Preparation and performance regulation and control method of oxide corner heterojunction with strong magnetic exchange bias effect

By constructing oxide corner heterojunctions, and using pulsed laser molecular beam epitaxial technology to deposit ferromagnetic and antiferromagnetic oxide films, the problem of small exchange bias field strength and difficult to manipulate is solved, and a large exchange bias intensity is achieved and good regulation, suitable for magnetic data storage and sensor fields.

CN118973366APending Publication Date: 2024-11-15UNIV OF JINAN
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411049420.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-01
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

In the prior art, the intensity of the exchange bias field is generally small and difficult to manipulate, making it difficult to effectively improve the performance of exchange bias, especially in the fields of magnetic data storage and sensors.

Method used

By constructing an oxide angle heterojunction with a strong exchange bias effect, using pulsed laser molecular beam epitaxial technology to deposit ferromagnetic and antiferromagnetic oxide films, and by controlling the growth conditions of each layer and the rotation angle during stacking, Regulates the generation, disappearance, growth and decrease of exchange bias.

Benefits of technology

A large exchange bias intensity is achieved, and by regulating the thickness and stacking angle of each layer, the regulation of exchange bias is significantly improved, providing higher stability and sensitivity, suitable for magnetic data storage and sensor fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118973366A_ABST
    Figure CN118973366A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of flexible spin electronic devices, and particularly relates to a preparation method and a performance regulation and control method of an oxide corner heterojunction with a strong magnetic exchange bias effect. The corner magnetic heterojunction with strong interface magnetic coupling is formed by mutually stacking the self-supporting single crystal ferromagnetic oxide thin film and the anti-ferromagnetic oxide thin film with magnetic ordered structures, and the magnetic performance of the corner magnetic heterojunction is regulated and controlled by increasing a covering layer and a stacking angle. According to the invention, the corner magnetic heterojunction is formed by the self-supporting antiferromagnetic layer and the ferromagnetic layer with different magnetic ordered structures, and the exchange bias of the corner magnetic heterojunction is regulated and controlled by controlling the coupling angle and distance. Therefore, the research on the physical mechanism of the corner magnetoelectronics is facilitated, and a material basis and a novel and effective regulation and control means are provided for the multifunctional spintronics material. The abstract drawing is figure 10.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of spin electronics materials, and in particular relates to a method for preparing an oxide turn heterojunction with a strong magnetic exchange bias effect and controlling its performance. Background Art

[0002] The exchange bias effect has been widely used in spin electronics devices such as spin valves and magnetic tunnel junctions; its application potential in magnetic data storage, sensors and other fields is also gradually emerging. These devices use the exchange bias effect to fix the magnetic moment direction of the ferromagnetic layer, thereby improving the stability and sensitivity of the device. Although some materials with excellent exchange bias effects have been discovered, how to further improve the performance of these materials remains a challenge. For example, increasing the intensity of the exchange bias field, reducing the coercive force, and increasing the cutoff temperature. In addition, the controllability of the exchange bias is also a difficult problem to solve. Summary of the invention

[0003] In view of the problem that the intensity of the current exchange bias field is generally small and the exchange bias is difficult to control, the present invention provides a stacked ferromagnetic and antiferromagnetic oxide film heterostructure with a strong exchange bias effect. The structure has a strong exchange bias field, and at the same time, the generation, disappearance, growth, and reduction of the exchange bias can be easily regulated by controlling the growth conditions of each layer (magnetic layer, antiferromagnetic layer, sacrificial layer, and covering layer), as well as the rotation angle during the stacking process. The invention provides many possibilities for further exploration and development in the fields of magnetic data storage, sensors, etc.

