Glass block, method for producing same, and plasma-resistant member

By controlling the oxide composition and manufacturing process of the glass block, the problem of wear of the components of the semiconductor manufacturing device in the plasma environment is solved, and the plasma resistance and mechanical strength are improved, reducing the frequency and cost of component replacement.

CN118973973AInactive Publication Date: 2024-11-15AGC INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380031505.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-31
Filing Date
2023-03-17
Publication Date
2024-11-15
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The components of semiconductor manufacturing devices wear rapidly in plasma environments, resulting in frequent replacement, affecting production efficiency, and existing materials such as sapphire are costly and difficult to process.

Method used

A glass block containing silicon, magnesium and calcium was developed to improve its plasma resistance and mechanical strength by controlling the composition of the reference mole percentage of oxides, and adopting a melting process below 1650°C and slowly cooling to form.

Benefits of technology

It has achieved significant improvements in plasma resistance and mechanical strength, reducing component replacement frequency, improving production efficiency, and reducing costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005064726540000191
    Figure BDA0005064726540000191
  • Figure BDA0005064726540000201
    Figure BDA0005064726540000201
  • Figure BDA0005064726540000211
    Figure BDA0005064726540000211
Patent Text Reader

Abstract

The present invention pertains to a glass block for a plasma-resistant member, the glass block containing silicon and at least one of magnesium and calcium, the total content of MgO and CaO being 3.0 mol% or more and less than 29.0 mol% in terms of oxide-based molar percentage, where R1 is an alkali metal element and R2 is an alkaline earth metal element, and the glass block containing silicon and at least one of magnesium and calcium, the glass block being characterized in that: the total content of MgO and CaO is not less than 3.0 mol% and less than 29.0 mol% in terms of oxide-based molar percentage; the content of R2O is 3.0 mol% or more but less than 35.0 mol%, and the content of R12O is 8.0 mol% or less.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a glass block, a method for producing the same, and a plasma-resistant component. Background Art

[0002] Components used in semiconductor manufacturing equipment are often exposed to plasma during operation of the semiconductor manufacturing equipment and gradually wear out. The worn components are replaced with new ones.

[0003] In recent years, as products manufactured by semiconductor manufacturing equipment have become taller and more complex, the plasma environment to which components are exposed has become increasingly severe, and in this case, components need to be frequently replaced.

[0004] However, the semiconductor manufacturing apparatus cannot be operated during the replacement of the parts. Therefore, if the replacement frequency of the parts increases, the production efficiency of the product will decrease.

[0005] Therefore, components used in semiconductor manufacturing equipment are required to have a further longer life, that is, to have good plasma resistance.

[0006] As a semiconductor manufacturing apparatus, a plasma etching apparatus is mentioned, for example.

[0007] The plasma etching device is equipped with components such as a top plate (inductive type), a microwave introduction tube, lift pins, various nozzles, an edge ring, an electrostatic chuck, a shower plate, and a protective cover for the sensor in the chamber.

[0008] Conventionally, materials such as cordierite sintered bodies have been used as these components (Patent Document 1).

[0009] Prior art literature

[0010] Patent Literature

[0011] Patent Document 1: Japanese Patent Application Laid-Open No. 9-295863 Summary of the invention

[0012] Materials used for plasma-resistant parts such as window materials for semiconductor manufacturing equipment (parts used to observe the inside of the device from the outside) are required to have excellent mechanical strength in addition to excellent plasma resistance.

[0013] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a material having excellent plasma resistance and mechanical strength.

[0014] The present inventors have conducted intensive studies and have found that the above-mentioned object can be achieved by adopting the following configuration, thereby completing the present invention.

[0015] That is, the inventors have found that the above-mentioned problems can be solved by the following configuration.

[0016] [1] A glass block for a plasma-resistant component, comprising silicon and at least one of magnesium and calcium, wherein the alkali metal element is R 1 , alkaline earth metal elements are set as R 2 When the total content of MgO and CaO is expressed as a molar percentage based on oxides, it is 3.0 mol% or more and less than 29.0 mol%, R 2 The content of O is 3.0 mol% or more and less than 35.0 mol%, and R 1 The content of 2O is 8.0 mol% or less.

[0017] [2] The glass block according to [1] above, wherein the content of SiO2 is 40.0 mol% or more and less than 90.0 mol%, and the content of B2O3 is less than 30.0 mol%.

[0018] [3] The glass block according to [1] above, wherein the ratio of the content of SrO to the total content of MgO and CaO is less than 0.50, and the content of SrO is less than 15.0 mol %.

[0019] [4] The glass block according to [1] above, wherein the ratio of the total content of BaO and SrO to the total content of MgO and CaO is less than 0.45.

[0020] [5] The glass block according to [1] above, wherein the ratio of the content of BaO to the total content of MgO and CaO is less than 0.35.

[0021] [6] The glass block according to [1] above, wherein the average thermal expansion coefficient at 50 to 350° C. is 5.0 ppm / ° C. or less.

[0022] [7] The glass block according to [1] above, wherein the content of Al2O3 is equal to R 2 The content ratio of O is less than 0.6, and the content of Al2O3 is less than 20.0 mol%.

[0023] [8] The glass block according to [1] above, wherein a fluorine content is 5.0% by mass or less relative to the total mass of the glass block.

[0024] [9] The glass block according to [1] above, wherein the visible light transmittance is 60% or more.

[0025]

[10] The glass block according to [1] above, wherein the ratio of the content of MgO to the total content of MgO and CaO is 0.1 to 0.9.

[0026]

[11] The glass block according to [1] above, wherein the content of P2O5 is 0.1 mol% or more and less than 5.5 mol%.

[0027]

[12] The glass block according to [1] above, wherein R 2 The content of O is 3.0 mol% or more and less than 20.0 mol%.

[0028]

[13] A method for producing a glass block, which is a method for producing the glass block according to any one of [1] to

[12] , comprising heating a glass raw material at 1650° C. or less to melt it, shaping the obtained molten glass, and slowly cooling it.

