO-melamine and ammonium polyphosphate, which can give full play to the heat insulation, oxygen isolation and smoke suppression effects of the carbon layer, thereby improving the flame retardant properties of the diaphragm.
[0027] According to some embodiments of the present application, the raw materials for preparing the DOPO-melamine include DOPO-OH and melamine.
[0028] According to some embodiments of the present application, the molar ratio of DOPO-OH to melamine is 1:0.9-1.1.
[0029] According to some embodiments of the present application, the particle size of the aluminum oxide is 20 nm to 50 nm.
[0030] According to some embodiments of the present application, raw materials for preparing the silica sol include tetraethoxysilane and a catalyst.
[0031] The second aspect of the present application provides a method for preparing the composite flame-retardant diaphragm for a lithium battery according to the first aspect of the present application, comprising the following steps:
[0032] Electrospinning is used to form a modified layer on at least one side of the polypropylene diaphragm body.
[0033] According to some embodiments of the present application, the method for preparing the silica-modified PVA fiber comprises the following steps:
[0034] Mixing silane polyethylene glycol carboxyl, ethanol and water and reacting them to obtain a first mixture;
[0035] The first mixture, ammonium polyphosphate and ethanol are mixed and reacted to obtain modified ammonium polyphosphate;
[0036] Mixing PVA and water to prepare a PVA solution;
[0037] The modified ammonium polyphosphate, PVA solution and silica sol were mixed and then electrospun.
[0038] According to some embodiments of the present application, the method for preparing the flame retardant comprises the following steps:
[0039] DOPO-OH, melamine and water are mixed and reacted.
[0040] According to some embodiments of the present application, the reaction temperature is 60°C to 80°C. BRIEF DESCRIPTION OF THE DRAWINGS
[0041] In order to more clearly illustrate the embodiments of the present drawings or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present drawings. For ordinary technicians in this field, other drawings can be obtained based on the structures shown in these drawings without paying any creative work.
[0042] Figure 1 It is a schematic diagram of the cross-sectional structure in an embodiment of the present application.
[0043] Description of Figure Numbers:
[0044] 100. Polypropylene diaphragm body; 101. First modified layer; 102. Second modified layer.
[0045] The purpose, features and advantages of this figure will be further described in conjunction with the embodiments with reference to the accompanying drawings. DETAILED DESCRIPTION
[0046] In order to make the purpose, technical solutions and advantages of the present application clearer, the present application is described and illustrated below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present application and are not intended to limit the present application. Based on the embodiments provided in the present application, all other embodiments obtained by ordinary technicians in the field without making creative work are within the scope of protection of the present application.
[0047] Obviously, the following descriptions are only some examples or embodiments of the present application. For ordinary technicians in this field, the present application can also be applied to other similar scenarios without creative work. In addition, it can also be understood that although the efforts made in this development process may be complicated and lengthy, for ordinary technicians in the field related to the content disclosed in this application, some changes in design, manufacturing or production based on the technical content disclosed in this application are just conventional technical means, and should not be understood as insufficient content disclosed in this application.
[0048] However, unnecessary detailed descriptions may be omitted. For example, detailed descriptions of well-known matters and repeated descriptions of substantially the same structures may be omitted. This is to avoid the following description from becoming unnecessarily lengthy and to facilitate understanding by those skilled in the art. In addition, the following description is provided for those skilled in the art to fully understand the present application and is not intended to limit the subject matter described in the claims.
[0049] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.
[0050] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form a new technical solution.
[0051] "Scope" disclosed in the present application is limited in the form of lower limit and upper limit, and a given range is limited by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundary of a special range. The scope limited in this way can be including end values or not including end values, and can be arbitrarily combined, that is, any lower limit can be combined with any upper limit to form a scope. For example, if the scope of 60-120 and 80-110 is listed for a specific parameter, it is understood that the scope of 60-110 and 80-120 is also expected. In addition, if the minimum range values 1 and 2 are listed, and if the maximum range values 3, 4 and 5 are listed, the following scope can be all expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5. In the present application, unless otherwise specified, the numerical range "ab" represents the abbreviation of any real number combination between a and b, wherein a and b are real numbers. For example, the numerical range "0-5" means that all real numbers between "0-5" are listed in this document, and "0-5" is just an abbreviation of these numerical combinations. In addition, when a parameter is expressed as an integer ≥ 2, it is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.
