Perovskite battery and preparation method thereof
By adding imidazole sulfonate to the perovskite precursor, the defects and non-radiative recombination of perovskite films are suppressed, and the efficiency loss caused by film defects in perovskite batteries is solved, which significantly improves the performance of the battery and photoelectric conversion. efficiency.
Patent Information
- Application Number
- CN202411004310.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-25
- Publication Date
- 2024-11-15
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Defects at the thin film surface and grain boundaries in perovskite batteries lead to losses in open circuit voltage and power conversion efficiency, and a modified perovskite film layer is required to improve battery efficiency.
Imidazole sulfonate is added to the perovskite precursor, and through the binding of imidazole ions and sulfonic acid groups, non-radiative recombination is inhibited, crystal growth is regulated, film defects are reduced, energy levels are optimized, and battery performance is improved.
Through the addition of imidazole sulfonate, the film defects are effectively passivated, non-radiative recombination is inhibited, the crystallization quality and battery performance of the perovskite layer are improved, and the photoelectric conversion efficiency is improved.
Smart Images

Figure CN118973288A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of battery preparation, and in particular relates to a perovskite battery and a preparation method thereof. Background Art
[0002] Solar cells are a technology that converts natural energy into usable energy. Perovskite is an excellent solar material with high electron mobility, high carrier lifetime, high absorption coefficient, and high photoelectric luminescence quantum efficiency. Although significant progress has been made in improving the efficiency of perovskite cells, there is still room for further development in the efficiency of perovskite cells. A large number of defects are inevitably formed on the surface and grain boundaries of perovskite films. These defects act as non-radiative recombination centers, causing the open circuit voltage and power conversion efficiency of perovskite cells to lose. Therefore, it is necessary to modify the perovskite film layer in perovskite cells to improve the efficiency of perovskite cells. Summary of the invention
[0003] In view of the above problems, the present invention provides a perovskite battery and a preparation method thereof, wherein imidazole sulfonate is added to the perovskite precursor to passivate film defects and inhibit non-radiative recombination, thereby improving battery performance.
[0004] The first object of the present invention is to provide a method for preparing a perovskite battery, comprising:
[0005] After the conductive glass is dried, UV treatment is performed to obtain a substrate;
[0006] Spin-coat NiO on the substrate and heat it to obtain a hole transport layer;
[0007] Spin coating a mixed solution of imidazole sulfonate and perovskite precursor solution on the hole transport layer to prepare a modified perovskite light absorption layer;
[0008] spin coating an electron transport layer on the modified perovskite light absorbing layer;
[0009] A metal electrode is vacuum-deposited on the electron transport layer to obtain a perovskite cell.
[0010] Furthermore, the conductive glass is ITO conductive glass or FTO conductive glass.
[0011] Furthermore, the process of spin coating NiO on the substrate substrate is as follows: the spin coating speed is 2000-5000 rpm, the spin coating time is 20-50s, the heating temperature is 80-120°C, and the heating time is 10-20min.
[0012] Furthermore, in the mixed solution of the imidazole sulfonate and the perovskite precursor solution, the mass of the imidazole sulfonate added per milliliter of the perovskite precursor solution is 0.1 mg-10 mg.
[0013] Furthermore, the imidazole sulfonate includes one or more of 1-methylimidazole trifluoromethane sulfonate, 1-methylimidazole p-toluene sulfonate, 1-ethylimidazole p-toluene sulfonate, 1,3-dimethylimidazole trifluoromethane sulfonate, 1-butyl-3-methylimidazole methane sulfonate, and 1-butyl-3-methylimidazole trifluoromethane sulfonate.
[0014] Furthermore, the specific operation of spin coating the mixed solution of imidazole sulfonate and perovskite precursor solution on the hole transport layer is as follows: spin coating the mixed solution of imidazole sulfonate and perovskite precursor solution at a rotation speed of 2000-5000 rpm for 20-60s, and then heating at 100-150°C for 10-60min.