[0029]

[14] A plasma-resistant component, comprising the glass block according to any one of [1] to

[12] above.

[0030]

[15] The plasma-resistant component according to

[14] above is mounted on a plasma etching device and serves as a window material, a top plate, a microwave introduction tube, a lifting pin, a nozzle, an edge ring, an electrostatic chuck, a shower plate or a protective cover for a sensor in a chamber.

[0031] According to the present invention, a raw material having excellent plasma resistance and mechanical strength can be provided. DETAILED DESCRIPTION

[0032] The meanings of the terms in the present invention are as follows.

[0033] The numerical range expressed using “to” means a range including the numerical values ​​described before and after “to” as the lower limit and the upper limit.

[0034] [Glass Block]

[0035] The glass block of the present invention is a glass block for a plasma-resistant member, comprising silicon and at least one of magnesium and calcium, and wherein the alkali metal element is R 1 , alkaline earth metal elements are set as R 2 When the total content of MgO and CaO is expressed as a molar percentage based on oxides, it is 3.0 mol% or more and less than 29.0 mol%, R 2 The content of O is 3.0 mol% or more and less than 35.0 mol%, and R 1 The content of 2O is 8.0 mol% or less.

[0036] Hereinafter, the glass block is simply referred to as "glass", and the glass block of the present invention is also referred to as "the present glass block" or "the present glass".

[0037] The glass block has excellent plasma resistance. This is presumably because the above-mentioned configuration can reduce the rate of deterioration due to plasma irradiation.

[0038] Furthermore, the glass block has excellent mechanical strength. This is presumably because the above-mentioned structure does not contain too much alkaline earth metal components that make the bonding state of the glass unstable, and can contain enough network-forming components such as SiO2 and Al2O3 that stabilize the bonding state of the glass.

[0039] In addition, in semiconductor manufacturing equipment, as a conventional component used in an environment exposed to plasma, a component made of sapphire can also be cited.

[0040] However, sapphire has poor mechanical strength and is difficult to process, so its cost is very high. In addition, since sapphire is produced by a single crystal growth method, its production characteristics are poor and the size that can be produced is limited.

[0041] In contrast, this glass block is excellent in mechanical strength and easy to process compared with sapphire, so cost is low. In addition, this glass block can be easily manufactured by the manufacturing method described later, so manufacturing characteristics are good, and size also can be appropriately changed.

[0042] Hereinafter, the present glass block will be described in detail.

[0043] Hereinafter, the composition (glass composition) of the present glass lump will be described first. That is, the content (expressed as molar percentage based on oxides) of elements that may be contained in the present glass lump will be described.

[0044] 〈Si, B and P〉

[0045] The glass block contains silicon (Si).

[0046] The present glass block may further contain boron (B) and phosphorus (P).

[0047] SiO2

[0048] From the reason that the transparency of the present glass block is more excellent, the content of SiO2 is preferably 40.0 mol% or more, more preferably 50.0 mol% or more, further preferably 55.0 mol% or more, further preferably 60.0 mol% or more, particularly preferably 62.0 mol% or more, and most preferably 64.0 mol% or more.

[0049] From the reason that the plasma resistance and transparency of the present glass block are more excellent, the content of SiO2 is preferably less than 90.0 mol%, more preferably less than 80.0 mol%, further preferably less than 75.0 mol%, and particularly preferably less than 70.0 mol%. That is, the content of SiO2 is preferably 40.0 mol% or more and less than 90.0 mol%.

[0050] B2O3

[0051] From the reason that the present glass block has excellent plasma resistance, the content of B2O3 is preferably less than 40.0 mol%, more preferably less than 30.0 mol%, further preferably less than 15.0 mol%, further preferably less than 12.0 mol%, particularly preferably less than 9.0 mol%, more particularly preferably less than 7.0 mol%, very preferably less than 5.0 mol%, and most preferably less than 3.0 mol%.

[0052] The lower limit of the content of B2O3 may be zero. For the reason that the manufacturing characteristics of the glass block are excellent, the content of B2O3 is preferably 0.5 mol% or more, more preferably 1.0 mol% or more, further preferably 1.5 mol% or more, particularly preferably 2.0 mol% or more, and most preferably 2.5 mol% or more. That is, the content of B2O3 may be 0 mol% or more and less than 40.0 mol%.

[0053] P2O5

[0054] From the reason that the present glass block has excellent plasma resistance, the content of P2O5 is preferably less than 5.5 mol%, more preferably 4.0 mol% or less, further preferably 2.0 mol% or less, and particularly preferably 1.0 mol% or less.

[0055] The lower limit of the content of P2O5 may be zero. From the reason that the devitrification temperature of the glass block is lowered, the content of P2O5 is preferably 0.1 mol% or more, more preferably 0.3 mol% or more, and further preferably 0.6 mol% or more. That is, the content of P2O5 may be 0 mol% or more and less than 5.5 mol%.

[0056] 《a: Total content of SiO2, B2O3 and P2O5》

[0057] In view of the excellent mechanical strength and transparency of the glass block, the total content (a) of SiO2, B2O3 and P2O5 is preferably 40.0 mol% or more, more preferably 50.0 mol% or more, further preferably 60.0 mol% or more, particularly preferably 65.0 mol% or more, and most preferably 70.0 mol% or more.

[0058] From the reason that the present glass block has excellent plasma resistance, the total content (a) of SiO2, B2O3 and P2O5 is preferably less than 95.0 mol%, more preferably less than 90.0 mol%, further preferably less than 85.0 mol%, particularly preferably less than 80.0 mol%, and most preferably less than 75.0 mol%. That is, the total content (a) of SiO2, B2O3 and P2O5 is preferably 40.0 mol% or more and less than 95.0 mol%.

[0059] 〈Al, Ga and In〉

[0060] The glass block may also contain aluminum (Al), gallium (Ga) and In (indium).

