Laminated glass
By setting a P-polarized light reflective film in the assumed projection area of the laminated glass and controlling the residual stress Δσ, the problem of obvious secondary images was solved, and a clear display of the HUD image was achieved.
Patent Information
- Application Number
- CN202380029942.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-30
- Filing Date
- 2023-03-28
- Publication Date
- 2024-11-15
AI Technical Summary
When existing laminated glass is poorly designed, the P-polarized light reflective film can cause obvious secondary images, affecting the visibility of the HUD image.
By setting a P-polarized light reflective film in the assumed projection area of the laminated glass and controlling the residual stress Δσ in the assumed projection area to satisfy specific inequalities (Equations 1, 2 and 3), the reflectivity of the secondary image can be reduced.
It effectively suppresses secondary images, improves the visibility of the HUD image, and ensures the clear display of the primary image.
Smart Images

Figure CN118973977A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to laminated glass. Background Art
[0002] In recent years, head-up displays (hereinafter also referred to as HUDs) that reflect images on the front windshield of a vehicle and display specific information in the driver's field of vision have been increasingly promoted. One of the issues of HUDs is to improve the visibility of HUD images, and attempts have been made to reduce secondary images (double images or triple images, etc.) for this purpose.
[0003] As an example, the following technology can be cited: a P-polarized light reflecting film composed of a coating or film that reflects P-polarized light is provided to the laminated glass, and the P-polarized light is incident on the laminated glass at an incident angle of the Brewster angle, thereby reducing the reflectivity of the P-polarized light refracted on the inner surface of the laminated glass on the outer surface of the vehicle, thereby suppressing the secondary image, and the HUD image is clearly projected mainly by reflection only on the P-polarized light reflecting film.
[0004] Prior art literature
[0005] Patent Literature
[0006] Patent Document 1: Japanese Patent No. 6302140 Summary of the invention
[0007] Technical problem to be solved by the invention
[0008] However, even in laminated glass having a P-polarized light reflective film, if the glass plates or the intermediate film constituting the laminated glass are not designed appropriately, the secondary image may become conspicuous, thereby reducing the visibility of the HUD image.
[0009] The present invention has been made in view of the above-mentioned problems, and an object of the present invention is to suppress secondary images in laminated glass having a P-polarized light reflecting film and to improve the visibility of a HUD image.
[0010] Solutions to technical problems
[0011] A laminated glass according to one embodiment of the present disclosure is a laminated glass comprising a first glass plate, a second glass plate, and an intermediate film located between the first glass plate and the second glass plate and bonding the first glass plate and the second glass plate together, wherein a projection assumed area used in a head-up display and into which P-polarized light can be incident from the first glass plate side is defined in a portion of the laminated glass, a P-polarized light reflecting film is provided in the projection assumed area, and a residual stress Δσ [MPa] in the projection assumed area satisfies an inequality obtained by combining the following equations (1), (2), and (3) with Rp, Ts, and t as variables.
[0012] ((1-Rp)×X×Ts 2 ×Rs) / Rp≤0.1……(1)
[0013] X=sinδ……(2)
[0014] Δσ=δ / 2π×λ / C / t……(3)
[0015] Here, when the P polarized light enters the projection assumed area of the laminated glass from the first glass plate side at an incident angle of 57 degrees, the P polarized light reflectance of the laminated glass is Rp, the P polarized light transmittance is (1-Rp), the polarization conversion factors of the first glass plate and the second glass plate are X, the S polarized light transmittance of the laminated glass is Ts, the S polarized light reflectance of the outer main surface of the second glass plate is Rs, the phase difference generated inside the first glass plate and the second glass plate is δ, and the circumference is π, the wavelength λ of the P polarized light is 555 [nm], the photoelastic coefficient C is 2.8 [nm / mm / MPa], and the total plate thickness of the first glass plate and the second glass plate is t [mm].
[0016] Effects of the Invention
[0017] According to one embodiment of the present disclosure, it is possible to suppress a secondary image in a laminated glass having a P-polarized light reflective film and improve the visibility of a HUD image. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 : is a schematic diagram showing the HUD system of the first embodiment.
[0019] Figure 2 It is a diagram illustrating the laminated glass according to the first embodiment.
[0020] Figure 3 A diagram illustrating the projection assumption area.
[0021] Figure 4 It is a diagram illustrating a laminated glass according to a modified example of the first embodiment.
[0022] Figure 5 These are diagrams for explaining examples and comparative examples. DETAILED DESCRIPTION
[0023] The following is a description of the method for implementing the invention with reference to the accompanying drawings. In each of the accompanying drawings, the same structural parts are marked with the same symbols, and repeated descriptions are sometimes omitted. In addition, in each of the accompanying drawings, in order to facilitate understanding of the content of the present invention, the size and shape are sometimes exaggerated.
[0024] The vehicle typically refers to an automobile, but also refers to a moving object capable of carrying laminated glass, including a train, a ship, an airplane, and the like.
[0025] In addition, the term "top view" refers to observing the object from the direction of the normal line passing through the center of gravity of the main surface of the object, and the shape seen at this time is called a planar shape.
[0026] In addition, the expressions "upper" and "lower" refer to upper and lower when the laminated glass is mounted on a vehicle.
[0027] In addition, the outermost side of a specific member is referred to as a "periphery", and a region of a specific member that is inscribed in the "periphery" and has a certain width is referred to as a "peripheral portion".
[0028] <First Embodiment>
[0029] [HUD system]
[0030] Figure 1 : is a schematic diagram showing the HUD system of the first embodiment. Figure 1 The HUD system 1 shown includes a laminated glass 10, a light source 50, a first optical system 60, an image display element 70, a second optical system 80, and a concave mirror 90. The HUD system 1 is a head-up display system for a vehicle that displays a virtual image on the outer side of the laminated glass 10. In addition, in the HUD system 1, the first optical system 60 and the second optical system 80 can be provided as needed.
[0031] The laminated glass 10 is, for example, a windshield for a vehicle, and P-polarized visible light is incident from the inside of the vehicle. The laminated glass 10 includes a P-polarized light reflecting film 15 in the region where the P-polarized visible light reflected by the concave mirror 90 is incident. The P-polarized light reflecting film 15 may be formed on the entire surface of the laminated glass 10, or may be formed only in the visible light transmission region of the laminated glass 10 excluding the shielding layer 14 described later. The P-polarized light reflecting film 15 only needs to be formed in the region where at least the P-polarized light emitted from the light source 50 is irradiated, and the edge of the P-polarized light reflecting film 15 may be formed near the outer periphery of the laminated glass 10 or on or near the shielding layer 14 so that the edge is not conspicuous.
[0032] Light source 50 is a light source that emits P-polarized visible light, such as a light emitting diode or a laser. Light source 50 may include optical components such as a polarizer or a lens that converts S-polarized light into P-polarized light. Light source 50 is composed of three light sources, for example, a red light source, a green light source, and a blue light source.
[0033] The first optical system 60 is composed of, for example, a prism or a lens that synthesizes light emitted from a plurality of light sources. The image display element 70 is an element that generates an intermediate image, such as a liquid crystal display element or an organic light emitting element. The second optical system 80 is composed of, for example, a lens or a reflector. The concave mirror 90 is an optical component that reflects the intermediate image with a reflective surface having a specific curvature, and is arranged at a position closest to the laminated glass 10 among the optical components arranged on the optical path between the light source 50 and the laminated glass 10.
[0034] In the HUD system 1, light emitted from the light source 50 reaches the image display element 70 via the first optical system 60, and forms an intermediate image on the image display element 70. The intermediate image formed on the image display element 70 is magnified via the second optical system 80 and the concave mirror 90, and irradiated onto the P polarized light reflecting film 15 of the laminated glass 10. The intermediate image irradiated onto the P polarized light reflecting film 15 is mainly reflected by the P polarized light reflecting film 15 and guided to the viewpoint position P of the passenger, and the passenger sees the intermediate image as a virtual image V (HUD image) in front of the laminated glass 10. The passenger is, for example, a driver of a vehicle.
[0035] Figure 1 Here, θ is the incident angle when the P-polarized visible light emitted from the light source 50 enters the P-polarized light reflecting film 15 via a specific optical system. The incident angle θ may be 57 degrees (Brewster angle), or may be larger or smaller than 57 degrees.
[0036] The HUD system 1 may have any other configurations as long as it has at least the laminated glass 10 and the light source 50. The HUD system 1 may be a laser scanning system in which a light scanning unit composed of a MEMS (Micro Electro Mechanical Systems) or the like scans laser light.