[0015] Furthermore, the process of spin coating the electron transport layer on the modified perovskite light absorption layer is: the spin coating speed is 2000-5000rpm, and the spin coating time is 20-60s; the electron transport layer is one or more of fullerene and fullerene derivatives.
[0016] Furthermore, the electrode thickness of the metal electrode is 80-140 nm, and the metal electrode is one or more of Au, Ag, Al, and Cu.
[0017] The second object of the present invention is to provide a perovskite cell, which is prepared by the above-mentioned preparation method.
[0018] The third object of the present invention is to provide the use of imidazole sulfonate as a perovskite precursor additive in the above-mentioned perovskite battery.
[0019] Beneficial effects of the present invention:
[0020] The present invention provides a perovskite battery and a preparation method thereof. By adding imidazole sulfonate to the perovskite precursor solution, the imidazole ion has low vapor pressure, is difficult to volatilize, has good solubility, and is an amphoteric compound. The imidazole ion is introduced into the perovskite precursor solution by combining the imidazole ion and the sulfonic acid group, and is evenly mixed with the perovskite precursor solution. The uniformity of the perovskite film is not affected, and the film defects can be passivated, non-radiative recombination can be inhibited, and good crystal quality of the perovskite layer can be obtained, thereby improving the battery performance. In addition, the O on the S=O bond in the sulfonic acid ion and the Pb in the perovskite are bonded to each other. 2+ Pb-O bonds are formed between the ions, and there is a Pb-O bond intermolecular interaction between the sulfonic acid group and the perovskite, thereby regulating the perovskite crystal.
[0021] Imidazole sulfonate is added to the perovskite precursor solution. The imidazole sulfonate reacts with Pb 2+The strong interaction of ions, self-assembly on the film surface and grain boundaries, effectively inhibits ion migration, controls crystal growth, reduces film defects, reduces trap-related non-radiative recombination, and improves film quality. In addition, imidazole sulfonates distributed on the top surface of perovskite can reduce interface recombination, optimize energy levels, and improve battery performance.
[0022] Other features and advantages of the present invention will be described in the following description, and partly become apparent from the description, or understood by practicing the present invention. The purpose and other advantages of the present invention can be realized and obtained by the structures pointed out in the description, claims and drawings. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the following briefly introduces the drawings required for use in the embodiments or the description of the prior art. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0024] Figure 1 A schematic structural diagram of a perovskite battery according to an embodiment of the present invention is shown;
[0025] Figure 2 The JV curve diagram of the perovskite battery prepared according to Example 1 and Comparative Example 1 of the present invention is shown;
[0026] In the figure:
[0027] 1. Substrate; 2. Hole transport layer; 3. Modified perovskite light absorption layer; 4. Organic electron transport layer; 5. Metal electrode. DETAILED DESCRIPTION
[0028] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0029] like Figure 1 As shown, a perovskite cell includes, from bottom to top, a substrate substrate 1, a hole transport layer 2, a modified perovskite light absorption layer 3, an organic electron transport layer 4 and a metal electrode 5.
[0030] The method for preparing the perovskite battery comprises:
[0031] Step 1: After the conductive glass is dried, UV treatment is performed to obtain a substrate substrate 1 (i.e., a battery anode);
[0032] Step 2: Spin-coating NiO on the substrate 1 and heating to obtain the hole transport layer 2;
[0033] Step 3: spin-coating a mixed solution of imidazole sulfonate and perovskite precursor solution on the hole transport layer 2 to obtain a modified perovskite light absorption layer 3;
[0034] Step 4: spin-coating the electron transport layer 4 on the modified perovskite light absorption layer 3;
[0035] Step 5: vacuum evaporate a metal electrode 5 (i.e., a battery anode) on the electron transport layer 4 to obtain a perovskite battery.
[0036] In step 1, the conductive glass is ITO (abbreviation for Indium-Tin Oxide, meaning indium tin oxide) conductive glass or FTO (abbreviation for Fluorine-doped Tin Oxide, meaning fluoride tin doped tin oxide) conductive glass.