[0004] To achieve the above purpose, a corner heterojunction with a strong magnetic exchange bias effect is realized by the following technical scheme:

[0005] (1) using pulsed laser molecular beam epitaxy (LMBE), first depositing a water-soluble sacrificial layer on a single crystal substrate, and then depositing a ferromagnetic oxide film, to obtain a single crystal substrate / sacrificial layer / single crystal ferromagnetic oxide film structure; placing the single crystal substrate / sacrificial layer / single crystal ferromagnetic oxide film structure in an etching solution, and after the sacrificial layer is dissolved, the single crystal ferromagnetic oxide film can be separated from the substrate;

[0006] (2) obtaining a single crystal antiferromagnetic oxide thin film by the same steps as above;

[0007] (3) transferring the flexible self-supporting ferromagnetic layer and antiferromagnetic layer oxide film to the target substrate through a high-precision transfer platform, and stacking them at a certain angle and number of layers to form a multi-layer stacked oxide film corner heterojunction with exchange bias;

[0008] (4) Place the stacked films into LMBE and deposit the cover layer.

[0009] Furthermore, the substrate in step (1) is SrTiO 3 (STO), the sacrificial layer is water-soluble (such as Sr 3 Al 2 O 6 , Sr 3- x Ca x Al 2 O 6 , Sr 4 Al 2 O 7 ), the ferromagnetic oxide is La 1-x Sr x MnO 3 (LSMO), La 1-x Ca x MnO 3 (LCMO), SrRuO 3 、CoFe 2 O 4 wait.

[0010] Furthermore, in step (2), the Néel transition point of the antiferromagnetic oxide is above room temperature, such as NiO.

[0011] Furthermore, the target substrate of step (3) can be selected from silicon, glass, metal, flexible substrate mica, etc.

[0012] Furthermore, in step (4), the cover layer is LaAlO 3 、SrTiO 3 or BaTiO 3 .

[0013] Furthermore, during the epitaxial growth of the sacrificial layer in step (1), the laser energy density is 1-3J / cm2, and the water-soluble sacrificial layer is deposited with a thickness of 1-80nm under the conditions of an oxygen pressure of 5-30Pa and a substrate temperature of 600-800°C; the ferromagnetic and antiferromagnetic single crystal oxide thin films are deposited under a vacuum of 15Pa-30Pa, a temperature of 300-800°C, and a thickness of 5-200nm.

[0014] Furthermore, after the deposition in step (1) is completed, the sample is heated at a growth temperature and an oxygen pressure of 5×10 3 The samples were annealed at 400 Pa for 30 min and then cooled to room temperature at a rate of 5 °C / min.

[0015] Furthermore, in step (3), the etching solution is deionized water; by dissolving the sacrificial layer (such as Sr 3 Al 2 O 6 , Sr 3- x Cax Al 2 O 6 , Sr 4 Al 2 O 7 ), and independent NiO and magnetic films were obtained. Polydimethylsiloxane (PDMS) was used as a support layer to lift, transfer and attach the film to the target substrate using liquid surface tension to complete the stacking.

[0016] Furthermore, in step (4), the covering layer is at an oxygen pressure of 10 3 -10 5 Pa and deposited under room temperature conditions.

[0017] The beneficial effects of the present invention are:

[0018] (1) The present invention forms a heterostructure with strong exchange interaction by stacking ferromagnetic and antiferromagnetic films, which has simple steps and is easy to operate.

[0019] (2) The present invention controls the thickness and stacking angle of each thin film layer, thereby changing the interlayer configuration and interaction, thereby achieving regulation of the exchange bias.

[0020] (3) The formation conditions and thickness of the deposited capping layer of the present invention can also be used to control the exchange bias, providing another simple and feasible method for controlling the exchange bias.

[0021] An oxide corner heterojunction with a strong magnetic exchange bias effect obtained by the above preparation method.

[0022] The mechanism of the present invention is as follows:

[0023] like Figure 1 As shown, the ferromagnetic layer grown in step (1) and step (2) neutralizes the antiferromagnetic layer, and is stacked together in step (3), so that the spin of the ferromagnetic layer can be pinned by the antiferromagnetic layer to generate an exchange bias. By adjusting the hard magnetic axis and the easy magnetic axis of the ferromagnet during the stacking process, the overall magnetic field response of the ferromagnetic (FM) / antiferromagnetic (AFM) film can be easily adjusted, thereby controlling the generation, disappearance, growth, and reduction of the exchange bias. In addition, during the deposition of the capping layer in step (4), by adjusting its growth rate, deposition time, temperature and other conditions, the interlayer coupling of the heterostructure can be significantly affected, thereby changing the strength of the exchange bias.