[0037] [Laminated glass]
[0038] Figure 2 FIG. 1 is a diagram illustrating a laminated glass according to a first embodiment. Figure 2 (a) is a diagram schematically showing a laminated glass viewed from inside a vehicle cabin to outside the vehicle cabin, Figure 2 (b) is along Figure 2 (a) is a partial enlarged cross-sectional view of line AA.
[0039] like Figure 2 As shown, the laminated glass 10 is a laminated glass for a vehicle including a first glass plate 11, a second glass plate 12, an intermediate film 13, a shielding layer 14, and a P-polarized light reflecting film 15. The laminated glass 10 can be applied to, for example, a windshield of a vehicle.
[0040] The first glass plate 11 and the second glass plate 12 are bonded via the intermediate film 13. The first glass plate 11 is arranged on the first side which becomes the vehicle interior side when the laminated glass 10 is installed in the vehicle, and the second glass plate 12 is arranged on the second side which becomes the vehicle exterior side when the laminated glass 10 is installed in the vehicle. In addition, the shielding layer 14 is provided as needed.
[0041] The laminated glass 10 is, for example, a multi-curved shape that is curved in two directions, the vertical direction and the horizontal direction, when installed on a vehicle. However, the multi-curved shape is not limited to a shape that is curved in the vertical direction and the horizontal direction when installed on a vehicle, and also includes a shape that is curved in any two or more different directions. Alternatively, the laminated glass 10 may be a single-curved shape that is curved only in the vertical direction or the horizontal direction when installed on a vehicle. However, the single-curved shape is not limited to a shape that is curved only in the vertical direction or the horizontal direction when installed on a vehicle, and also includes a shape that is curved only in any one direction.
[0042] The laminated glass 10 is preferably bent to be convex toward the outside of the vehicle. That is, the second glass plate 12 is preferably bent to be convex toward the side opposite to the intermediate film 13, and the first glass plate 11 is preferably bent to be convex toward the intermediate film 13 side. Figure 2 In (a), the laminated glass 10 is trapezoidal in plan view, but the laminated glass 10 is not limited to the trapezoidal shape, and may be any shape including a rectangle.
[0043] The first glass plate 11 is a vehicle interior glass plate that becomes the vehicle interior side (first side) when the laminated glass 10 is installed in a vehicle, and the second glass plate 12 is a vehicle exterior glass plate that becomes the vehicle exterior side (second side) when the laminated glass 10 is installed in a vehicle.
[0044] In the laminated glass 10, the minimum value of the radius of curvature is preferably greater than 500 mm and less than 100000 mm. The radius of curvature of the first glass plate 11 and the second glass plate 12 may be the same or different. When the radius of curvature of the first glass plate 11 and the second glass plate 12 are different, the radius of curvature of the first glass plate 11 is preferably smaller than the radius of curvature of the second glass plate 12.
[0045] The first glass plate 11 and the second glass plate 12 are a pair of glass plates facing each other, and the intermediate film 13 is located between the pair of glass plates. The first glass plate 11 and the second glass plate 12 are fixed in a state of sandwiching the intermediate film 13. The intermediate film 13 is a film that bonds the first glass plate 11 and the second glass plate 12.
[0046] The outer peripheral side of the intermediate film 13 is preferably edge-processed. That is, the outer peripheral side of the intermediate film 13 is preferably processed so as not to protrude significantly from the outer peripheral side of the first glass plate 11 and the second glass plate 12. If the amount of the outer peripheral side of the intermediate film 13 protruding from the outer peripheral side of the first glass plate 11 and the second glass plate 12 is 150 μm or less, it is preferred from the perspective of not impairing the appearance. The first glass plate 11, the second glass plate 12, and the intermediate film 13 will be described later.
[0047] The shielding layer 14 is an opaque layer, for example, provided in a strip shape along the peripheral portion of the laminated glass 10. The shielding layer 14 is, for example, an opaque colored ceramic layer, and its color is arbitrary, but preferably a dark color such as black, brown, gray, dark navy blue, and more preferably black. The shielding layer 14 may be a colored interlayer film or a colored film having a light-shielding property, a combination of a colored interlayer film and a colored ceramic layer, or a layer having a light-adjusting function. The colored film may also be integrated with an infrared reflective film or the like.
[0048] The width of the shielding layer 14 is, for example, about 10 mm to 250 mm, preferably 20 mm to 220 mm, and more preferably 30 mm to 200 mm when viewed from above. The presence of the opaque shielding layer 14 on the laminated glass 10 can prevent the adhesive made of a resin such as polyurethane that holds the peripheral portion of the laminated glass 10 on the vehicle body from being degraded by ultraviolet rays.
[0049] The shielding layer 14 can be formed, for example, by applying a ceramic color paste containing a fusible glass material containing a black pigment on a glass plate by screen printing or the like and then firing it, but is not limited thereto. The shielding layer 14 can also be formed, for example, by applying an organic ink containing a black or dark pigment on a glass plate by screen printing or the like and then drying it.
[0050] The shielding layer 14 is, for example, provided only on the peripheral portion of the inner main surface of the second glass plate 12. However, the shielding layer 14 may be provided only on the peripheral portion of the outer main surface 11a of the first glass plate 11, or may be provided on both the peripheral portion of the inner main surface of the second glass plate 12 and the peripheral portion of the outer main surface 11a of the first glass plate 11. In addition, for the first glass plate 11 and the second glass plate 12, the inner main surface refers to the surface facing the intermediate film 13 side, and the outer main surface refers to the surface on the opposite side to the inner main surface.
[0051] A projection assumed region into which P polarized light can be incident from the first glass plate 11 side, which is used in a head-up display, is defined on a portion of the laminated glass 10. A P polarized light reflecting film 15 is provided in the projection assumed region. Figure 3 Describe the projection assumption area. Figure 3 This is a diagram for explaining the projection assumed area, and schematically shows a state where a laminated glass is viewed from inside a vehicle cabin to the outside of the vehicle cabin. Figure 3In the figure, the dividing line L1 is a straight line connecting the point P1 that bisects the upper side 10t of the laminated glass 10 in a plan view and the point P2 that bisects the lower side 10b in a plan view. In addition, the dividing line L2 is a straight line that is orthogonal to the dividing line L1 in a plan view and bisects the portion between the point P1 and the point P2 of the dividing line L1. In addition, the dividing line L3 is a line that indicates a position W=5 mm inside the inner edge of the shielding layer 14 in a plan view. Figure 3 In the example of FIG. 4 , the dividing line L3 is a trapezoid.
[0052] The area surrounded by the dividing line L3 is divided into four areas R1, R2, R3 and R4 by the dividing lines L1 and L2. The areas R1, R2, R3 and R4 are projection assumed areas. In addition, the laminated glass 10 is sometimes provided with a sensor area where a sensor such as a camera sends and / or receives information, but a small and independent transparent area surrounded by a shielding layer like the sensor area is not included in the projection assumed area. The projection assumed area can reflect light emitted from a light source of a HUD system configured in the vehicle when the laminated glass is installed in the vehicle.
[0053] like Figure 2 As shown, a HUD display area R for HUD is defined on the laminated glass 10. The HUD display area R is a display area that reflects a projection image emitted from the interior of the vehicle to display information. The HUD display area R is a range where light emitted from the light source 50 is irradiated onto the laminated glass 10 when the HUD display position is moved in the field of view based on SAE-J1757-2 (2018).
[0054] The HUD display area R is set to Figure 3 In any of the regions R1, R2, R3 and R4 of the projection assumption region shown. Figure 2 In the example of Figure 3 The HUD display area R may be set in the area R1 shown in FIG. 1 , but may also be set in the area R2, R3 or R4. In addition, the HUD display area R may also span Figure 3 In addition, the HUD display area R may also be set to any two or more of the areas R1, R2, R3 and R4 shown in FIG. Figure 3 Multiple locations within regions R1, R2, R3 and R4 are shown.
[0055] Figure 2 In the example of FIG. 1 , the P-polarized light reflective film 15 is provided on the entire outer principal surface 11a of the first glass plate 11. However, the P-polarized light reflective film 15 may be provided only in the HUD display region R and its vicinity. In addition, if the P-polarized light reflective film 15 is provided on the entire outer principal surface 11a of the first glass plate 11, it is preferable from the point of view that the boundary between the region where the P-polarized light reflective film 15 is provided and its surrounding region is not visible.
[0056] The P-polarized light reflecting film 15 is a film that reflects the P-polarized visible light incident from the concave mirror 90 toward the inside of the vehicle, and is, for example, a P-polarized light reflecting coating applied on the outer principal surface 11a of the first glass plate 11. A P-polarized light reflecting film may be used as the P-polarized light reflecting film 15 and attached to the outer principal surface 11a of the first glass plate 11 via an adhesive layer. The P-polarized light reflecting film 15 is transparent to visible light.