[0037] In step 2, the process of spin coating NiO on the substrate substrate is as follows: the spin coating speed is 2000-5000 rpm, the spin coating time is 20-50 s, the heating temperature is 80-120° C., and the heating time is 10-20 min;
[0038] Specifically, in step 2, the spin coating speed is any one of 2000rpm, 2100rpm, 2200rpm, 2300rpm, 2400rpm, 2500rpm, 2600rpm, 2700rpm, 2800rpm, 2900rpm, 3000rpm, 3100rpm, 3200rpm, 3300rpm, 3400rpm, 3500rpm, 3600rpm, 3700rpm, 3800rpm, 3900rpm, 4000rpm, 4100rpm, 4200rpm, 4300rpm, 4400rpm, 4500rpm, 4600rpm, 4700rpm, 4800rpm, 4900rpm, and 5000rpm;
[0039] The spin coating time is any one of 20s, 21s, 22s, 23s, 24s, 25s, 26s, 27s, 28s, 29s, 30s, 31s, 32s, 33s, 34s, 35s, 36s, 37s, 38s, 39s, 40s, 41s, 42s, 43s, 44s, 45s, 46s, 47s, 48s, 49s, and 50s;
[0040] The heating temperature is any one of 80°C, 81°C, 82°C, 83°C, 84°C, 85°C, 86°C, 87°C, 88°C, 89°C, 90°C, 91°C, 92°C, 93°C, 94°C, 95°C, 96°C, 97°C, 98°C, 99°C, 100°C, 101°C, 102°C, 103°C, 104°C, 105°C, 106°C, 107°C, 108°C, 109°C, 110°C, 111°C, 112°C, 113°C, 114°C, 115°C, 116°C, 117°C, 118°C, 119°C, and 120°C;
[0041] The heating time is any one of 10 min, 11 min, 12 min, 13 min, 14 min, 15 min, 16 min, 17 min, 18 min, 19 min, and 20 min.
[0042] In step 3, in the mixed solution of the imidazole sulfonate and the perovskite precursor solution, the mass of the imidazole sulfonate added per milliliter of the perovskite precursor solution is 0.1 mg-10 mg, specifically 0.1 mg / mL, 0.2 mg / mL, 0.3 mg / mL, 0.4 mg / mL, 0.5 mg / mL, 0.6 mg / mL, 0.7 mg / mL, 0.8 mg / mL, 0.9 mg / mL, 1 mg / mL, 1.1 mg / mL, 1.2 mg / mL, 1.3 mg / mL, 1.4 mg / mL, 1.5 mg / mL, 1.6 mg / mL, 1.7 mg / mL, 1.8 mg / mL, 1.9 mg / mL L, 2mg / mL, 2.1mg / mL, 2.2mg / mL, 2.3mg / mL, 2.4mg / mL, 2.5mg / mL, 2.6mg / mL, 2.7mg / mL, 2.8mg / mL, 2.9mg / mL, 3mg / mL, 3.1mg / mL, 3.2mg / mL, 3.3m g / mL, 3.4mg / mL, 3.5mg / mL, 3.6mg / mL, 3.7mg / mL, 3.8mg / mL, 3.9mg / mL, 4mg / mL, 4.1mg / mL, 4.2mg / mL, 4.3mg / mL, 4.4mg / mL, 4.5mg / mL, 4.6mg / mL , 4.7mg / mL, 4.8mg / mL, 4.9mg / mL, 5mg / mL, 5.1mg / mL, 5.2mg / mL, 5.3mg / mL, 5.4mg / mL, 5.5mg / mL, 5.6mg / mL, 5.7mg / mL, 5.8mg / mL, 5.9mg / mL, 6mg / mL, 6.1mg / mL, 6.2mg / mL, 6.3mg / mL, 6.4mg / mL, 6.5mg / mL, 6.6mg / mL, 6.7mg / mL, 6.8mg / mL, 6.9mg / mL, 7mg / mL, 7.1mg / mL, 7.2mg / mL, 7.3mg / mL, 7.4mg / mL, 7.5mg / mL, 7.6mg / mL, 7.7mg / mL, 7.8mg / mL, 7.9mg / mL, 8mg / mL, 8.1mg / mL, 8.2mg / mL, 8.3mg / mL, 8.4mg / mL, 8.5mg / mL, 8.6mg / mL, 8.7m g / mL, 8.8mg / mL, 8.9mg / mL, 9mg / mL, 9.1mg / mL, 9.2mg / mL, 9.3mg / mL, 9.4mg / mL, 9.5mg / mL, 9.6mg / mL, 9.7mg / mL, 9.8mg / mL, 9.9mg / mL or 10mg / mL;