[0052] If there is no special explanation, all steps of the present application can be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), which means that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), which means that step (c) may be added to the method in any order. For example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.
[0053] If there is no special explanation, the "include" and "comprising" mentioned in this application are open-ended or closed-ended. For example, the "include" and "comprising" may mean that other components not listed may also be included or only the listed components may be included or only the listed components may be included.
[0054] If not specifically stated, in this application, the term "or" is inclusive. For example, the phrase "A or B" means "A, B, or both A and B". More specifically, any of the following conditions satisfies the condition "A or B": A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).
[0055] The properties of some raw materials in this application are as follows:
[0056] Alumina, particle size 20nm~50nm.
[0057] The preparation method of DOPO-OH in this application consists of the following steps:
[0058] DOPO (CAS No.: 35948-25-5) and hydrogen peroxide (mass fraction 30%) were mixed and refluxed at 80° C. for 6 hours. After the reaction was completed, solid-liquid separation was performed, and the solid phase was collected and dried at 100° C. for 12 hours to obtain DOPO-OH.
[0059] DOPO-OH, melamine (the molar ratio of DOPO-OH to melamine is 1:1) and water (melamine) were mixed and reacted at 70°C for 5 hours. After the reaction was completed, the solid phase was collected by filtration and dried at 100°C for 12 hours to obtain DOPO-melamine.
[0060] Example 1
[0061] This embodiment is a composite flame retardant diaphragm for lithium batteries. The cross-sectional results are as follows Figure 1 As shown, it includes a polypropylene diaphragm body 100 (Celgard2500, thickness is 25 μm);
[0062] A first modified layer 101 is provided on one side of the polypropylene diaphragm body 100;
[0063] A second modified layer 102 is provided on the other side of the polypropylene diaphragm body 100;
[0064] The first modified layer 101 and the second modified layer 102 are prepared using the same raw materials and the same preparation method;
[0065] The modified layers (i.e., the first modified layer and the second modified layer) include the following preparation materials:
[0066] 100 parts of polyimide (soluble polyimide, PY5006T, Suzhou Pinyu Optoelectronics Technology Co., Ltd.), 6 parts of flame retardant (DOPO-melamine), 3 parts of alumina and 13 parts of silica-modified PVA fibers;
[0067] The preparation method of the composite flame-retardant separator for lithium batteries in this embodiment is composed of the following steps:
[0068] S1. Preparation of modified slurry:
[0069] The polyimide, flame retardant, alumina, silica-modified PVA fiber and solvent (the volume ratio of N,N-dimethylacetamide (DMAC) to methyl pyrrolidone (NMP) is 8:2, and the mass ratio of solvent to polyimide is 5:1) are uniformly mixed to prepare a modified slurry;
[0070] S2, using electrostatic spinning to form a first modified layer and a second modified layer on both sides of a polypropylene diaphragm body (width 20 cm*length 30 cm) to obtain a composite flame-retardant diaphragm for a lithium battery;
[0071] The spinning parameters are:
[0072] The relative humidity was 40% and the injection speed was 0.1 mm / min;
[0073] The spinning voltage was 8 KV, the receiving distance was 15 cm, and the temperature was 25°C.
[0074] The silica-modified PVA fiber in this embodiment includes the following raw materials in parts by weight:
[0075] 100 parts of PVA, 18 parts of silica sol, 12 parts of ammonium polyphosphate (CAS No.: 68333-79-9, degree of polymerization of 30-50, purchased from Maclean, item No. A875115) and 1.8 parts of silane polyethylene glycol carboxyl (Silane-PEG2000-COOH, Mw is 2000);
[0076] The preparation method of silica-modified PVA fiber in this embodiment consists of the following steps:
[0077] S1. Dissolve PVA (PVA1799, degree of polymerization of 1.7K, degree of alcoholysis of 99%) in water (the dissolving temperature is 90°C, and the dissolving time is 3h) to obtain a PVA solution (the mass fraction of the PVA solution is 12%).