[0061] 《Al2O3》

[0062] From the reason that the present glass block has excellent plasma resistance, the Al2O3 content is preferably less than 20.0 mol%, more preferably less than 18.0 mol%, further preferably less than 16.0 mol%, further preferably less than 14.0 mol%, particularly preferably less than 12.0 mol%, very preferably less than 10.0 mol%, and most preferably less than 8.0 mol%.

[0063] The lower limit of the content of Al2O3 may be 0. From the perspective of excellent manufacturing characteristics of the glass block, the content of Al2O3 is preferably greater than 3.0 mol%, more preferably greater than 5.0 mol%, and further preferably greater than 7.0 mol%. That is, the content of Al2O3 may be greater than 0 mol% and less than 20.0 mol%.

[0064] Ga2O3

[0065] From the reason that the present glass block has excellent plasma resistance and transparency, the Ga2O3 content is preferably 3.0 mol% or less, more preferably 1.0 mol% or less, and further preferably 0.5 mol% or less.

[0066] The lower limit of the Ga2O3 content is preferably zero. That is, the Ga2O3 content is preferably 0 mol% to 3.0 mol%.

[0067] In2O3

[0068] From the reason that the plasma resistance and transparency of the present glass block are more excellent, the content of In2O3 is preferably 5.0 mol% or less, more preferably 3.0 mol% or less, and further preferably 1.0 mol% or less.

[0069] The lower limit of the content of In2O3 is preferably zero. That is, the content of In2O3 is preferably 0 mol% to 5.0 mol%.

[0070] 〈R 2 〉

[0071] The glass block may also contain alkaline earth metal elements (R 2 ).

[0072] As alkaline earth metal elements (R 2 ) include beryllium (Be), magnesium (Mg), calcium (Ca), strontium (Sr), barium (Ba) and radium (Ra).

[0073] Among them, the present glass block contains at least one of Mg and Ca as an essential element.

[0074] 《R 2 O》

[0075] Since the present glass block has excellent plasma resistance, R 2 The content of O is 3.0 mol % or more, preferably 5.0 mol % or more, more preferably 10.0 mol % or more, and further preferably 15.0 mol % or more.

[0076] On the other hand, since the mechanical strength and transparency of the glass block are more excellent, R 2 The content of O is less than 35.0 mol%, preferably less than 33.0 mol%, more preferably less than 31.0 mol%, further preferably less than 29.0 mol%, particularly preferably less than 27.0 mol%, and most preferably less than 20.0 mol%. 2 The content of O is 3.0 mol% or more and less than 35.0 mol%.

[0077] MgO

[0078] Because the present glass block has excellent mechanical strength and transparency, the MgO content is preferably less than 20.0 mol %, more preferably less than 15.0 mol %, further preferably less than 13.0 mol %, particularly preferably less than 11.0 mol %.

[0079] On the other hand, because the present glass block has excellent plasma resistance, the MgO content is preferably 2.0 mol% or more, more preferably 4.0 mol% or more, further preferably 6.0 mol% or more, and particularly preferably 8.0 mol% or more. That is, the MgO content is preferably 2.0 mol% or more and less than 20.0 mol%.

[0080] 《CaO》

[0081] From the reason that the present glass lump has more excellent plasma resistance, the CaO content is preferably 5.0 mol % or more, more preferably 10.0 mol % or more, further preferably 15.0 mol % or more, particularly preferably 18.0 mol % or more.

[0082] On the other hand, because the plasma resistance, mechanical strength and transparency of the present glass block are more excellent, the CaO content is preferably less than 25.0 mol%, more preferably less than 23.0 mol%, further preferably less than 21.0 mol%, and particularly preferably less than 19.0 mol%. That is, the CaO content is preferably 5.0 mol% or more and less than 25.0 mol%.

[0083] 《Total content of MgO and CaO》

[0084] From the reason that the present glass block has better plasma resistance, the total content of MgO and CaO is preferably 3.0 mol% or more, preferably 9.0 mol% or more, more preferably 13.0 mol% or more, further preferably 17.0 mol% or more, and particularly preferably 20.0 mol% or more.

[0085] On the other hand, because the mechanical strength and transparency of the present glass block are more excellent, the total content of MgO and CaO is less than 29.0 mol%, preferably less than 27.0 mol%, more preferably less than 25.0 mol%, further preferably less than 23.0 mol%, and particularly preferably less than 21.0 mol%. That is, the total content of MgO and CaO is 3.0 mol% or more and less than 29.0 mol%.

[0086] 《Ratio (MgO / (MgO+CaO))》

[0087] From the reason that the present glass block has excellent plasma resistance, the ratio of the MgO content (unit: mol %) to the total content of MgO and CaO (unit: mol %) (MgO / (MgO+CaO)) is preferably 0.1 to 0.9, more preferably 0.14 to 0.5, further preferably 0.17 to 0.4, particularly preferably 0.2 to 0.35, and most preferably 0.23 to 0.30.

[0088] Among them, MgO / (MgO+CaO) is preferably 0.1 or more, more preferably 0.14 or more, further preferably 0.17 or more, further preferably 0.2 or more, and particularly preferably 0.23 or more. In addition, MgO / (MgO+CaO) is preferably 0.9 or less, more preferably 0.5 or less, further preferably 0.4 or less, further preferably 0.35 or less, and particularly preferably 0.30 or less.

[0089] 《Ratio (CaO / SiO2)》

[0090] Based on the reason that the glass block has excellent plasma resistance, the total ratio of the CaO content (unit: mol %) to the SiO2 content (unit: mol %) (CaO / SiO2) is preferably 0.1 to 0.9, more preferably 0.14 to 0.5, further preferably 0.17 to 0.4, particularly preferably 0.2 to 0.35, and most preferably 0.23 to 0.30.

[0091] Here, CaO / SiO2 is preferably 0.1 or more, more preferably 0.14 or more, further preferably 0.17 or more, further preferably 0.2 or more, and particularly preferably 0.23 or more. In addition, CaO / SiO2 is preferably 0.9 or less, more preferably 0.5 or less, further preferably 0.4 or less, further preferably 0.35 or less, and particularly preferably 0.30 or less.