[0043] The perovskite precursor solution is Cs 0.05FA 0.8 MA 0.2 Pb(I 0.85 Br 0.15 )3, the concentration of the precursor solution is 1M-1.6M, and the specific concentration values are 1M, 1.1M, 1.2M, 1.3M, 1.4M, 1.5M or 1.6M;
[0044] The imidazole sulfonate includes one or more of 1-methylimidazole trifluoromethane sulfonate, 1-methylimidazole p-toluene sulfonate, 1-ethylimidazole p-toluene sulfonate, 1,3-dimethylimidazole trifluoromethane sulfonate, 1-butyl-3-methylimidazole methane sulfonate, and 1-butyl-3-methylimidazole trifluoromethane sulfonate.
[0045] In step 4, the specific operation of spin coating the mixed solution of imidazole sulfonate and perovskite precursor solution on the hole transport layer is as follows: spin coating the mixed solution of imidazole sulfonate and perovskite precursor solution at a rotation speed of 2000-5000 rpm for 20-60 seconds, and then heating at a temperature of 100-150° C. for 10-60 minutes;
[0046] Specifically, in step 4, the rotation speed is any one of 2000rpm, 2100rpm, 2200rpm, 2300rpm, 2400rpm, 2500rpm, 2600rpm, 2700rpm, 2800rpm, 2900rpm, 3000rpm, 3100rpm, 3200rpm, 3300rpm, 3400rpm, 3500rpm, 3600rpm, 3700rpm, 3800rpm, 3900rpm, 4000rpm, 4100rpm, 4200rpm, 4300rpm, 4400rpm, 4500rpm, 4600rpm, 4700rpm, 4800rpm, 4900rpm, and 5000rpm;
[0047] The specific time of the spin coating 20-60s is any one of 20s, 21s, 22s, 23s, 24s, 25s, 26s, 27s, 28s, 29s, 30s, 31s, 32s, 33s, 34s, 35s, 36s, 37s, 38s, 39s, 40s, 41s, 42s, 43s, 44s, 45s, 46s, 47s, 48s, 49s, 50s, 51s, 52s, 53s, 54s, 55s, 56s, 57s, 58s, 59s, and 60s;
[0048] The heating treatment at a temperature of 100-150°C for 10-60 min is any one of 100°C, 101°C, 102°C, 103°C, 104°C, 105°C, 106°C, 107°C, 108°C, 109°C, 110°C, 111°C, 112°C, 113°C, 114°C, 115°C, 116°C, 117°C, 118°C, 119°C, 120°C, 130°C, 131°C, 132°C, 133°C, 134°C, 135°C, 136°C, 137°C, 138°C, 139°C, 140°C, 141°C, 142°C, 143°C, 144°C, 145°C, 146°C, 147°C, 148°C, 149°C, and 150°C;
[0049] The heating treatment time for 10-60 min at a temperature of 100-150°C is any one of 10 min, 11 min, 12 min, 13 min, 14 min, 15 min, 16 min, 17 min, 18 min, 19 min, 20 min, 20 min, 21 min, 22 min, 23 min, 24 min, 25 min, 26 min, 27 min, 28 min, 29 min, 50 min, 51 min, 52 min, 53 min, 54 min, 55 min, 56 min, 57 min, 58 min, 59 min and 60 min.