[0024] The present invention has the following advantages:

[0025] A relatively large exchange bias strength can be obtained, and the exchange bias strength can be easily controlled by the rotation angle during the stacking process and the growth of the covering layer; each layer is an oxide, can be grown on a large area and maintain chemical stability in the air and at room temperature, and is easy to store. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 is La with a stacking angle of 0 degrees 0.67 Sr 0.33 MnO 3 Schematic diagram of NiO corner heterojunction;

[0027] Figure 2 is La with a stacking angle of 0 degrees 0.67 Sr 0.33 MnO 3 / NiO corner heterojunction hysteresis loop;

[0028] Figure 3 is the X-ray diffraction pattern of the corner heterojunction;

[0029] Figure 4 Is to stack La at different angles 0.67 Sr 0.33 MnO 3 Schematic diagram of the method for / NiO corner heterojunction;

[0030] Figure 5 (a) and (b) are morphology images under optical microscope at 10-degree stacking and 30-degree stacking, respectively.

[0031] Figure 6 It is the hysteresis loop when stacked at 20 degrees;

[0032] Figure 7 is a schematic diagram of the growth of the overburden layer;

[0033] Figure 8 is the hysteresis loop after the growth of the cover layer;

[0034] Fig. 9 It is the hysteresis loop of the non-stacked grown LSMO / NiO heterostructure;

[0035] Fig.10 This is a schematic diagram of a corner heterojunction stack. DETAILED DESCRIPTION

[0036] In order to make the purpose of this application clearer, the technical solutions and advantages clearer, the technical solutions of this application will be described in detail and clearly in combination with specific embodiments and corresponding drawings. Obviously, the described embodiments are only part of the embodiments of this application, not all of them. Based on the embodiments in this application, all other embodiments obtained by those skilled in the art without creative work are within the scope of protection of this application.

[0037] The schematic diagram of the stacked magnetic oxide heterostructure with strong magnetic exchange bias effect prepared by the present invention is as follows Figure 1 As shown, the invention will now be described in conjunction with specific embodiments.

[0038] Example 1 La with stacking angle of 0 degrees 0.67 Sr 0.33 MnO 3 Preparation of NiO / NiO corner heterostructures

[0039] (1) Take an STO single crystal substrate, ultrasonically clean it with acetone and ethanol for 5 minutes in sequence, and finally dry it in a nitrogen flow.

[0040] (2) The substrate temperature was raised to 700°C and kept for 30 minutes. After the oxygen pressure in the chamber was adjusted to 7 Pa, Sr was deposited using a pulsed laser. 3 Al 2 O 6 (SAO) sacrificial layer, thickness 45nm;

[0041] (3) After growing the SAO sacrificial layer, use laser to clean the ferromagnetic La 0.67 Sr 0.33 MnO 3 1000 pulses of (LSMO) target, oxygen pressure adjusted to 15Pa, and LSMO film with a thickness of about 80nm was grown;

[0042] (4) Place the STO single crystal substrate from step (1) into the LMBE cavity.

[0043] (5) The substrate temperature was raised to 700°C and kept for 30 minutes. After the oxygen pressure in the cavity was adjusted to 7 Pa, a SAO sacrificial layer with a thickness of 45 nm was deposited using a pulsed laser.