[0092] SrO

[0093] From the reason that the present glass block has excellent plasma resistance, the SrO content is preferably less than 15.0 mol %, more preferably less than 10.0 mol %, further preferably less than 5.0 mol %, further preferably less than 4.0 mol %, particularly preferably less than 3.0 mol %, very preferably less than 2.0 mol %, and most preferably less than 1.0 mol %.

[0094] The lower limit of the SrO content is preferably 0. That is, the total SrO content is preferably 0 mol% or more and less than 15.0 mol%.

[0095] 《Ratio (SrO / (MgO+CaO))》

[0096] From the reason that the present glass block has excellent plasma resistance, the ratio of the SrO content (unit: mol %) to the total content of MgO and CaO (unit: mol %) (SrO / (MgO+CaO)) is preferably less than 0.50, more preferably less than 0.30, further preferably less than 0.20, and particularly preferably less than 0.10.

[0097] The lower limit of the ratio (SrO / (MgO+CaO)) is preferably zero. That is, the ratio (SrO / (MgO+CaO)) is preferably 0 or more and less than 0.50.

[0098] BaO

[0099] From the reason that the plasma resistance of the present glass block is more excellent, the BaO content is preferably less than 15.0 mol%, more preferably less than 10.0 mol%, further preferably less than 5.0 mol%, further preferably less than 4.0 mol%, particularly preferably less than 3.0 mol%, very preferably less than 2.0 mol%, and most preferably less than 1.0 mol%.

[0100] The lower limit of the BaO content is preferably 0. The BaO content is preferably 0 mol% or more and less than 15.0 mol%.

[0101] 《Ratio (BaO / (MgO+CaO))》

[0102] From the reason that the present glass block has excellent plasma resistance, the ratio of the BaO content (unit: mol %) to the total content of MgO and CaO (unit: mol %) (BaO / (MgO+CaO)) is preferably less than 0.35, more preferably less than 0.25, further preferably less than 0.15, and particularly preferably less than 0.05.

[0103] The lower limit of the ratio (BaO / (MgO+CaO)) is preferably 0. That is, the ratio (BaO / (MgO+CaO)) is preferably 0 or more and less than 0.35.

[0104] "Ratio ((BaO+SrO) / (MgO+CaO))"

[0105] From the reason that the present glass block has excellent plasma resistance, the ratio of the total content of BaO and SrO (unit: mol %) to the total content of MgO and CaO (unit: mol %) ((BaO+SrO) / (MgO+CaO)) is preferably less than 0.75, more preferably less than 0.45, further preferably less than 0.30, particularly preferably less than 0.15, and most preferably less than 0.10.

[0106] The lower limit of the ratio ((BaO+SrO) / (MgO+CaO)) is preferably 0. That is, the ratio ((BaO+SrO) / (MgO+CaO)) is preferably 0 or more and less than 0.75.

[0107] Ratio (Al2O3 / R 2 O)》

[0108] Based on the reason that the present glass block has excellent plasma resistance, the content of Al2O3 (unit: mol%) and R 2 O content (unit: mol%) ratio (Al2O3 / R 2 O) is preferably less than 1.8, more preferably less than 1.0, further preferably less than 0.6, further preferably less than 0.5, particularly preferably less than 0.4, and most preferably less than 0.3.

[0109] Ratio (Al2O3 / R 2 The lower limit of (Al2O3 / R2O3) may be zero. 2 O) is preferably greater than 0.1, more preferably greater than 0.2, and further preferably greater than 0.25. 2 O) is preferably greater than or equal to 0 and less than 1.8.

[0110] 〈Y〉

[0111] The present glass block may further contain yttrium (Y).

[0112] The Y2O3 content of the present glass block is preferably 5.0 mol% or less, more preferably 3.0 mol% or less, and further preferably 1.0 mol% or less.

[0113] The lower limit of the total content of Y2O3 may be 0. From the perspective of the excellent plasma resistance of the glass block, it is preferably 0.4 mol% or more, and more preferably 0.8 mol% or more. That is, the content of Y2O3 may be 0 mol% to 5.0 mol%.

[0114] 〈R 1 〉

[0115] The glass block may also contain alkali metal elements (R 1 ).

[0116] As alkali metal elements (R 1 ), lithium (Li), sodium (Na), potassium (K), rubidium (Rb), cesium (Cs) and francium (Fr). Among these, lithium (Li), sodium (Na) and potassium (K) are substantially preferred.

[0117] 《R 1 2O》

[0118] Since the present glass block has excellent plasma resistance, R 1 The 2O content is 8.0 mol% or less, preferably 4.0 mol% or less, more preferably 1.2 mol% or less, further preferably 0.8 mol% or less, further preferably 0.4 mol% or less, particularly preferably 0.1 mol% or less, and most preferably 0.01 mol% or less.

[0119] R 1 The lower limit of the content of 2O is preferably zero. 1 The content of 2O is, for example, 0 mol % to 8.0 mol %.

[0120] 〈Zn and Zr〉

[0121] The glass block may further contain zinc (Zn) and zirconium (Zr).

[0122] ZnO

[0123] Because the present glass block has excellent plasma resistance and mechanical strength, the ZnO content is preferably 7.0 mol % or less, more preferably 4.0 mol % or less, further preferably 1.0 mol % or less, particularly preferably 0.5 mol % or less.

[0124] The lower limit of the ZnO content is preferably 0. That is, the ZnO content is preferably 0 mol% to 7.0 mol%.

[0125] ZrO2

[0126] Because the present glass block has excellent plasma resistance, the ZrO 2 content is preferably 6.0 mol % or less, more preferably 2.5 mol % or less, further preferably 1.0 mol % or less, and particularly preferably 0.5 mol % or less.

[0127] The lower limit of the ZrO2 content is preferably zero. That is, the ZrO2 content is preferably 0 mol% to 6.0 mol%.