[0050] In step 5, the process of spin coating an electron transport layer on the modified perovskite layer is: the spin coating speed is 2000-5000 rpm, and the spin coating time is 20-60 s; the electron transport layer is one or more of fullerene and fullerene derivatives, wherein the fullerene is such as fullerene C60, fullerene C70, and the fullerene derivatives are such as PC61BM, PC71BM;
[0051] Specifically, in step five, the spin coating speed is any one of 2000rpm, 2100rpm, 2200rpm, 2300rpm, 2400rpm, 2500rpm, 2600rpm, 2700rpm, 2800rpm, 2900rpm, 3000rpm, 3100rpm, 3200rpm, 3300rpm, 3400rpm, 3500rpm, 3600rpm, 3700rpm, 3800rpm, 3900rpm, 4000rpm, 4100rpm, 4200rpm, 4300rpm, 4400rpm, 4500rpm, 4600rpm, 4700rpm, 4800rpm, 4900rpm, and 5000rpm;
[0052] The spin coating time is any one of 20s, 21s, 22s, 23s, 24s, 25s, 26s, 27s, 28s, 29s, 30s, 31s, 32s, 33s, 34s, 35s, 36s, 37s, 38s, 39s, 40s, 41s, 42s, 43s, 44s, 45s, 46s, 47s, 48s, 49s, 50s, 51s, 52s, 53s, 54s, 55s, 56s, 57s, 58s, 59s, and 60s.
[0053] In step six, the electrode thickness of the metal electrode is 80-140 nm, and the metal electrode is one or more of Au, Ag, Al, and Cu.
[0054] Example 1
[0055] This embodiment provides a method for preparing a perovskite crystalline silicon stacked solar cell using 1-butyl-3-methylimidazolium methanesulfonate as an additive, comprising the following steps:
[0056] 1) The conductive glass substrate plated with indium tin oxide (ITO) was ultrasonically cleaned for 20 minutes using a cleaning solution, ultrapure water, and ethanol in sequence, and the glass substrate was blown dry after cleaning. The glass substrate was treated with ultraviolet-ozone for 20 minutes to obtain a pretreated substrate substrate 1.
[0057] 2) Spin coating NiO on the pre-treated ITO glass surface at a spin coating speed of 3000 rpm for 30 seconds, and then annealing treatment at 100° C. for 10 minutes to form a hole transport layer 2.
[0058] 3) Spin coating perovskite on the hole transport layer: spin coating a mixed solution of imidazole sulfonate and perovskite precursor solution to form a perovskite film, which is the modified perovskite light absorption layer 3. The specific steps are:
[0059] a) preparing a perovskite precursor solution, stirring and dissolving it, and then adding 1-butyl-3-methylimidazolium methanesulfonate, stirring for 1 hour to allow the 1-butyl-3-methylimidazolium methanesulfonate to mix with the perovskite precursor solution;
[0060] b) Spin coating the perovskite: imidazole sulfonate mixed solution on the hole transport layer at 4000 rpm for 40 seconds, and adding the anti-solvent ethyl acetate solution to promote the crystallization of perovskite when the spin coating lasts for 20 seconds. Then, heat at 100°C for 30 minutes to obtain a perovskite film;
[0061] c) In the perovskite precursor solution, the added mass of 1-butyl-3-methylimidazolium methanesulfonate is 1 mg / mL, and the concentration of the perovskite precursor solution is 1.5M.
[0062] 4) Spin-coat the PCBM solution on the perovskite layer at 4000 rpm for 30 s to form an electron transport layer.
[0063] 5) Vacuum evaporate 100 nm Ag on the electron transport layer as an electrode to obtain an inverted perovskite cell.
[0064] The device structure obtained in this embodiment is ITO / NiO / PVK / PCBM / Ag.
[0065] Comparative Example 1:
[0066] Preparation of perovskite crystalline silicon tandem solar cells:
[0067] Compared with Example 1, 1-butyl-3-methylimidazolium methanesulfonate is not added to the perovskite precursor solution in step (3), and the rest is the same.