[0057] As the P polarized light reflective film 15, for example, a birefringent interference type polarizer composed of a polymer multilayer film containing two or more polymers with different refractive indices, a polarizer having a fine concave-convex structure called a wire grid type, a film containing a polarizer composed of a cholesteric liquid crystal layer, etc. can be used. In the case of using a P polarized light reflective film as the P polarized light reflective film 15, the thickness of the P polarized light reflective film is preferably 25 μm or more and 200 μm or less. The thickness of the P polarized light reflective film is more preferably 150 μm or less, and further preferably 100 μm or less.
[0058] When a P-polarized light reflective coating is used as the P-polarized light reflective film 15, it is preferable to use a P-polarized light reflective film in terms of excellent visibility in low-light conditions such as at night or at a wider viewing angle. In addition, the use of a P-polarized light reflective coating is preferable in terms of easy control of the film thickness and easy smoothing of the reflection surface to prevent the HUD image from being easily deformed.
[0059] When a P-polarized light reflective coating is used as the P-polarized light reflective film 15 , the film thickness of the P-polarized light reflective coating is, for example, 50 nm to 500 nm, preferably 50 nm to 400 nm, and more preferably 50 nm to 300 nm.
[0060] As the P-polarized light reflective coating, there can be exemplified a film having a certain degree of P-polarized light reflectivity, for example, a film having a laminated structure of a high refractive index film / a low refractive index film or a Low-e film. Among them, from the point of view of being able to highly maintain the P-polarized light reflectivity, a film having a laminated structure of a high refractive index film / a low refractive index film is preferred. In the case where the high refractive index film / the low refractive index film is a two-layer structure, for example, a high refractive index film and a low refractive index film are sequentially laminated on the outer principal surface 11a of the first glass plate 11. In the case where the high refractive index film / the low refractive index film is a three-layer structure or more, a high refractive index film and a low refractive index film are alternately laminated in any order on the outer principal surface 11a of the first glass plate 11.
[0061] The refractive index of the high refractive index film is 1.8 or more, 1.9 or more, 2.0 or more, or 2.1 or more, preferably 2.5 or less, at a wavelength of 550 nm. The refractive index of the low refractive index film is typically less than 1.8, 1.7 or less, or 1.6 or less, preferably 1.2 or more, at a wavelength of 550 nm.
[0062] Specifically, the high refractive index film preferably comprises at least one of the following: oxides of Zr, Nb, Sn, mixed oxides of Ti, Zr, Nb, Si, Sb, Sn, Zn, In, nitrides of Si, Zr, mixed nitrides of Si, Zr. The low refractive index film preferably comprises at least one of the following: silicon oxide, silicon oxynitride, silicon oxycarbide, or a mixture thereof, such as a mixed oxide of silicon and aluminum, or a mixed oxide of silicon and zirconium.
[0063] The first layer of the high refractive index film is optionally composed of one or more sublayers. The thickness (geometric film thickness) of the first layer of the high refractive index film is preferably 50nm to 100nm, and particularly preferably 60nm to 80nm. The first layer of the low refractive index film is optionally composed of one or more sublayers. The thickness (geometric film thickness) of the first layer of the low refractive index film is preferably 70nm to 160nm, and particularly preferably 80nm to 120nm.
[0064] The P-polarized light reflecting coating can be formed on the surface of the glass plate by, for example, a sputtering method or a CVD method.
[0065] The FOV (Field Of View) of the HUD image can be greater than 4deg×1deg, greater than 5deg×1.5deg, greater than 6deg×2deg, or greater than 7deg×3deg. If a P-polarized light reflective film is used as the P-polarized light reflective film 15, when the FOV of the HUD image is greater than 4deg×1deg, a larger HUD image than before will be projected on the laminated glass 10, making it easy to see the undulations of the P-polarized light reflective film. Therefore, it is preferred to control the thickness of the adhesive layer for bonding the P-polarized light film to an appropriate value to reduce the deformation of the HUD image.
[0066] In the HUD display area R of the laminated glass 10, the curvature in the horizontal direction is preferably a radius of 1000 mm or more and 100000 mm or less. In addition, in the HUD display area R of the laminated glass 10, the curvature in the vertical direction is preferably a radius of 4000 mm or more and 20000 mm or less, and more preferably a radius of 6000 mm or more and 20000 mm or less. If the curvatures in the vertical and horizontal directions are within the above ranges, the P-polarized light reflective film 15 is less likely to produce undulations, thereby reducing the deformation of the HUD image projected onto the P-polarized light reflective film 15. The horizontal direction here is Figure 3The vertical direction is the direction of the dividing line L2, and the vertical direction is the direction of the dividing line L1.
[0067] When the incident angle of the P polarized light incident on the P polarized light reflective film is 57 degrees and the incident P polarized light is completely reflected by the P polarized light reflective film 15, only the primary image is generated and no secondary image is generated. On the other hand, when the incident P polarized light is not completely reflected by the P polarized light reflective film 15, a secondary image is generated. The image observed with the highest brightness is the primary image, and the image observed with a brightness lower than that of the primary image is the secondary image.
[0068] If the design of the first glass plate 11, the second glass plate 12, and the intermediate film 13 constituting the laminated glass 10 is inappropriate, the secondary image will become conspicuous. For example, when P-polarized light enters the interior of the laminated glass 10, if there is residual stress in the first glass plate 11 and the second glass plate 12, part of the P-polarized light will be converted into S-polarized light and become elliptically polarized light. The S-polarized light component of the elliptically polarized light is reflected by the outer principal surface 12a of the second glass plate 12 and advances to the first glass plate 11 side, and is emitted to the outside of the laminated glass 10 through the P-polarized light reflective film 15, thereby generating a secondary image.
[0069] In particular, in the laminated glass 10, the residual stress in the area near the shielding layer 14 is high. This is because, when the first glass plate 11 and the second glass plate 12 are heated, bent and slowly cooled, the shielding layer 14 is not easy to cool, while the portion without the shielding layer 14 is easy to cool. Therefore, when the HUD display area R is set at a position near the shielding layer 14, the secondary image caused by the residual stress is particularly easy to become conspicuous. Therefore, for the laminated glass 10, in the projection assumption area, an appropriate relationship between the residual stress and the P polarized light reflectivity is defined, thereby suppressing the secondary image and improving the visibility of the HUD image. This is explained as follows.
[0070] According to the inventor's research, by making the secondary image reflectivity / primary image reflectivity below 10%, the secondary image becomes inconspicuous. In order to make the secondary image more inconspicuous, the secondary image reflectivity / primary image reflectivity is preferably below 7%, more preferably below 5%, and further preferably below 3%. The secondary image reflectivity / primary image reflectivity is the ratio of the secondary image brightness to the primary image brightness when P-polarized light is incident on the laminated glass 10 from the inside of the vehicle and the brightness of the primary image and the brightness of the secondary image are measured respectively with a brightness meter. The brightness is measured based on SAE J1757-2 (2018). Here, the main image brightness refers to the brightness of the image reflected by the main reflection surface. In addition, the main reflection surface refers to the surface that reflects the image observed with the highest brightness among the multiple images observed when P-polarized light is incident on the laminated glass 10 from the inside of the vehicle. In this embodiment, it is the surface on the side of the first glass plate 11 of the P-polarized light reflection film 15.
[0071] The laminated glass 10 is designed so that the residual stress Δσ [MPa] in the projection assumed area satisfies the inequality obtained by combining the following equations (1), (2) and (3) with Rp, Ts and t as variables. Here, the residual stress Δσ in the projection assumed area is the difference (principal stress difference) between the principal stresses (values integrated along the cross-sectional direction) acting on the first glass plate 11 and the second glass plate 12 in the projection assumed area. That is, the residual stress Δσ of the laminated glass 10 is the difference in principal stresses acting on the plane direction of the laminated glass 10, and can be measured using the photoelastic stress measurement system "EdgeMaster" manufactured by Stress Photonics. "Edge Master" is a device for measuring the residual stress of the edge portion of the laminated glass, but it is possible to remove the fixture, etc. to measure the residual stress Δσ in the projection assumed area. The residual stress Δσ can represent either compressive stress or tensile stress, and its absolute value is used regardless of the sign.
[0072] ((1-Rp)×X×Ts 2 ×Rs) / Rp≤0.1……(1)
[0073] X=sinδ……(2)
[0074] Δσ=δ / 2π×λ / C / t……(3)
[0075] Here, when P-polarized light enters the projection assumed area of the laminated glass from the first glass plate 11 side at an incident angle of 57 degrees, the P-polarized light reflectance of the laminated glass 10 is Rp, the P-polarized light transmittance is (1-Rp), the polarization conversion factor of the first glass plate 11 and the second glass plate 12 is X, the S-polarized light transmittance of the laminated glass 10 is Ts, the S-polarized light reflectance of the outer main surface 12a of the second glass plate 12 is Rs, and the phase difference generated inside the first glass plate 11 and the second glass plate 12 is δ. The circumference is π, the wavelength λ of the P-polarized light is 555 [nm], the photoelastic coefficient C is 2.8 [nm / mm / Mpa], and the total plate thickness of the first glass plate and the second glass plate is t [mm].