[0078] TEOS (tetraethoxysilane), H3PO4, and H2O were mixed in a molar ratio of 1:0.01:11, and stirred at 25°C for 12 h to obtain SiO2 sol;
[0079] Mixing silane polyethylene glycol carboxyl, ethanol and distilled water in a mass ratio of 20, 72 and 8, and stirring at 50° C. for 30 min to obtain a first mixture;
[0080] Then, the first mixture, ammonium polyphosphate and ethanol (the mass volume ratio of ammonium polyphosphate to ethanol is 1:3) are mixed, stirred at 60° C. for 1 h, ball-milled to a D50 of 1 μm, solid-liquid separated, and the solid phase is dried at 60° C. for 4 h to obtain modified ammonium polyphosphate.
[0081] The PVA solution, SiO2 sol and modified ammonium polyphosphate were mixed and stirred at 1000 r / min for 4 h to obtain an electrospinning solution.
[0082] S2, spinning the electrospinning solution in an electrospinning machine, the parameters of the spinning process are as follows:
[0083] The relative humidity was 40% and the spinning solution injection speed was 0.05 mm / min;
[0084] The spinning voltage was 17 kV, the receiving distance was 25 cm, and the temperature was 25°C.
[0085] After spinning, the spinning product was placed in an oven at 80°C for 2 hours to dry out the moisture to obtain silica-modified PVA fibers.
[0086] Example 2
[0087] This embodiment is a composite flame-retardant diaphragm for lithium batteries, which differs from Embodiment 1 in that:
[0088] The modified layers (i.e., the first modified layer and the second modified layer) include the following preparation materials:
[0089] 100 parts of polyimide (soluble polyimide, PY5006T, Suzhou Pinyu Optoelectronics Technology Co., Ltd.), 5 parts of flame retardant (DOPO-melamine), 4 parts of alumina and 12 parts of silica-modified PVA fibers.
[0090] The silica-modified PVA fiber in this embodiment includes the following raw materials in parts by weight:
[0091] 100 parts of PVA, 20 parts of silica sol, 8 parts of ammonium polyphosphate (CAS No.: 68333-79-9, degree of polymerization of 30-50, purchased from McLean, item No. A875115) and 2 parts of silane polyethylene glycol carboxyl (Silane-PEG2000-COOH, Mw is 2000).
[0092] The preparation method of the diaphragm in this example is carried out with reference to Example 1.
[0093] Example 3
[0094] This embodiment is a composite flame-retardant diaphragm for lithium batteries, which differs from Embodiment 1 in that:
[0095] The modified layers (i.e., the first modified layer and the second modified layer) include the following preparation materials:
[0096] 100 parts of polyimide (soluble polyimide, PY5006T, Suzhou Pinyu Optoelectronics Technology Co., Ltd.), 7 parts of flame retardant (DOPO-melamine), 2 parts of alumina and 14 parts of silica-modified PVA fibers.
[0097] The silica-modified PVA fiber in this embodiment includes the following raw materials in parts by weight:
[0098] 100 parts of PVA, 10 parts of silica sol, 15 parts of ammonium polyphosphate (CAS No.: 68333-79-9, degree of polymerization of 30-50, purchased from McLean, item No. A875115) and 1 part of silane polyethylene glycol carboxyl (Silane-PEG2000-COOH, Mw is 2000).
[0099] The preparation method of the diaphragm in this example is carried out with reference to Example 1.
[0100] Example 4
[0101] This embodiment is a composite flame-retardant diaphragm for lithium batteries, which differs from Embodiment 1 in that:
[0102] The modified layers (i.e., the first modified layer and the second modified layer) include the following preparation materials:
[0103] 100 parts of polyimide (soluble polyimide, PY5006T, Suzhou Pinyu Optoelectronics Technology Co., Ltd.), 7 parts of flame retardant (DOPO-melamine), 4 parts of alumina and 14 parts of silica-modified PVA fibers.