[0128] 〈Impurity Elements〉

[0129] From the reason that the present glass block has excellent plasma resistance, the content of the impurity element in terms of oxide is preferably 15.0 mol % or less, more preferably 10.0 mol % or less, further preferably 7.5 mol % or less, further preferably 5.0 mol % or less, particularly preferably 1.0 mol % or less, very preferably 0.5 mol % or less, and most preferably 0.05 mol % or less.

[0130] The lower limit of the content of the impurity element in terms of oxide is preferably zero.

[0131] Impurity elements are silicon (Si), boron (B), phosphorus (P), aluminum (Al), gallium (Ga), indium (In), alkaline earth metal elements (R 2 ), yttrium (Y), alkali metal elements (R 1 ), zirconium (Zr) and zinc (Zn) other metal elements.

[0132] Examples of impurity elements include Cu, Fe, Ni, Cr, Sn, Co, V, Bi, Se, Ce, Er, Nd, Ge, Ti, Mn, and Ta.

[0133] Specifically, the content of Cu calculated as oxide refers to the content of CuO.

[0134] Specifically, the Fe content calculated as oxide refers to the Fe2O3 content.

[0135] Specifically, the Ni content calculated as oxide refers to the NiO content.

[0136] Specifically, the Cr content calculated as oxide refers to the Cr2O3 content.

[0137] Specifically, the content of Sn calculated as oxide refers to the content of SnO2.

[0138] Specifically, the content of Co calculated as oxide refers to the content of Co 3 O 4 .

[0139] Specifically, the V content calculated as oxide refers to the V2O5 content.

[0140] Specifically, the Bi content calculated as oxide refers to the Bi2O3 content.

[0141] Specifically, the Se content calculated as an oxide refers to the SeO 2 content.

[0142] Specifically, the Ce content calculated as oxide refers to the CeO 2 content.

[0143] Specifically, the Er content converted into oxide refers to the Er2O3 content.

[0144] Specifically, the Nd content calculated as oxide refers to the Nd2O3 content.

[0145] Specifically, the content of Ge calculated as oxide refers to the content of GeO2.

[0146] Specifically, the Ti content calculated as oxide refers to the TiO2 content.

[0147] Specifically, the content of Mn calculated as oxide refers to the content of MnO2.

[0148] Specifically, the Ta content calculated as oxide refers to the Ta2O5 content.

[0149] 〈F〉

[0150] The present glass block may further contain fluorine (F).

[0151] From the reason that the manufacturing characteristics of the present glass block are excellent, the content of F is preferably 5.0 mass % or less, more preferably 4.0 mass % or less, further preferably 3.0 mass % or less, particularly preferably 2.0 mass % or less, and most preferably 1.0 mass % or less, relative to the total mass of the glass block.

[0152] The lower limit of the F content may be 0. That is, the F content may be 0% by mass to 5.0% by mass.

[0153] The content (expressed as a molar percentage based on an oxide) of each of the above elements (except Si) in the glass block was measured using a fluorescent X-ray device (XRF) (Rigaku Corporation, ZSX100e). That is, the X-ray intensity of each element on the surface of the glass block was measured and quantitatively analyzed to determine the content of each element.

[0154] The content of SiO2 in the glass block was determined as follows.

[0155] First, a powder sample was collected from the center of a glass block by grinding, and the total oxygen content Z1 in the glass block was determined by an infrared absorption method using an oxygen / hydrogen analyzer (ROH-600 manufactured by LECO Corporation).

[0156] The oxygen amount Z3 is calculated by subtracting the oxygen amount Z2 of the elements (excluding Si) contained in the glass block and combined in a stoichiometric composition from the total oxygen amount Z1 in the glass block (oxygen amount Z3 = total oxygen amount Z1 - oxygen amount Z2).

[0157] Assuming that the total amount of oxygen Z3 is used for bonding with silicon atoms, the oxygen Z3 is converted into the amount of SiO2. The amount of SiO2 obtained in this way is regarded as the content of SiO2 in the glass block.

[0158] 〈Expansion coefficient〉

[0159] From the viewpoint of suppressing cracks during the production of the present glass block, the average thermal expansion coefficient of the present glass block at 50 to 350°C (hereinafter referred to as "expansion coefficient") is preferably 5.0 ppm / °C or less, more preferably 4.5 ppm / °C or less, further preferably 4.0 ppm / °C or less, further preferably 3.5 ppm / °C or less, particularly preferably 3.0 ppm / °C or less, very preferably 2.5 ppm / °C or less, and most preferably 2.0 ppm / °C or less.

[0160] The expansion coefficient is measured using a differential thermal dilatometer according to the method described in JIS R 3102-1995.

[0161] 〈Visible light transmittance〉

[0162] The visible light transmittance of the glass block is preferably 60% or more, more preferably 70% or more, further preferably 80% or more, further preferably 85% or more, more particularly preferably 90% or more, very preferably 93% or more, and most preferably 95% or more. The upper limit is preferably 100%.

[0163] The visible light transmittance is measured by a method in accordance with JIS R3106 (1998).

[0164] In order to make the visible light transmittance within the above range, it is preferred that each component be contained in the above content and a glass block be produced by the method described later (this production method).

[0165] <shape>

[0166] Examples of the shape of the glass block include a plate shape (for example, a disk shape, a flat plate shape), a spherical shape, an ellipsoidal shape, and the shape can be appropriately selected depending on the intended use.

[0167] It should be noted that the term “glass block” refers to a concept that does not include glass frit, glass powder, and glass fiber, regardless of the shape.

[0168] When the glass block is in the form of a plate, the area of ​​at least one surface (for example, the main surface) of the glass block is preferably 25 mm 2 More than 100 mm is more preferred 2 More than, more preferably 500mm 2 More than 1000 mm is more preferred 2 Above, particularly preferably 5000mm 2 More preferably, 10000 mm 2 Above, 40000mm is very preferred 2 Above, most preferably 90000mm 2 above.