[0076] In addition, in formula (1), the units of P-polarized light reflectivity Rp, P-polarized light transmittance (1-Rp), polarization conversion rate X, and S-polarized light reflectivity Rs are not [%]. For example, when S-polarized light reflectivity Rs = 50 [%], S-polarized light reflectivity Rs in formula (1) = 0.5. When P-polarized light reflectivity Rp, P-polarized light transmittance (1-Rp), polarization conversion rate X, and S-polarized light reflectivity Rs are expressed as percentages, the unit of [%] is clearly indicated.
[0077] The S-polarized light reflectivity Rs of the outer main surface 12a of the second glass plate 12 is calculated by assuming that the incident angle of the P-polarized light incident on the laminated glass 10 is θ0 [deg], the refraction angle of the P-polarized light incident on the laminated glass 10 is θ1 [deg], the refractive index of air is N0, and the refractive index of the second glass plate 12 is N1: Rs = (N0COSθ0-N1COSθ1) / (N0COSθ0+N1COSθ1) 2 Here, θ1=arcsin(N0 / N1×sinθ0). In addition, θ0=57[deg], N0=1. In addition, N1 varies depending on the type of the second glass plate 12, and for example, N1=1.52.
[0078] Formula (3) is derived from Brewster's law. In formula (3), λ=555 [nm] is used because human visual acuity is highest at this wavelength.
[0079] In formula (1), the denominator Rp represents the main image reflectance, and the numerator ((1-Rp)×X×Ts 2 ×Rs) represents the secondary image reflectance. That is, if the intensity of the P polarized light incident on the laminated glass 10 is set to I, the P polarized light with an intensity of Rp×I is reflected on the surface of the laminated glass 10. This is the intensity of the primary image. The P polarized light with an intensity of (1-Rp)×I enters the interior of the laminated glass 10. A portion of the P polarized light with an intensity of (1-Rp)×I that enters the interior of the laminated glass 10 is converted into S polarized light with an intensity of (1-Rp)×X×I based on the polarization conversion rate X. Among them, the S polarized light multiplied by the polarization transmittance Ts reaches the outer main surface 12a of the second glass plate 12. That is, the intensity of the S polarized light reaching the outer main surface 12a is (1-Rp)×X×Ts×I.
[0080] Of the S polarized light reaching the outer principal surface 12a, the S polarized light multiplied by the S polarized light reflectivity Rs of the outer principal surface 12a is reflected by the outer principal surface 12a, and the S polarized light multiplied by the polarized light transmittance Ts reaches the outer principal surface 11a of the first glass plate 11, and is emitted to the outside of the laminated glass 10 through the P polarized light reflective film 15. That is, the intensity of the S polarized light emitted to the outside of the laminated glass 10 is (1-Rp)×X×Ts 2 ×Rs×I. This is the intensity of the secondary image. In addition, the reflection of S-polarized light on the outer main surface 11a or the P-polarized light reflecting film 15 and the absorption of S-polarized light in the laminated glass 10 are not included in the calculation here. This is because ignoring these items allows the intensity of S-polarized light to be evaluated more strictly.
[0081] Therefore, by making the residual stress Δσ in the projection assumed area satisfy the inequality that combines equations (1), (2) and (3), the secondary image reflectance / primary image reflectance of the laminated glass 10 is less than 0.1, that is, it can be less than 10% when expressed as a percentage, and the secondary image can be made inconspicuous. That is, by reducing the residual stress Δσ in the projection assumed area, the laminated glass 10 can suppress the polarization state of P polarized light from being destroyed and generate S polarized light. Thereby, the secondary image can be suppressed and the visibility of the HUD image can be improved.
[0082] In addition, the P-polarized light reflectance Rp is calculated by measuring the spectral reflectance described in JIS R 3106:2019 with P-polarized light of a visible light wavelength as the incident light at an incident angle of θ=57 degrees, and based on this, it is calculated according to the calculation method of the visible light reflectance described in JIS R 3106:2019. The S-polarized light transmittance Ts is calculated by measuring the spectral transmittance described in JIS R 3106:2019 with S-polarized light as the incident light, and based on this, it is calculated according to the calculation method of the visible light transmittance described in JIS R 3106:2019.
[0083] The residual stress Δσ is preferably less than 1 MPa, more preferably less than 0.8 MPa, further preferably less than 0.7 MPa, further preferably less than 0.6 MPa, and particularly preferably less than 0.4 MPa. For example, if the slow cooling time when the first glass plate 11 and the second glass plate 12 are slowly cooled is extended, the residual stress Δσ can be reduced. In addition, in the case of press-forming the first glass plate 11 and the second glass plate 12, the residual stress Δσ can be reduced by suppressing the temperature distribution in the glass surface during the vacuum process of the vacuum nozzle or the slow cooling process using the blowing mouth. In particular, from the viewpoint of suppressing the deformation of the HUD image, it is preferred that the first glass plate 11 and the second glass plate 12 are formed by press forming, but the residual stress Δσ can also be reduced as in the present invention by lowering the forming temperature for bending the glass to be lower than before, or extending the slow cooling process to take longer than before.
[0084] In addition, the S-polarized light transmittance of the first glass plate 11 and / or the second glass plate 12 at an incident angle of 57 degrees incident on the projection assumed area is preferably 70% or less, and more preferably 65% or less. If such a value is achieved, the S-polarized light transmittance Ts of the laminated glass 10 can be reduced, so the intensity of the S-polarized light emitted to the outside of the laminated glass 10 can be reduced, and the secondary image can be made inconspicuous. The S-polarized light transmittance Ts of the laminated glass 10 is preferably 80% or less, more preferably 75% or less, further preferably 70% or less, and further preferably 65% or less.
[0085] In the projection assumed area, the visible light transmittance of the first glass plate 11 and / or the second glass plate 12 may be 87% or less, or 84% or less. If such a value is used, the intensity of the S-polarized light emitted to the outside of the laminated glass 10 can be reduced, and the secondary image can be made inconspicuous. When the visible light transmittance of the first glass plate 11 and / or the second glass plate 12 is low, heat is easily absorbed during the glass plate forming and residual stress is easily generated. However, the laminated glass 10 can reduce the residual stress by, for example, extending the slow cooling time when the first glass plate 11 and the second glass plate 12 are slowly cooled after forming, so it does not matter if the visible light transmittance of the first glass plate 11 and / or the second glass plate 12 is reduced. The visible light transmittance can be measured by the standard method according to JIS R 3106:2019. In addition, in the projection assumed area, the visible light transmittance of the laminated glass 10 is preferably 70% or more.
[0086] In addition, in the projection assumption area, the difference in visible light transmittance between the first glass plate 11 and the second glass plate 12 may be 3% or more, 5% or more, or 8% or more. When there is a difference in visible light transmittance between the first glass plate 11 and the second glass plate 12, there will be a difference in the slow cooling time when the glass plates are formed, so residual stress is likely to be generated. However, the laminated glass 10 can reduce the residual stress by extending the slow cooling time when the first glass plate 11 and the second glass plate 12 are formed and then slowly cooled, so there is no problem even if there is a difference in visible light transmittance between the first glass plate 11 and the second glass plate 12.
[0087] In addition, in the projection assumption area, the thickness of the second glass plate 12 may be 1.9 mm or more, 2.2 mm or more, or 2.4 mm or more. If such a value is used, the strength of the flying stone resistance performance and the like is sufficient. When the thickness of the second glass plate 12 is increased, heat is easily absorbed during the glass plate forming process and residual stress is easily generated. However, the laminated glass 10 can reduce the residual stress by extending the slow cooling time when the second glass plate 12 is formed and slowly cooled, so it is not a problem even if the thickness of the second glass plate 12 is increased.
[0088] In addition, in the projection assumed area, the total thickness of the laminated glass 10 is preferably 4.6 mm or less, and more preferably 4.4 mm or less. By reducing the total thickness of the laminated glass 10, the separation amount of the secondary image relative to the primary image becomes smaller, so that the secondary image can be made less conspicuous. In addition, the laminated glass 10 can be made lighter. In addition, if the visible light transmittance of the first glass plate 11 is greater than the visible light transmittance of the second glass plate 12, it is preferable to reduce the total thickness of the laminated glass 10 while maintaining the secondary image in a dark state.