[0104] The silica-modified PVA fiber in this embodiment includes the following raw materials in parts by weight:
[0105] 100 parts of PVA, 20 parts of silica sol, 15 parts of ammonium polyphosphate (CAS No.: 68333-79-9, degree of polymerization of 30-50, purchased from McLean, item No. A875115) and 2 parts of silane polyethylene glycol carboxyl (Silane-PEG2000-COOH, Mw is 2000).
[0106] The preparation method of the diaphragm in this example is carried out with reference to Example 1.
[0107] Example 5
[0108] This embodiment is a composite flame-retardant diaphragm for lithium batteries, which differs from Embodiment 1 in that:
[0109] The modified layers (i.e., the first modified layer and the second modified layer) include the following preparation materials:
[0110] 100 parts of polyimide (soluble polyimide, PY5006T, Suzhou Pinyu Optoelectronics Technology Co., Ltd.), 5 parts of flame retardant (DOPO-melamine), 2 parts of alumina and 12 parts of silica-modified PVA fibers.
[0111] The silica-modified PVA fiber in this embodiment includes the following raw materials in parts by weight:
[0112] 100 parts of PVA, 10 parts of silica sol, 8 parts of ammonium polyphosphate (CAS No.: 68333-79-9, degree of polymerization of 30-50, purchased from McLean, product No. A875115) and 1 part of silane polyethylene glycol carboxyl (Silane-PEG2000-COOH, Mw is 2000).
[0113] The preparation method of the diaphragm in this example is carried out with reference to Example 1.
[0114] Comparative Example 1
[0115] This comparative example is a separator for lithium batteries, which differs from Example 5 in that:
[0116] The silica-modified PVA fiber in this comparative example includes the following raw materials in parts by weight:
[0117] 100 parts of PVA, 10 parts of silica sol and 8 parts of ammonium polyphosphate (CAS No.: 68333-79-9, degree of polymerization of 30 to 50, purchased from McLean, product No. A875115).
[0118] The preparation method of silica-modified PVA fiber in this comparative example consists of the following steps:
[0119] S1. Dissolve PVA (PVA1799, degree of polymerization of 1.7K, degree of alcoholysis of 99%) in water (the dissolving temperature is 90°C, and the dissolving time is 3h) to obtain a PVA solution (the mass fraction of the PVA solution is 12%).
[0120] TEOS (tetraethoxysilane), H3PO4, and H2O were mixed in a molar ratio of 1:0.01:11, and stirred at 25°C for 12 h to obtain SiO2 sol;
[0121] Ammonium polyphosphate was mixed with ethanol (the mass volume ratio of ammonium polyphosphate to ethanol was 1:3), stirred at 60°C for 1 hour, ball-milled until D50 was 1 μm, solid-liquid separated, and the solid phase was dried at 60°C for 4 hours to obtain modified ammonium polyphosphate.
[0122] The PVA solution, SiO2 sol and modified ammonium polyphosphate were mixed and stirred at 1000 r / min for 4 h to obtain an electrospinning solution.
[0123] S2, spinning the electrospinning solution in an electrospinning machine, the parameters of the spinning process are as follows:
[0124] The relative humidity was 40% and the spinning solution injection speed was 0.05 mm / min;
[0125] The spinning voltage was 17 kV, the receiving distance was 25 cm, and the temperature was 25°C.
[0126] After spinning, the spinning product was placed in an oven at 80°C for 2 hours to dry out the moisture to obtain silica-modified PVA fibers.
[0127] Comparative Example 2
[0128] This comparative example is a separator for lithium batteries, which differs from Example 5 in that:
[0129] The modified layers (i.e., the first modified layer and the second modified layer) include the following preparation materials:
[0130] 100 parts of polyimide (soluble polyimide, PY5006T, Suzhou Pinyu Optoelectronics Technology Co., Ltd.), 5 parts of flame retardant (DOPO-melamine), 2 parts of alumina and 12 parts of silica-modified PVA fibers.