[0169] When the glass block is in the form of a plate, the thickness (thickness of the thinnest part) of the glass block is preferably 0.3 mm or more, more preferably 0.5 mm or more, further preferably 1 mm or more, further preferably 3 mm or more, particularly preferably 6 mm or more, more particularly preferably 10 mm or more, very preferably 15 mm or more, and most preferably 20 mm or more.

[0170] On the other hand, because the crystallization of the glass block is suppressed and the transparency is more excellent, the thickness of the glass block is preferably 500 mm or less, more preferably 100 mm or less, further preferably 80 mm or less, further preferably 60 mm or less, very preferably 50 mm or less, particularly preferably 40 mm or less, and most preferably 30 mm or less. That is, the thickness of the glass block is preferably 0.3 mm to 500 mm.

[0171] From the reason that the present glass block has excellent transparency, it is preferred to suppress the generation of a different phase (crystal phase, colloidal metal, ceramic particles, etc.).

[0172] In addition, as a conventional transparent member used in an environment exposed to plasma in a semiconductor manufacturing apparatus, for example, a member made of quartz can be cited.

[0173] However, quartz has insufficient plasma resistance.

[0174] On the other hand, the present glass lump is excellent in both plasma resistance and mechanical strength.

[0175] <use>

[0176] The present glass block can be suitably used as a plasma-resistant member. However, the use of the present glass block is not limited thereto.

[0177] Examples of plasma-resistant components include components mounted on a plasma etching device, such as window materials, top plates, microwave introduction tubes, lift pins, nozzles, edge rings, electrostatic chucks, shower plates, and protective covers for sensors in chambers.

[0178] [Method for producing glass block]

[0179] Next, a method for producing the present glass block (hereinafter also referred to as "the present production method") is described. In the present production method, in brief, glass raw materials are heated to be melted, the obtained molten glass is molded, and then slowly cooled.

[0180] More specifically, first, various glass raw materials are weighed and mixed so that the composition of the obtained glass block becomes the above-mentioned glass composition.

[0181] Next, the mixed glass raw materials are heated and melted using a glass melting furnace or the like. At this time, the melt is appropriately subjected to degassing, homogenization, etc. according to a known method, thereby obtaining molten glass.

[0182] Then, the obtained molten glass is formed into a desired shape and slowly cooled. The forming method is not particularly limited, and for example, a float process, a pressurization process, a melting process, and a down-draw process can be cited. It should be noted that the obtained molten glass is formed into a temporary shape and slowly cooled, and the obtained temporary shape body can be processed by cutting and the like. Thus, a glass block of a desired shape is obtained.

[0183] The obtained glass block may be subjected to treatments such as grinding and polishing as required.

[0184] The temperature when the glass raw material is heated to melt (hereinafter also referred to as "melting temperature") is preferably 1650°C or lower, more preferably 1600°C or lower, and further preferably 1550°C or lower because of excellent production characteristics.

[0185] 〈Temperature T2〉

[0186] It should be noted that, because the manufacturing characteristics of the present glass block are more excellent, the temperature T2 (unit: ° C.) at which the viscosity of the present glass block reaches logη=2 is preferably 1735° C. or less, more preferably 1690° C. or less, further preferably 1650° C. or less, particularly preferably 1610° C. or less, and most preferably 1570° C. or less. The lower limit is preferably 1100° C.

[0187] The temperature T2 at which the viscosity of the glass block reaches logη=2 can be measured by the following method. The slow cooling point of the glass block is measured according to JIS R3103-2, and the softening point is measured according to JIS R3103-1. Next, the temperature at which the viscosity reaches from 100 dPa·s to 10000 dPa·s is measured by a rotational viscometer, and the measured temperature is fitted to the Fulcher equation together with the slow cooling point and the softening point to obtain the temperature (unit: °C) at which the viscosity η (unit: dPa·s) of the glass plate reaches logη=2.

[0188] From the viewpoint of clarity, the time for heating the glass raw material to melt it (hereinafter also referred to as "melting time") is preferably 24 hours or less, more preferably 12 hours or less, further preferably 10 hours or less, further preferably 8 hours or less, particularly preferably 6 hours or less, and most preferably 4 hours or less.

[0189] From the viewpoint of crystallization acceleration, the cooling rate when cooling the molten glass is preferably 0.5°C / min or more, more preferably 1°C / min or more, further preferably 5°C / min or more, particularly preferably 10°C / min or more.

[0190] As described above, the following configurations are disclosed in this specification.

[0191] <1> A glass block for a plasma-resistant member, comprising silicon and at least one of magnesium and calcium,

[0192] And, let the alkali metal element be R 1 , alkaline earth metal elements are set as R 2 When the molar percentage is expressed as oxide,

[0193] The total content of MgO and CaO is 3.0 mol% or more and less than 29.0 mol%,

[0194] R 2 The content of O is 3.0 mol% or more and less than 35.0 mol%,

[0195] R 1 The content of 2O is 8.0 mol% or less.

[0196] <2> The glass block according to <1> above, wherein a content of SiO 2 is 40.0 mol % or more and less than 90.0 mol %, and a content of B 2 O 3 is less than 30.0 mol %.

[0197] <3> The glass lump according to <1> or <2>, wherein the ratio of the content of SrO to the total content of MgO and CaO is less than 0.50, and the content of SrO is less than 15.0 mol %.

[0198] <4> The glass lump according to any one of <1> to <3>, wherein a ratio of a total content of BaO and SrO to a total content of MgO and CaO is less than 0.45.

[0199] <5> The glass lump according to any one of <1> to <4>, wherein a ratio of a content of BaO to a total content of MgO and CaO is less than 0.35.

[0200] <6> The glass lump according to any one of <1> to <5>, wherein an average thermal expansion coefficient at 50 to 350°C is 5.0 ppm / °C or less.

[0201] <7> The glass block according to any one of <1> to <6>, wherein the content of Al2O3 is equal to R 2 The content ratio of O is less than 0.6, and the content of Al2O3 is less than 20.0 mol%.