[0089] In addition, in the projection assumed area, the thickness of the first glass plate 11 may be 1.8 mm or less, 1.6 mm or less, 1.3 mm or less, 1.0 mm or less, 0.7 mm or less, or 0.5 mm or less. If such a value is used, the total thickness of the laminated glass 10 can be reduced while maintaining the thickness of the second glass plate 12. As a result, the laminated glass 10 can reduce the separation amount of the secondary image with respect to the primary image and achieve weight reduction.
[0090] In addition, in the projection assumption area, the difference in thickness between the first glass plate 11 and the second glass plate 12 may be greater than 0.1 mm, or greater than 0.3 mm. When there is a difference in thickness between the first glass plate 11 and the second glass plate 12, there will be a difference in the slow cooling time when the glass plates are formed, so residual stress is likely to be generated. However, the laminated glass 10 can reduce the residual stress by extending the slow cooling time when the first glass plate 11 and the second glass plate 12 are slowly cooled after being formed, so there is no problem even if there is a difference in thickness between the first glass plate 11 and the second glass plate 12.
[0091] In addition, the S-polarized light transmittance of the intermediate film 13 when the incident angle is 57 degrees into the projection assumed area is preferably 73% or less. If it is such a value, the S-polarized light transmittance Ts of the laminated glass 10 can be reduced, so the intensity of the S-polarized light emitted to the outside of the laminated glass 10 can be reduced, and the secondary image can be made inconspicuous.
[0092] In addition, in the projection assumed area, the visible light transmittance of the intermediate film 13 may be 90% or more. In this case, it is better to reduce the visible light transmittance of the first glass plate 11 and / or the second glass plate 12 to attenuate the secondary image. However, as described above, when the visible light transmittance of the first glass plate 11 and / or the second glass plate 12 is low, it is easy to absorb heat during the glass plate forming and to generate residual stress. However, the laminated glass 10 can reduce the residual stress by extending the slow cooling time when the first glass plate 11 and the second glass plate 12 are formed and slowly cooled, so it does not matter if the visible light transmittance of the first glass plate 11 and / or the second glass plate 12 is reduced.
[0093] In the projection assumed area, the P-polarized light reflectance Rp of the laminated glass 10 is preferably 10% or more. If the P-polarized light reflectance Rp of the laminated glass 10 is 10% or more, the main image becomes bright enough, so the visibility of the HUD image is improved. In addition, since the secondary image reflectance / primary image reflectance becomes large, the secondary image can be made less conspicuous.
[0094] In the projection assumed area, the P-polarized light reflectance Rp of the laminated glass 10 is preferably 12% or more, and more preferably 15% or more. The higher the P-polarized light reflectance Rp of the laminated glass 10, the higher the brightness of the main image, so the visibility of the HUD image is further improved. In addition, since the secondary image reflectance / primary image reflectance is further increased, the secondary image can be made less conspicuous.
[0095] In the projection assumed area, the P-polarized light reflectance Rp of the laminated glass 10 is preferably 25% or less, and more preferably 20% or less. If the P-polarized light reflectance Rp of the laminated glass 10 is 25% or less, the reflection into the interior materials such as the instrument panel of the vehicle can be suppressed, and if it is 20% or less, the reflection can be further suppressed.
[0096] Usually, in a HUD system having a P-polarized light reflective film, a light source or an optical system is set so that the incident angle of the P-polarized light incident on the P-polarized light reflective film is about 57 degrees. However, since the position where the light source or optical system can be set in the HUD system having a P-polarized light reflective film is limited in the vehicle, the incident angle θ sometimes deviates from 57 degrees. Since the laminated glass 10 reduces the residual stress Δσ, the incident angle dependence of the secondary image is small, and even when the incident angle θ deviates from 57 degrees, the secondary image is not easy to be conspicuous. Therefore, the incident angle θ at at least a part of the HUD display area R can be above 60 degrees, and can also be above 65 degrees. However, if the incident angle θ significantly deviates from 57 degrees, the light passing through the P-polarized light reflective film 15 will increase, so the secondary image is easy to be conspicuous. Therefore, the incident angle θ is preferably above 42 degrees and below 72 degrees, more preferably above 47 degrees and below 67 degrees, and further preferably above 52 degrees and below 62 degrees.
[0097] It is preferred that the entire HUD display area R is at least 100 mm away from the edge of the laminated glass 10 and at least 20 mm away from the edge of the shielding layer 14 when viewed from above. This is because if the distance from the edge of the laminated glass 10 is at least 100 mm and the distance from the edge of the shielding layer 14 is at least 20 mm when viewed from above, the residual stress Δσ will be smaller. At least a portion of the HUD display area R may be arranged in an area within 200 mm from the edge of the laminated glass 10 or within 100 mm from the edge of the shielding layer 14. This is because the residual stress Δσ of the laminated glass 10 in this area is also sufficiently small.
[0098] The laminated glass 10 can be designed so that the residual stress Δσ satisfies the inequality that combines equations (1), (2) and (3) only in any one or more and no more than three of the regions R1, R2, R3 and R4 as the projection assumption region. For example, the laminated glass 10 can be designed so that the residual stress Δσ satisfies the inequality that combines equations (1), (2) and (3) only in the region R1 as the projection assumption region. In this case, the HUD system 1 can be designed so that the HUD display region R is set in region 1. That is, in the present application, "the residual stress Δσ in the projection assumption region satisfies the inequality that combines equations (1), (2) and (3) with Rp, Ts and t as variables" means that the residual stress Δσ satisfies the inequality that combines equations (1), (2) and (3) in any one or more of the regions R1, R2, R3 and R4.
[0099] In addition, the conspicuity of the secondary image also changes according to the projection distance of the HUD image. The projection distance of the HUD image is preferably more than 2m, more preferably more than 3m, further preferably more than 5m, and particularly preferably more than 10m. Here, the projection distance of the HUD image refers to the distance from the center of the field of view based on SAE J 1757-2 (2018) to the focal position of the virtual image V. The measurement method of the HUD focal distance is based on SAE J1757-2 (2018). If the projection distance of the HUD image becomes longer, the separation of the secondary image from the main image will be suppressed while the secondary image becomes darker, so the secondary image becomes inconspicuous. Moreover, if the projection distance of the HUD image becomes longer, the HUD image will be close to the focal distance of the driver during driving, so the visibility of the HUD image is improved.
[0100] Next, the first glass plate 11 , the second glass plate 12 , and the intermediate film 13 will be described in detail.
[0101] [glass plate]
[0102] The first glass plate 11 and the second glass plate 12 may be inorganic glass or organic glass. As inorganic glass, for example, soda-lime glass, aluminosilicate glass, borosilicate glass, alkali-free glass, quartz glass, etc. may be used without particular limitation. The second glass plate 12 located outside the laminated glass 10 is preferably inorganic glass from the viewpoint of scratch resistance, and preferably soda-lime glass from the viewpoint of formability. When the first glass plate 11 and the second glass plate 12 are soda-lime glass, transparent glass, green glass containing a predetermined amount or more of iron components, and dark green glass may be preferably used.
[0103] The inorganic glass may be any of unreinforced glass and reinforced glass. Unreinforced glass is glass formed by shaping molten glass into a flat plate and slowly cooling it. Reinforced glass is glass having a compressive stress layer formed on the surface of the unreinforced glass. In addition, in the case of reinforced glass, residual stress Δσ can be reduced by isotropically distributing stress.
[0104] Tempered glass may be, for example, physically tempered glass such as air-cooled tempered glass or chemically tempered glass. In the case of physically tempered glass, for example, by rapidly cooling a glass sheet uniformly heated during bending from a temperature near its softening point, other than slow cooling, a compressive stress layer is generated on the glass surface due to the temperature difference between the glass surface and the interior of the glass, thereby strengthening the glass surface.
[0105] In the case of chemically strengthened glass, the glass surface can be strengthened by generating compressive stress on the glass surface by ion exchange method, etc., or the glass surface can be strengthened by generating compressive stress on the glass surface after bending, etc. In addition, glass that absorbs ultraviolet rays or infrared rays can be used, and transparent glass is more preferably used, but a glass plate colored to the extent that transparency is not impaired can also be used.
[0106] On the other hand, examples of the material of the organic glass include polycarbonate, acrylic resins such as polymethyl methacrylate, and transparent resins such as polyvinyl chloride and polystyrene.
[0107] The first glass plate 11 and the second glass plate 12 are not limited to trapezoidal or rectangular shapes, and may be processed into shapes with various shapes and curvatures. In the bending forming of the first glass plate 11 and the second glass plate 12, gravity forming, pressure forming, roll forming, etc. may be used. There is no particular limitation on the forming method of the first glass plate 11 and the second glass plate 12. For example, in the case of inorganic glass, glass plates formed by a float process or the like are preferred.