[0044] (6) After the SAO sacrificial layer is grown, the NiO target is cleaned with a laser for 1000 pulses, and then the substrate temperature is raised to 780°C, the oxygen pressure is adjusted to 30 Pa, and a NiO film with a thickness of 10 nm is grown;

[0045] (7) combining the obtained substrate / sacrificial layer / LSMO film with the PDMS support layer, and then immersing the whole in deionized water for etching;

[0046] (8) After the sacrificial layer is completely etched, take out the sample and put it into a beaker filled with deionized water, and use the tension of the deionized water to separate the film from the substrate;

[0047] (9) Start extracting the deionized water. During the extraction process, use a thin stick to gently scratch the deionized water on the side of the film.

[0048] (10) The self-supporting LSMO film was annealed at 60°C for 30 minutes to evaporate the water so that the film was tightly bonded to the substrate.

[0049] (11) Follow steps (8)-(10) to obtain a self-supporting NiO film

[0050] (12) Using a high-precision transfer platform that can be heated to 80-100 degrees for 5-20 minutes, the self-supporting LSMO and self-supporting NiO films are separated from the PDMS. At the same time, the platform can rotate 0-360 degrees in the plane, thereby forming LSMO / NiO angle heterojunctions with different stacking angles on the Si target substrate. The stacking angle of this sample is 0 degrees, which means that the

[100] of LSMO is parallel to the

[100] of NiO, and the

[010] of LSMO is parallel to the

[010] of NiO. In order to obtain a strong exchange bias effect, the antiferromagnetic layer completely covers the LSMO layer.

[0051] Comparative Example 1 Preparation of non-stacked LSMO / NiO heterostructure

[0052] (1) Take an STO single crystal substrate, ultrasonically clean it with acetone and ethanol for 5 minutes in sequence, and finally dry it in a nitrogen flow.

[0053] (2) The LSMO target was cleaned with laser for 1000 pulses, the oxygen pressure was adjusted to 15 Pa, and an LSMO film with a thickness of about 80 nm was grown;

[0054] (3) Use laser to clean NiO target for 1000 pulses, then raise the substrate temperature to 780℃, adjust the oxygen pressure to 30Pa, and grow NiO film with a thickness of 10nm

[0055] Example 2 Preparation of LSMO / NiO corner heterostructures stacked at different angles

[0056] (1)-(11) are the same as steps (1)-(11) of Example 1.

[0057] (12) Using a high-precision transfer platform that can be heated to 80-100 degrees for 5-20 minutes, the self-supporting LSMO and self-supporting NiO films are separated from the PDMS. At the same time, the platform can rotate 0-360 degrees in the plane, thereby forming LSMO / NiO corner heterojunctions with different stacking angles on the flexible target substrate. The sample stacking angle is 10 degrees, which means that the

[100] of LSMO and the

[100] of NiO form an angle of 10 degrees, and the

[010] of LSMO and the

[010] of NiO form an angle of 10 degrees. The sample stacking angle is 20 degrees, which means that the

[100] of LSMO and the

[100] of NiO form an angle of 20 degrees, and the

[010] of LSMO and the

[010] of NiO form an angle of 20 degrees. Similarly, corner magnetic heterojunctions with different stacking angles are prepared. In order to obtain a strong exchange bias effect, the antiferromagnetic layer of all corner heterojunctions completely covers the LSMO layer.

[0058] Example 3 Preparation of a heterostructure with stacked LSMO / NiO and added capping layer

[0059] (1)-(11) as in Example 1, steps (1)-(11).

[0060] (12) The entire heterojunction is placed back into the LMBE cavity. The LaAlO is cleaned with a laser. 3 1000 pulses of target material, oxygen pressure adjusted to 30Pa, LaAlO grown at room temperature 3 Covering film.