[0131] The silica-modified PVA fiber in this comparative example includes the following raw materials in parts by weight:
[0132] 100 parts of PVA, 10 parts of silica sol and 1 part of silane polyethylene glycol carboxyl (Silane-PEG2000-COOH, Mw is 2000).
[0133] The preparation method of silica-modified PVA fiber in this comparative example consists of the following steps:
[0134] S1. Dissolve PVA (PVA1799, degree of polymerization of 1.7K, degree of alcoholysis of 99%) in water (the dissolving temperature is 90°C, and the dissolving time is 3h) to obtain a PVA solution (the mass fraction of the PVA solution is 12%).
[0135] TEOS (tetraethoxysilane), H3PO4, and H2O were mixed in a molar ratio of 1:0.01:11, and stirred at 25°C for 12 h to obtain SiO2 sol;
[0136] The PVA solution, SiO2 sol and silane polyethylene glycol carboxyl were mixed and stirred at 1000 r / min for 4 h to obtain an electrospinning solution.
[0137] S2, spinning the electrospinning solution in an electrospinning machine, the parameters of the spinning process are as follows:
[0138] The relative humidity was 40% and the spinning solution injection speed was 0.05 mm / min;
[0139] The spinning voltage was 17 kV, the receiving distance was 25 cm, and the temperature was 25°C.
[0140] After spinning, the spinning product was placed in an oven at 80°C for 2 hours to dry out the moisture to obtain silica-modified PVA fibers.
[0141] Comparative Example 3
[0142] This comparative example is a separator for lithium batteries, which differs from Example 5 in that:
[0143] DOPO-melamine was replaced by DOPO (equal mass).
[0144] Comparative Example 4
[0145] This comparative example is a separator for lithium batteries, which differs from Example 5 in that:
[0146] DOPO-melamine was replaced by melamine (equal mass).
[0147] Comparative Example 5
[0148] This comparative example is a separator for lithium batteries, which differs from Example 5 in that:
[0149] The silica-modified PVA fiber in this comparative example includes the following raw materials in parts by weight:
[0150] 100 parts of PVA and 10 parts of silica sol.
[0151] The preparation method of silica-modified PVA fiber in this comparative example consists of the following steps:
[0152] S1. Dissolve PVA (PVA1799, degree of polymerization of 1.7K, degree of alcoholysis of 99%) in water (the dissolving temperature is 90°C, and the dissolving time is 3h) to obtain a PVA solution (the mass fraction of the PVA solution is 12%).
[0153] TEOS (tetraethoxysilane), H3PO4, and H2O were mixed in a molar ratio of 1:0.01:11, and stirred at 25°C for 12 h to obtain SiO2 sol;
[0154] The PVA solution and SiO2 sol were mixed and stirred at 1000 r / min for 4 h to obtain an electrospinning solution.
[0155] S2, spinning the electrospinning solution in an electrospinning machine, the parameters of the spinning process are as follows:
[0156] The relative humidity was 40% and the spinning solution injection speed was 0.05 mm / min;
[0157] The spinning voltage was 17 kV, the receiving distance was 25 cm, and the temperature was 25°C.
[0158] After spinning, the spinning product was placed in an oven at 80°C for 2 hours to dry out the moisture to obtain silica-modified PVA fibers.
[0159] The performance of the diaphragms prepared in the above examples and comparative examples was tested, and the results are shown in Table 1. The test items are as follows:
[0160] Membrane breaking temperature:
[0161] The film breaking temperature is measured by the resistance mutation method, and the point where the resistance suddenly increases is the film breaking temperature;
[0162] LOI Test:
[0163] According to the ASTM D2863-23 test standard, the standard size of the specimen is 130 × 6.5 × 3.2 mm 3 ;.
[0164] Table 1
[0165]
[0166]
[0167] It can be seen from Table 1 that the membrane rupture temperature and LOI value of the separators in Examples 1 to 5 are high; they have excellent high temperature resistance and flame retardancy, which is beneficial to improving the safety performance of lithium batteries.