[0108] The thickness of the second glass plate 12 is preferably 1.1 mm or more and 3 mm or less at the thinnest portion. When the thickness of the second glass plate 12 is 1.1 mm or more, the strength of the flying stone resistance performance and the like is sufficient, and when the thickness is 3 mm or less, the mass of the laminated glass 10 does not become too large, which is preferable from the viewpoint of vehicle fuel consumption. The thickness of the second glass plate 12 is more preferably 1.8 mm or more and 2.8 mm or less at the thinnest portion, further preferably 1.8 mm or more and 2.6 mm or less, further preferably 1.8 mm or more and 2.2 mm or less, and further preferably 1.8 mm or more and 2.1 mm or less.
[0109] The thickness of the first glass plate 11 is preferably 0.3 mm or more and 2.3 mm or less. When the thickness of the first glass plate 11 is 0.3 mm or more, the handling property is good, and when the thickness is 2.3 mm or less, the weight does not become too large.
[0110] In addition, when the thickness of the first glass plate 11 is inappropriate, when two glasses with particularly deep bends are formed as the first glass plate 11 and the second glass plate 12, the two glasses will not match in shape, which will have a great impact on the glass quality such as residual stress after crimping.
[0111] However, by setting the thickness of the first glass plate 11 to be between 0.3 mm and 2.3 mm, the glass quality such as residual stress can be maintained. Setting the thickness of the first glass plate 11 to be between 0.3 mm and 2.3 mm is particularly effective in maintaining the glass quality of deeply curved glass. The thickness of the first glass plate 11 is more preferably between 0.5 mm and 2.2 mm, and further preferably between 0.7 mm and 2.1 mm. Within this range, the above-mentioned effect is more significant.
[0112] A film having waterproofing, ultraviolet or infrared cut-off function, or a film having low reflection property or low radiation property may be provided on the outer side of the first glass plate 11 and / or 12. In addition, a film having ultraviolet or infrared cut-off or low radiation property, visible light absorption, coloring, etc. may be provided on the side of the first glass plate 11 and / or 12 in contact with the intermediate film 13.
[0113] When the first glass plate 11 and the second glass plate 12 are inorganic glasses in a curved shape, the first glass plate 11 and the second glass plate 12 are bent after being formed by a float process or the like and before being bonded via the intermediate film 13. The bending is performed by heating to soften the glass. The heating temperature of the glass during the bending can be controlled in the range of approximately 550° C. to 700° C.
[0114] [Intermediate film]
[0115] As the intermediate film 13, a thermoplastic resin is generally used, for example, thermoplastic resins conventionally used for such purposes such as plasticized polyvinyl acetal resins, plasticized polyvinyl chloride resins, saturated polyester resins, plasticized saturated polyester resins, polyurethane resins, plasticized polyurethane resins, ethylene-vinyl acetate copolymer resins, ethylene-ethyl acrylate copolymer resins, cycloolefin polymer resins, ionomer resins, etc. In addition, a resin composition containing a hydrogenated modified block copolymer described in Japanese Patent No. 6065221 can also be preferably used.
[0116] Among them, plasticized polyvinyl acetal resins are preferably used because of their excellent balance of various properties such as transparency, weather resistance, strength, adhesion, penetration resistance, impact energy absorption, moisture resistance, heat insulation and sound insulation. These thermoplastic resins can be used alone or in combination of two or more. The "plasticity" in the above-mentioned plasticized polyvinyl acetal resins means that they can be plasticized by adding a plasticizer. The same meaning is also expressed for other plasticized resins.
[0117] However, when a specific object is enclosed in the intermediate film 13, the enclosed object may be degraded due to a specific plasticizer, depending on the type of the enclosed object. In this case, it is preferred to use a resin that does not substantially contain the plasticizer. As a resin that does not contain a plasticizer, ethylene-vinyl acetate copolymer (EVA) resins and the like can be cited.
[0118] As the above-mentioned polyvinyl acetal resin, polyvinyl formal resin obtained by reacting polyvinyl alcohol (PVA) with formaldehyde, polyvinyl acetal resin in a narrow sense obtained by reacting PVA with acetaldehyde, polyvinyl butyral resin (PVB) obtained by reacting PVA with n-butyraldehyde, etc. can be exemplified, and PVB is suitable from the viewpoint of excellent balance of various properties such as transparency, weather resistance, strength, adhesion, penetration resistance, impact energy absorption, moisture resistance, heat insulation and sound insulation. These polyvinyl acetal resins can be used alone or in combination of two or more.
[0119] However, the material forming the intermediate film 13 is not limited to thermoplastic resins. The intermediate film 13 may also contain functional particles such as infrared absorbers, ultraviolet absorbers, and luminescent agents. In addition, the intermediate film 13 may have a colored portion called a light-shielding band. As the coloring pigment used to form the colored portion, any coloring pigment that can be used as a plastic and whose visible light transmittance is adjusted to 40% or less by adjusting the amount added, for example, organic coloring pigments such as azo, phthalocyanine, quinacridone, perylene, pyrene, dioxazine, anthraquinone, and isoindolinone, or inorganic coloring pigments such as oxides, hydroxides, sulfides, chromic acid, sulfates, carbonates, silicates, phosphates, arsenates, ferrocyanide, carbon, and metal powders may be cited. These coloring pigments may be used alone or in combination of two or more.
[0120] The intermediate film 13 may have a plurality of layers. For example, the intermediate film 13 may have three or more layers. For example, if three or more intermediate films are formed and the plasticizer is adjusted so that the shear elastic modulus of any layer other than the two side layers is smaller than the shear elastic modulus of the two side layers, the sound insulation of the laminated glass 10 can be improved. In this case, the shear elastic modulus of the two side layers may be the same or different.
[0121] The thickness of the intermediate film 13 is preferably 0.5 mm or more at the thinnest part. In addition, when the intermediate film 13 has multiple layers, the thickness of the intermediate film 13 refers to the thickness of the film thickness of each layer added together. If the thickness of the thinnest part of the intermediate film 13 is 0.5 mm or more, the impact resistance required as a laminated glass is sufficient. In addition, the thickness of the intermediate film 13 is preferably 3 mm or less at the thickest part. If the maximum value of the thickness of the intermediate film 13 is 3 mm or less, the mass of the laminated glass will not become too large. The maximum value of the thickness of the intermediate film 13 is more preferably 2.8 mm or less, and further preferably 2.6 mm or less.
[0122] In addition, when the intermediate film 13 has a plurality of layers, each layer included in the intermediate film 13 is preferably formed of the same material, but may be formed of different materials. However, from the viewpoint of adhesion with the first glass plate 11 and the second glass plate 12, or functional materials sealed in the laminated glass 10, it is preferred that the above-mentioned material is used for 50% or more of the film thickness of the intermediate film 13.
[0123] The intermediate film 13 is manufactured by, for example, appropriately selecting the above-mentioned resin material forming the intermediate film and extruding it in a heated molten state using an extruder. Extrusion conditions such as the extrusion speed of the extruder are set to uniform conditions. Then, the resin film obtained by extrusion is made to match the design of the laminated glass, for example, it is stretched as needed so that the upper and lower sides of the resin film have curvature, thereby completing the intermediate film 13.
[0124] [Laminated glass]
[0125] The total thickness of the laminated glass 10 is preferably 2.8 mm or more and 10 mm or less. When the total thickness of the laminated glass 10 is 2.8 mm or more, sufficient rigidity can be ensured. When the total thickness of the laminated glass 10 is 10 mm or less, sufficient transmittance can be obtained and haze can be reduced.
[0126] The plate deviation between the first glass plate 11 and the second glass plate 12 is preferably 1.5 mm or less, more preferably 1 mm or less, on at least one side of the laminated glass 10. Here, the plate deviation between the first glass plate 11 and the second glass plate 12 refers to the deviation between the outer peripheral side of the first glass plate 11 and the outer peripheral side of the second glass plate 12 in a plan view.
[0127] It is preferred that the plate deviation between the first glass plate 11 and the second glass plate 12 is 1.5 mm or less on at least one side of the laminated glass 10 in order not to impair the appearance. It is more preferred that the plate deviation between the first glass plate 11 and the second glass plate 12 is 1.0 mm or less on at least one side of the laminated glass 10 in order not to impair the appearance.
[0128] The laminated glass 10 is manufactured by forming a P-polarized light reflective film 15 on the outer main surface 11a of the first glass plate 11, and then sandwiching an intermediate film 13 between the first glass plate 11 and the second glass plate 12 so that the P-polarized light reflective film 15 is on the outer side to form a laminate. Then, for example, the laminate is placed in a rubber bag, a rubber chamber, a bag made of resin, etc., and bonded under a temperature range of about 70°C to 110°C in a vacuum controlled at a gauge pressure range of -100 kPa to -65 kPa. The heating conditions, temperature conditions, and lamination method are appropriately selected.