[0202] <8> The glass lump according to any one of <1> to <7>, wherein a content of fluorine is 5.0% by mass or less based on the total mass of the glass lump.

[0203] <9> The glass block according to any one of <1> to <8>, wherein a visible light transmittance is 60% or more.

[0204] <10> The glass lump according to any one of <1> to <9>, wherein a ratio of a content of MgO to a total content of MgO and CaO is 0.1 to 0.9.

[0205] <11> The glass lump according to any one of <1> to <10>, wherein a content of P2O5 is 0.1 mol% or more and less than 5.5 mol%.

[0206] <12> The glass block according to any one of <1> to <11>, wherein R 2 The content of O is 3.0 mol% or more and less than 20.0 mol%.

[0207] <13> A method for producing a glass block, the method comprising producing the glass block according to any one of <1> to <12>,

[0208] Glass raw materials are heated to 1650° C. or lower to be melted, and the obtained molten glass is formed and slowly cooled.

[0209] <14> A plasma-resistant member comprising the glass block according to any one of <1> to <12>.

[0210] <15> The plasma-resistant component according to <14> is mounted on a plasma etching device,

[0211] As window material, top plate, microwave inlet tube, lift pin, nozzle, edge ring, electrostatic chuck, shower plate or protective cover for chamber sensors.

[0212] Example

[0213] The present invention will be described in detail below with reference to examples, but the present invention is not limited to the examples described below.

[0214] Hereinafter, Examples 1 to 35 are embodiments, and Examples 36 to 41 are comparative examples.

[0215] 〈Example 1~Example 41〉

[0216] The glass blocks of each example were obtained as follows.

[0217] The obtained glass blocks had the compositions shown in Tables 1 to 5 below (expressed in terms of molar percentage based on oxides), and glass raw materials were weighed and mixed so as to give 400 g.

[0218] The mixed glass raw materials are placed in a platinum crucible and introduced into an electric furnace, and heated at a temperature of 1500 to 1700° C. for about 3 hours to be melted, degassed and homogenized to obtain molten glass.

[0219] A portion of the obtained molten glass was poured into a metal mold, kept at a temperature about 50°C higher than the glass transition point for 1 hour, and then cooled to room temperature at a rate of 0.5°C / min to obtain a plate-shaped glass block (main surface area: 10000mm 2 , thickness: 10mm).

[0220] However, in Examples 38 and 41, instead of glass blocks, commercially available quartz and silicon blocks were used, respectively.

[0221] Hereinafter, for convenience, the blocks of Examples 38 and 41 are also referred to as "glass blocks".

[0222] 〈Content of each element〉

[0223] The content of each element (expressed as a molar percentage based on oxide) was determined for the glass block of each example by the above-mentioned method. The results are shown in Tables 1 to 5 below.

[0224] It should be noted that Cu was measured among the impurity elements in Example 34. That is, in Example 34, the numerical value described in the column "Impurity elements (in terms of oxides)" in the table represents the content of CuO.

[0225] Regarding Example 41 (Silicon), for convenience, the Si content is recorded as 100 mol%.

[0226] 〈Expansion coefficient〉

[0227] The expansion coefficient of the glass block of each example was determined by the above method. The results are shown in Tables 1 to 5 below.

[0228] 〈Visible light transmittance〉

[0229] The visible light transmittance of the glass block of each example was determined by the above method. The results are shown in Tables 1 to 5 below.

[0230] In the "visible light transmittance" column of Tables 1 to 5, "90% or more" refers to a visible light transmittance of 90 to 100%, "80% or more" refers to a visible light transmittance of 80% or more and less than 90%, "70% or more" refers to a visible light transmittance of 70% or more and less than 80%, "60% or more" refers to a visible light transmittance of 60% or more and less than 70%, and "less than 60%" refers to a visible light transmittance of 0% or more and less than 60%. In the measurement of visible light transmittance, a test piece of 20 mm × 20 mm × 2 mm size cut out from a glass block was used for measurement. The test piece used was a test piece after mirror finishing of a 20 mm × 20 mm surface.

[0231] 〈Temperature T2〉

[0232] The temperature T2 (unit: °C) at which the viscosity of the glass block of each example reached logη=2 was determined by the above method. The results are shown in Tables 1 to 5 below.

[0233] The lower T2 is, the better the manufacturing characteristics can be evaluated. Specifically, if T2 is 1735°C or less, the manufacturing characteristics are evaluated to be excellent. From the reason of better manufacturing characteristics, T2 is more preferably 1690°C or less, further preferably 1650°C or less, particularly preferably 1610°C or less, and most preferably 1570°C or less.

[0234] 〈Manufacturing Characteristics〉

[0235] The manufacturing characteristics of the glass block of each example were evaluated.

[0236] The evaluation was conducted based on the occurrence of three types of defects (bubbles, cracks, and opaque crystals) in the glass block. 2 There are no more than 3 bubbles above 1.0mm, no more than 1 crack above 0.1mm 2 If the total area ratio of the above crystals is less than 0.1%, it is marked as "○", and if one or more of the three defects are outside these criteria, 0.1 mm 2 There are 4 to 5 bubbles above 1.0mm, 2 to 3 cracks above 0.1mm 2The case where the total area ratio of the crystals is 0.1% or more and less than 0.5% is marked as "△", and the 0.1 mm 2 There are more than 6 bubbles, more than 4 cracks larger than 1.0 mm, and more than 0.1 mm 2 The case where the total area ratio of the above crystals was 0.5% or more was marked as "×".

[0237] If it is "○" or "△", it is evaluated that the manufacturing characteristics are excellent.

[0238] 〈Etching amount〉

[0239] The etching amount of the glass block of each example was determined to evaluate the plasma resistance.