[0168] It should be noted that the present application is not limited to the above-mentioned embodiments. The above-mentioned embodiments are only examples, and the embodiments having the same structure as the technical idea and exerting the same effect within the scope of the technical solution of the present application are all included in the technical scope of the present application. In addition, without departing from the scope of the main purpose of the present application, various modifications that can be thought of by those skilled in the art to the embodiments and other methods of combining some of the constituent elements in the embodiments are also included in the scope of the present application.
Claims
1. A composite flame retardant diaphragm for lithium batteries, It is characterized in that including a polypropylene diaphragm body; A modified layer is provided on either side of the polypropylene diaphragm body; The modified layer comprises the following preparation raw materials: Polyimide, flame retardant, alumina and silica modified PVA fiber; The silica-modified PVA fiber comprises the following preparation raw materials: PVA, silica sol, ammonium polyphosphate and silane polyethylene glycol carboxyl.
2. The composite flame-retardant separator for lithium battery according to claim 1, It is characterized in that The modified layer includes the following raw materials in parts by weight: 100 parts of polyimide, 5 to 7 parts of flame retardant, 2 to 4 parts of alumina and 12 to 14 parts of silica-modified PVA fiber; And / or, the raw materials for preparing the modified layer further include a solvent.
3. The composite flame-retardant separator for lithium battery according to claim 1, It is characterized in that The silica-modified PVA fiber comprises the following raw materials in parts by weight: 100 parts of PVA, 10-20 parts of silica sol, 8-15 parts of ammonium polyphosphate and 1-2 parts of silane polyethylene glycol carboxyl; And / or, the degree of polymerization of the PVA is 15K to 18K; And / or, the raw materials for preparing the silica-modified PVA fiber also include a solvent.
4. The composite flame-retardant separator for lithium battery according to claim 1, It is characterized in that The thickness of the polypropylene diaphragm body is 5 μm to 30 μm.
5. The composite flame-retardant separator for lithium battery according to claim 1, It is characterized in that The flame retardant includes DOPO-melamine; And / or, the raw materials for preparing the DOPO-melamine include DOPO-OH and melamine; And / or, the molar ratio of DOPO-OH to melamine is 1:0.9-1.
1.
6. The composite flame-retardant separator for lithium battery according to claim 1, It is characterized in that The particle size of the aluminum oxide is 20nm to 50nm.
7. The composite flame-retardant separator for lithium battery according to claim 1, It is characterized in that The raw materials for preparing the silica sol include tetraethoxysilane and a catalyst.
8. A method for preparing a composite flame-retardant separator for a lithium battery according to any one of claims 1 to 7, It is characterized in that The following steps are involved: Electrospinning is used to form a modified layer on at least one side of the polypropylene diaphragm body.
9. The preparation method according to claim 8, It is characterized in that The preparation method of the silica-modified PVA fiber comprises the following steps: Mixing silane polyethylene glycol carboxyl, ethanol and water and reacting them to obtain a first mixture; The first mixture, ammonium polyphosphate and ethanol are mixed and reacted to obtain modified ammonium polyphosphate; Mixing PVA and water to prepare a PVA solution; The modified ammonium polyphosphate, PVA solution and silica sol were mixed and then electrospun.
10. The preparation method according to claim 8, It is characterized in that The method for preparing the flame retardant comprises the following steps: DOPO-OH, melamine and water are mixed and reacted; And / or, the reaction temperature is 60°C to 80°C.
Citation Information
Patent Citations
Flame-retardant composite material with DOPO (9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide) modified nano mesoporous molecular sieve
CN102675895A
Halogen-free flame-retardant polypropylene fiber and preparation method thereof
CN103173884A
Flame-retardant expandable polymers
CN103608388A
Safe flame-retardant polyimide diaphragm and preparation method thereof
CN114284634A
Isolating membrane and battery
CN117937050A
Cited By
High-density flame-retardant battery film and preparation method thereof
CN119627366A