[0068] The solar cells obtained in Example 1 and Comparative Example 1 were tested for cell performance. The test results are as follows: Figure 2 .
[0069] from Figure 2 It can be seen that the solar cell of Example 1 has a power of 100 mW / cm 2 The open circuit voltage under simulated sunlight is 1.12V and the short circuit current is 20.49mA / cm 2 , the fill factor is 82.79%, the photoelectric conversion efficiency is 19.07%, while the open circuit voltage of the solar cell of comparative example 1 is 1.09V and the short circuit current is 20.60mA / cm 2 , the filling factor is 78.75% and the photoelectric conversion efficiency is 17.80%.
[0070] It can be seen that in Example 1 of the present invention, the photoelectric conversion efficiency of the solar cell is improved by adding the imidazole sulfonate additive to the perovskite precursor.
[0071] Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent substitutions for some of the technical features therein; and these modifications or substitutions do not make the essence of the corresponding technical solutions deviate from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for preparing a perovskite battery, characterized in that: include: After the conductive glass is dried, UV treatment is performed to obtain a substrate; Spin-coat NiO on the substrate and heat it to obtain a hole transport layer; Spin coating a mixed solution of imidazole sulfonate and perovskite precursor solution on the hole transport layer to prepare a modified perovskite light absorption layer; spin coating an electron transport layer on the modified perovskite light absorbing layer; A metal electrode is vacuum-deposited on the electron transport layer to obtain a perovskite cell.
2. The method for preparing a perovskite battery according to claim 1, characterized in that: The conductive glass is ITO conductive glass or FTO conductive glass.
3. The method for preparing a perovskite battery according to claim 1, characterized in that: The process of spin coating NiO on the substrate substrate is as follows: the spin coating speed is 2000-5000rpm, the spin coating time is 20-50s, the heating temperature is 80-120°C, and the heating time is 10-20min.
4. The method for preparing a perovskite battery according to claim 1, characterized in that: In the mixed solution of the imidazole sulfonate and the perovskite precursor solution, the mass of the imidazole sulfonate added per milliliter of the perovskite precursor solution is 0.1 mg-10 mg.
5. The method for preparing a perovskite battery according to claim 1, characterized in that: The imidazole sulfonate includes one or more of 1-methylimidazole trifluoromethane sulfonate, 1-methylimidazole p-toluene sulfonate, 1-ethylimidazole p-toluene sulfonate, 1,3-dimethylimidazole trifluoromethane sulfonate, 1-butyl-3-methylimidazole methane sulfonate, and 1-butyl-3-methylimidazole trifluoromethane sulfonate.
6. The method for preparing a perovskite battery according to claim 1, characterized in that: The specific operation of spin coating the mixed solution of imidazole sulfonate and perovskite precursor solution on the hole transport layer is as follows: spin coating the mixed solution of imidazole sulfonate and perovskite precursor solution at a rotation speed of 2000-5000 rpm for 20-60 seconds, and then heating at 100-150° C. for 10-60 minutes.
7. The method for preparing a perovskite battery according to claim 1, characterized in that: The process of spin coating the electron transport layer on the modified perovskite light absorption layer is as follows: the spin coating speed is 2000-5000 rpm, and the spin coating time is 20-60s; the electron transport layer is one or more of fullerene and fullerene derivatives.
8. A method for preparing a perovskite battery according to any one of claims 1 to 7, characterized in that: The electrode thickness of the metal electrode is 80-140nm, and the metal electrode is one or more of Au, Ag, Al, and Cu.
9. A perovskite battery, characterized in that: The perovskite battery is prepared by the preparation method described in any one of claims 1-8.
10. The use of imidazole sulfonate as a perovskite precursor additive in a perovskite battery, characterized in that: The perovskite cell is the perovskite cell according to claim 9.
Citation Information
Patent Citations
Preparation method of perovskite thin film and perovskite assembly
CN116981321A