[0240] Specifically, a test piece of 10 mm × 5 mm × 4 mm size was cut out from a glass block, and the surface of 10 mm × 5 mm was mirror-finished. Kapton tape was pasted on a portion of the mirror-finished surface for masking, and etching was performed with plasma gas. Then, a stylus-type surface shape measuring device (manufactured by ULVAC, Dectak150) was used to measure the height difference between the etched portion and the non-etched portion, thereby obtaining the etching amount.

[0241] As a plasma etching apparatus, EXAM (manufactured by Shinko Seiki Co., Ltd., model: POEM) was used. In RIE mode (Reactive Ion Etching model), etching was performed with CF4 gas at a pressure of 10 Pa and an output of 350 W for 195 minutes.

[0242] The smaller the etching amount (unit: nm), the better the plasma resistance can be evaluated.

[0243] Specifically, if the etching amount is 4000 nm or less, the plasma resistance is evaluated to be excellent. For the reason that the plasma resistance is more excellent, the etching amount is preferably 1000 nm or less, preferably 700 nm or less, preferably 500 nm or less, preferably 400 nm or less, and preferably 350 nm or less.

[0244] 〈Whether there is a difference〉

[0245] The glass block of each example was visually observed to confirm the presence or absence of a different phase (crystalline phase, colloidal metal, ceramic particles, etc.).

[0246] In the following Tables 1 to 5, the case where there is no heterogeneous phase is recorded as "○", the case where there is a heterogeneous phase but the total area of ​​the region where the heterogeneous phase exists is less than 10% of the area of ​​the main surface of the glass block is recorded as "△", and the case where there is a heterogeneous phase but the total area of ​​the region where the heterogeneous phase exists is greater than 10% of the area of ​​the main surface of the glass block is recorded as "×".

[0247] If it is "○" or "△", it is evaluated that the transparency is excellent. "○" is preferred because the transparency is more excellent.

[0248] 〈Processability〉

[0249] The workability of the glass block of each example was evaluated.

[0250] Specifically, 10 test pieces of 10 mm×5 mm×4 mm in size were cut out from the glass block, and the prepared test pieces were visually observed to check for damage such as cracks, scratches, and fissures.

[0251] In the following Tables 1 to 5, the case where all 10 test pieces were free of damage was marked as "○", the case where the number of test pieces with damage was 1 was marked as "△", and the case where the number of test pieces with damage was 2 or more was marked as "×".

[0252] If it is "○" or "△", it is evaluated that the mechanical strength is excellent. "○" is preferred because the mechanical strength is better.

[0253] [Table 1]

[0254]

[0255] [Table 2]

[0256]

[0257] [Table 3]

[0258]

[0259] [Table 4]

[0260]

[0261] [Table 5]

[0262]

[0263] 〈Summary of evaluation results〉

[0264] As shown in Tables 1 to 5, the glass blocks of Examples 1 to 35 were excellent in both plasma resistance and mechanical strength.

[0265] On the other hand, the glass blocks of Examples 36 to 41 were insufficient in at least one of plasma resistance and mechanical strength.

[0266] The above describes the embodiments of the present invention, but the embodiments are not limited to the contents of the embodiments. In addition, the above-mentioned constituent elements include elements that can be easily thought of by those skilled in the art, substantially the same elements, and elements of so-called equivalent scopes. Furthermore, the above-mentioned constituent elements can be appropriately combined. Furthermore, various constituent elements can be omitted, replaced or changed within the scope of the gist of the above-mentioned embodiments.

[0267] This application is based on the Japanese patent application (Japanese Patent Application No. 2022-060326) filed on March 31, 2022, the contents of which are incorporated herein by reference.

Claims

1. A glass block for a plasma-resistant component, comprising at least one of silicon, magnesium and calcium, And, let the alkali metal element be R 1 , alkaline earth metal elements are set as R 2 When the molar percentage is expressed as oxide, The total content of MgO and CaO is 3.0 mol% or more and less than 29.0 mol%, R 2 The content of O is 3.0 mol% or more and less than 35.0 mol%, R 1 The content of 2O is 8.0 mol % or less.

2. The glass block according to claim 1, wherein: The content of SiO2 is greater than 40.0 mol% and less than 90.0 mol%, and the content of B2O3 is less than 30.0 mol%.

3. The glass block according to claim 1, wherein: The ratio of the content of SrO to the total content of MgO and CaO is less than 0.50, and the content of SrO is less than 15.0 mol %.

4. The glass block according to claim 1, wherein: The ratio of the total content of BaO and SrO to the total content of MgO and CaO is less than 0.

45.

5. The glass block according to claim 1, wherein: The ratio of the content of BaO to the total content of MgO and CaO is less than 0.

35. The glass block according to claim 1 , wherein an average thermal expansion coefficient at 50 to 350° C. is 5.0 ppm / ° C. or less.

7. The glass block according to claim 1, wherein: The content of Al2O3 and R 2 The content ratio of O is less than 0.6, and the content of Al2O3 is less than 20.0 mol%.

8. The glass block according to claim 1, wherein: The content of fluorine is 5.0 mass % or less relative to the total mass of the glass block.

9. The glass block according to claim 1, wherein: The visible light transmittance is more than 60%.

10. The glass block according to claim 1, wherein: The ratio of the content of MgO to the total content of MgO and CaO is 0.1 to 0.

9.

11. The glass block according to claim 1, wherein: The content of P2O5 is greater than 0.1 mol % and less than 5.5 mol %.

12. The glass block according to claim 1, wherein: R 2 The content of O is 3.0 mol% or more and less than 20.0 mol%.

13. A method for producing a glass block, the method being a method for producing the glass block according to any one of claims 1 to 12, Glass raw materials are heated to 1650° C. or lower to be melted, and the obtained molten glass is formed and slowly cooled.

14. A plasma-resistant member, comprising the glass block according to any one of claims 1 to 12.

15. The plasma-resistant component according to claim 14, mounted on a plasma etching device. As window material, top plate, microwave inlet tube, lift pin, nozzle, edge ring, electrostatic chuck, shower plate or protective cover for chamber sensors.