[0061] Prepared materials and characterization

[0062] Figure 1 The La prepared above with a stacking angle of 0 degrees 0.67 Sr 0.33 MnO 3 Schematic diagram of the / NiO corner heterostructure. Figure 2 is La with a stacking angle of 0 degrees on a Si substrate 0.67 Sr 0.33 MnO 3 The X-ray diffraction pattern of the / NiO corner heterostructure shows an epitaxial (001) curve. Figure 3 is the in-plane hysteresis loop of the sample. The test parameters are 4000Oe field cooling to 5K, and at 5K, the magnetic moment size under different external magnetic fields is tested at positive and negative 20000Oe. From the figure, it can be seen that the in-plane hysteresis loop is asymmetric and shifts to the left as a whole, proving that the corner heterojunction has strong interface magnetic coupling and the exchange bias is 120Oe. The comparative example is the non-stacked LSMO / NiO heterojunction, whose exchange bias is only 100Oe (such as Fig. 9 That is, the exchange bias of the corner stacked heterojunction is increased by 20% compared with the non-stacked rigid heterojunction.

[0063] Example 2 is a LSMO / NiO corner heterostructure with different angles. Figure 4 It is a schematic diagram of the method of selecting different angles when stacking flexible mica substrates; through different methods, any angle can be conveniently selected for stacking. Figure 5 (a) and (b) are the morphology images under optical microscope of 10-degree stacking and 30-degree stacking respectively; the exchange bias can reach a maximum of 160Oe. Figure 6 It is the hysteresis loop when stacked at 20 degrees.

[0064] Example 3 is a heterostructure in which LSMO / NiO is stacked and a capping layer is added. The growth diagram of the capping layer is shown in FIG. Figure 7 As shown, the hysteresis loop is Figure 8 As shown, the exchange bias can reach 180Oe, which is 1.8 times higher than that of the rigid heterojunction.

Claims

1. An oxide corner heterojunction with a strong magnetic exchange bias effect, characterized in that: The oxide heterojunction with magnetic exchange bias is formed by stacking different oxide single crystal films connected by van der Waals force; a covering film can be deposited on top to change the interlayer spacing; the exchange bias strength of the heterojunction can be regulated by different thicknesses and angles of different magnetic oxide films when stacking, or by changing the thickness of the covering layer.

2. A method for preparing and controlling the performance of a corner oxide heterojunction with a strong magnetic exchange bias effect as claimed in claim 1, characterized in that: The following steps are involved: (1) Using pulsed laser molecular beam epitaxy (LMBE) technology, a water-soluble or acid-soluble sacrificial layer is first deposited on a single crystal substrate, and then a ferromagnetic or antiferromagnetic oxide film is deposited to obtain a single crystal substrate / sacrificial layer / single crystal oxide film structure; (2) placing the single crystal substrate / sacrificial layer / single crystal oxide film structure into an etching solution, and after the sacrificial layer is dissolved, the single crystal oxide film can be separated from the substrate; (3) After the film is completely separated from the substrate, the self-supporting single crystal oxide film is transferred to any target substrate and stacked at a certain angle and number of layers to form a multi-layer stacked oxide heterojunction with exchange bias. (4) Place the heterostructure into the LMBE deposited cover layer.

3. The preparation method according to claim 2, characterized in that The substrate described in step (1) is SrTiO3 (STO), the sacrificial layer is Sr3Al2O6, and the ferromagnetic oxide is La0.67Sr0.33MnO3 (LSMO) or La1-xCaxMnO3 (LCMO) or the like.

4. The preparation method according to claim 2, characterized in that The covering layer described in step (4) is LaAlO3 or BaTiO3.

5. The preparation method according to claim 2, characterized in that During the epitaxial growth of the sacrificial layer in step (1), the laser energy density is 1-3J / cm2, and the Sr3Al2O6 layer is deposited with a thickness of 1-80nm under the conditions of an oxygen pressure of 5-30Pa and a substrate temperature of 600-800°C; the ferromagnetic and antiferromagnetic single crystal oxide thin films are deposited under a vacuum of 15Pa-30Pa, a temperature of 300-800°C, and a thickness of 5-200nm.

6. The preparation method according to claim 2, characterized in that The deposition of the covering layer in step (4) is carried out under an oxygen pressure of 103 Pa and room temperature.

Citation Information

Cited By

  • Self-supporting thin film high-voltage electricity transport measuring device and preparation method and application of self-supporting thin film high-voltage electricity transport measuring device

    CN120044287A