[0129] Furthermore, for example, by controlling the temperature to be 100° C. to 150° C. and the absolute pressure to be 0.6 MPa to 1.5 MPa, a laminated glass 10 with better durability can be obtained. However, in some cases, in consideration of the simplification of the process and the characteristics of the material sealed in the laminated glass 10, this heating and pressing process may not be used.
[0130] Alternatively, a method called "cold bending" may be used in which one or both of the first glass sheet 11 and the second glass sheet 12 are joined in a mutually elastically deformed state. Cold bending can be achieved by using a laminate consisting of the first glass sheet 11, the intermediate film 13, and the second glass sheet 12 fixed by temporary fixing means such as tape, and a conventionally known pre-pressing device such as a nip roller, a rubber bag, a rubber chamber, and an autoclave.
[0131] Without prejudice to the effects of the present application, in addition to the intermediate film 13, a thin film or device having functions such as electric heating line, infrared reflection, light emission, power generation, dimming, touch screen, visible light reflection, scattering, decoration, absorption, etc. may be provided between the first glass plate 11 and the second glass plate 12. In addition, the surface of the laminated glass 10 may have a film having functions such as anti-fog, water repellent, heat insulation, low reflection, etc. In addition, a film having functions such as heat insulation and heating may be provided on the inner main surface of the first glass plate 11 or the inner main surface of the second glass plate 12.
[0132] 〈Variation Example〉
[0133] exist Figure 2 In the laminated glass 10 shown in the figure, an example is shown in which the P polarized light reflecting film 15 is provided on the outer main surface 11a of the first glass plate 11. However, this is not limited to this, and it is also possible to Figure 4 As in the laminated glass 10A shown in FIG. 1A , a P-polarized light reflective film 15 is provided on the inner principal surface 11b of the first glass plate 11. The P-polarized light reflective film 15 is, for example, a P-polarized light reflective coating applied on the inner principal surface 11b of the first glass plate 11. A P-polarized light reflective film may be used as the P-polarized light reflective film 15 and attached to the inner principal surface 11b of the first glass plate 11 via an adhesive layer.
[0134] Or, you can also do Figure 4 (b) As in the laminated glass 10B shown in FIG. 1 , a P-polarized light reflective film 15 is provided on the inner principal surface 12b of the second glass plate 12. The P-polarized light reflective film 15 is, for example, a P-polarized light reflective coating applied on the inner principal surface 12b of the second glass plate 12. A P-polarized light reflective film may be used as the P-polarized light reflective film 15 and attached to the inner principal surface 12b of the second glass plate 12 via an adhesive layer.
[0135] In the case of the laminated glasses 10A and 10B, similarly to the laminated glass 10, by making the residual stress Δσ in the projection assumption region satisfy the inequality that combines the equations (1), (2) and (3), the secondary image reflectivity / primary image reflectivity can be made 10% or less, and the secondary image can be made inconspicuous. In addition, if the P-polarized light reflecting film 15 is provided on the outer main surface 11a of the first glass plate 11 as in the laminated glass 10, the main reflecting surface becomes the surface on the first glass plate 11 side of the P-polarized light reflecting film 15, and the secondary image is limited to one, which is preferable from the viewpoint that the secondary image can be made more inconspicuous.
[0136] <Examples, Comparative Examples>
[0137] Assume that the first glass plate A and the second glass plate B are bonded via an intermediate film C, and a laminated glass is coated with a P-polarized light reflective film (a laminated film of TiZrO2 / SiO2, with a geometric film thickness of 73.9nm / 99.5nm) on the entire outer main surface of the first glass plate A. The first glass plate A, the second glass plate B, and the intermediate film C are assumed to be non-wedge-shaped in cross-sectional view and have a constant thickness. In addition, the calculation is performed assuming that P-polarized light (wavelength 555nm) enters the projected assumed area of the laminated glass at an incident angle of 57deg from the P-polarized light reflective film side. Specifically, by assuming that the first glass plate A and the second glass plate B in the laminated glass are various combinations and the residual stress Δσ is a specified value, it is calculated to determine whether the secondary image reflectance / primary image reflectance is less than 10%, that is, whether the formula (1) is satisfied. In addition, this calculation is usually performed when the optical performance of automotive glass is required, and is consistent with the actual numerical value.
[0138] First, the optical properties (refractive index, extinction coefficient) of the first glass sheet A, the second glass sheet B and the interlayer C constituting the laminated glass are set according to specific assumed glass sheets (green glass, dark green glass, clear glass) and interlayer films (transparent interlayer films).
[0139] Next, the visible light transmittance of the first glass plate A, the visible light transmittance of the second glass plate B, the visible light transmittance of the interlayer C, the P-polarized light reflectance Rp, the S-polarized light transmittance Ts, and the S-polarized light reflectance Rs of the laminated glass are obtained based on the optical properties (refractive index, extinction coefficient) and the thickness of the first glass plate A, the second glass plate B, and the interlayer C obtained as described above. The specific calculation method is shown in "Basic Theory of Optical Thin Films (Basic Theory of Optical Thin Films) - Supplementary Revised Edition - Kohiyama Mitsunobu (Optironics Co., Ltd.)".
[0140] Then, assuming a predetermined value for the residual stress Δσ, the phase difference δ is obtained according to equation (3), and the polarization conversion efficiency X is obtained using the phase difference δ according to equation (2). The secondary image reflectance = ((1-Rp) × X × Ts) is obtained using the polarization conversion efficiency X and the P polarization reflectance Rp, S polarization transmittance Ts, and S polarization reflectance Rs obtained above. 2 × Rs. Furthermore, considering that the primary image reflectance = the P-polarized light reflectance Rp, the secondary image reflectance / primary image reflectance is obtained.
[0141] The following describes examples and comparative examples, but the present invention is not limited to these examples. Examples 1 and 3 to 9 are examples, and Example 2 is a comparative example.
[0142] [Example 1]
[0143] Assuming that the first glass plate A is a 1.8 mm thick green glass, the second glass plate B is a 1.8 mm thick green glass, and the intermediate film C is a 0.76 mm thick transparent intermediate film, and assuming that the residual stress Δσ value is 0.9 MPa, the secondary image reflectivity / primary image reflectivity is calculated.
[0144] [Example 2]
[0145] Assuming that the first glass plate A is a 1.8 mm thick green glass, the second glass plate B is a 1.8 mm thick green glass, and the intermediate film C is a 0.76 mm thick transparent intermediate film, and assuming that the residual stress Δσ value is 1.3 MPa, the secondary image reflectivity / primary image reflectivity is calculated.
[0146] [Example 3]
[0147] Assuming that the first glass plate A is a 1.8 mm thick dark green glass, the second glass plate B is a 1.8 mm thick dark green glass, and the intermediate film C is a 0.76 mm thick transparent intermediate film, and assuming that the residual stress Δσ value is 0.9 MPa, the secondary image reflectivity / primary image reflectivity is calculated.
[0148] [Example 4]
[0149] Assuming that the first glass plate A is a green glass with a thickness of 1.8 mm, the second glass plate B is a dark green glass with a thickness of 1.8 mm, and the intermediate film C is a transparent intermediate film with a thickness of 0.76 mm, and assuming that the residual stress Δσ value is 0.9 MPa, the secondary image reflectivity / primary image reflectivity is calculated.
[0150] [Example 5]
[0151] Assuming that the first glass plate A is a 1.8 mm thick transparent glass, the second glass plate B is a 1.8 mm thick green glass, and the intermediate film C is a 0.76 mm thick transparent intermediate film, and assuming that the value of the residual stress Δσ is 1 MPa, the secondary image reflectivity / primary image reflectivity is calculated.
[0152] [Example 6]
[0153] Assuming that the first glass plate A is a 1.8 mm thick transparent glass, the second glass plate B is a 1.8 mm thick dark green glass, and the intermediate film C is a 0.76 mm thick transparent intermediate film, and assuming that the residual stress Δσ value is 1 MPa, the secondary image reflectivity / primary image reflectivity is calculated.
[0154] [Example 7]
[0155] Assuming that the first glass plate A is a 1.8 mm thick transparent glass, the second glass plate B is a 1.8 mm thick dark green glass, and the intermediate film C is a 0.76 mm thick transparent intermediate film, and assuming that the residual stress Δσ value is 0.6 MPa, the secondary image reflectivity / primary image reflectivity is calculated.
[0156] [Example 8]
[0157] Assuming that transparent glass with a thickness of 1.6 mm is used as the first glass plate A, dark green glass with a thickness of 1.8 mm is used as the second glass plate B, and a transparent intermediate film with a thickness of 0.76 mm is used as the intermediate film C, and assuming that the residual stress Δσ value is 0.9 MPa, the secondary image reflectivity / primary image reflectivity is calculated.
[0158] [Example 9]
[0159] Assuming that a transparent glass with a thickness of 2 mm is used as the first glass plate A, a dark green glass with a thickness of 2 mm is used as the second glass plate B, and a transparent intermediate film with a thickness of 0.76 mm is used as the intermediate film C, and assuming that the residual stress Δσ value is 1 MPa, the secondary image reflectivity / primary image reflectivity is calculated.
[0160] The calculation results of Examples 1 to 9 are shown in Figure 5 . Figure 5In the equation, the case where the secondary image reflectivity / primary image reflectivity (θ=57deg) is less than 5% is recorded as ◎, the case where it is greater than 5% and less than 10% is recorded as ○, and the case where it is greater than 10% is recorded as ×. That is, the case where the secondary image reflectivity / primary image reflectivity does not satisfy the formula (1) is recorded as ×, the case where the secondary image reflectivity / primary image reflectivity satisfies the formula (1) is recorded as ○, and the case where the secondary image reflectivity / primary image reflectivity satisfies the formula (1) is recorded as ◎.
[0161] like Figure 5 As shown in Examples 1 and 3 to 9, it can be seen that when the residual stress Δσ is 1 MPa or less, the secondary image reflectivity / primary image reflectivity (θ=57 degrees) can be made less than 10%. The results of Examples 1 and 3 to 9 show that if the residual stress Δσ is adjusted to less than 1 MPa by slow cooling time during the manufacturing process of laminated glass, a laminated glass that satisfies the requirements can be used. Figure 5 The first glass plate A and the second glass plate A of the conditions shown in Examples 1 and 3 to 9 make the secondary image reflectivity / primary image reflectivity less than 10%. That is, if the conditions satisfying Figure 5 By adjusting the residual stress Δσ to 1 MPa or less for the first glass sheet A and the second glass sheet A under the conditions shown in Examples 1 and 3 to 9, it is possible to realize a laminated glass in which a secondary image is less noticeable.
[0162] On the other hand, Example 2 shows that even if the same first glass sheet A and second glass sheet A as in Example 1 are used, the secondary image reflectivity / primary image reflectivity cannot be made less than 10% if the residual stress Δσ is assumed to be 1.3 MPa. That is, when the residual stress Δσ exceeds 1 MPa due to a short slow cooling time or the like, the secondary image reflectivity / primary image reflectivity cannot be made less than 10%, and thus the secondary image is conspicuous.
[0163] In addition, as shown in Example 3, when the visible light transmittance of the first glass sheet A and the second glass sheet B is low, heat is easily absorbed during the forming of the glass sheets, and residual stress is easily generated. However, if the residual stress Δσ is adjusted to 1 MPa or less by slow cooling time, etc., a laminated glass in which a secondary image is not easily conspicuous can be realized.
[0164] In addition, as in Examples 4 to 6, if there is a difference in visible light transmittance between the first glass sheet A and the second glass sheet B, there will be a difference in the slow cooling time when the glass sheets are formed, so residual stress is likely to be generated. However, if the residual stress Δσ is adjusted to 1 MPa or less by adjusting the slow cooling time, etc., a laminated glass in which a secondary image is not easily noticeable can be realized.
[0165] In addition, as shown in Example 8, when there is a difference in the thickness of the first glass sheet A and the second glass sheet B, a difference in the slow cooling time occurs when the glass sheets are formed, so residual stress is likely to be generated. However, if the residual stress Δσ is adjusted to 1 MPa or less by adjusting the slow cooling time, etc., a laminated glass in which a secondary image is not easily noticeable can be realized.
[0166] In addition, as shown in Example 9, when the first glass sheet A and the second glass sheet B are thick, heat is easily absorbed during the forming of the glass sheets, and residual stress is easily generated. However, if the residual stress Δσ is adjusted to 1 MPa or less by slow cooling time, etc., a laminated glass in which a secondary image is not easily conspicuous can be realized.
[0167] Although preferred embodiments and the like have been described in detail above, the present invention is not limited to the above embodiments and the like, and various modifications and substitutions may be made to the above embodiments and the like without departing from the scope described in the claims.
[0168] In addition to the above embodiment, the following supplementary notes are disclosed.
[0169] (Note 1)
[0170] A laminated glass comprising a first glass plate, a second glass plate, and an intermediate film located between the first glass plate and the second glass plate and bonding the first glass plate and the second glass plate.
[0171] A projection assumption area used in a head-up display and into which P-polarized light can be incident from the first glass plate side is defined in a portion of the laminated glass, and a P-polarized light reflecting film is provided in the projection assumption area.
[0172] The residual stress Δσ [MPa] in the projection assumption region satisfies the inequality obtained by combining the following equations (1), (2) and (3) with Rp, Ts and t as variables:
[0173] ((1-Rp)×X×Ts 2 ×Rs) / Rp≤0.1……(1)
[0174] X=sinδ……(2)
[0175] Δσ=δ / 2π×λ / C / t……(3)
[0176] Here, when the P polarized light enters the projection assumed area of the laminated glass from the first glass plate side at an incident angle of 57 degrees, the P polarized light reflectance of the laminated glass is Rp, the P polarized light transmittance is (1-Rp), the polarization conversion factors of the first glass plate and the second glass plate are X, the S polarized light transmittance of the laminated glass is Ts, the S polarized light reflectance of the outer main surface of the second glass plate is Rs, the phase difference generated inside the first glass plate and the second glass plate is δ, and the circumference is π, the wavelength λ of the P polarized light is 555 [nm], the photoelastic coefficient C is 2.8 [nm / mm / Mpa], and the total plate thickness of the first glass plate and the second glass plate is t [mm].
[0177] (Note 2)
[0178] The laminated glass according to Supplementary Note 1, wherein the residual stress Δσ is 1 MPa or less.
[0179] (Note 3)
[0180] The laminated glass according to Supplementary Note 1 or 2, wherein the residual stress Δσ is 0.7 MPa or less.
[0181] (Note 4)
[0182] The laminated glass according to any one of Appendixes 1 to 3, wherein the P-polarized light reflectivity Rp is 10% to 25%.
[0183] (Note 5)
[0184] The laminated glass according to any one of Supplementary Notes 1 to 4, wherein the P-polarized light reflective film is provided on the outer main surface of the first glass plate.
[0185] (Note 6)
[0186] The laminated glass according to any one of Supplementary Notes 1 to 5, wherein an S-polarized light transmittance Ts of the laminated glass when the incident angle of the laminated glass entering the projection assumed area is 57 degrees is 80% or less.
[0187] (Note 7)
[0188] The laminated glass as described in any one of Supplementary Notes 1 to 6, wherein the visible light transmittance of the first glass plate is greater than the visible light transmittance of the second glass plate.
[0189] (Note 8)
[0190] The laminated glass as described in any one of Supplementary Notes 1 to 7, wherein the total thickness of the projection assumed area is 4.6 mm or less.
[0191] (Note 9)
[0192] The laminated glass as described in any one of Supplementary Notes 1 to 8, wherein a thickness of the first glass plate in the projection assumed area is 1.8 mm or less.
[0193] (Note 10)
[0194] The laminated glass according to any one of Supplementary Notes 1 to 9, wherein an S-polarized light transmittance Ts of the laminated glass when the incident angle of the laminated glass entering the projection assumed area is 57 degrees is 75% or less.
[0195] (Note 11)
[0196] The laminated glass according to any one of Supplementary Notes 1 to 10, wherein the second glass plate in the projection assumed area has a thickness of 1.9 mm or more.
[0197] (Note 12)
[0198] The laminated glass according to any one of Supplementary Notes 1 to 11, wherein the visible light transmittance of any one of the first glass plate and the second glass plate in the projection assumed area is 87% or less.
[0199] (Note 13)
[0200] The laminated glass according to any one of Supplementary Notes 1 to 12, wherein a difference in visible light transmittance between the first glass plate and the second glass plate in the projection assumed area is 3% or more.
[0201] (Note 14)
[0202] The laminated glass according to any one of Supplementary Notes 1 to 13, wherein a difference in plate thickness between the first glass plate and the second glass plate in the projection assumed area is 0.1 mm or more.
[0203] (Note 15)
[0204] The laminated glass according to any one of Supplementary Notes 1 to 14, wherein the transmittance of the intermediate film in the projection assumed area is 90% or more.
[0205] (Note 16)
[0206] The laminated glass according to any one of Supplementary Notes 1 to 15, wherein the laminated glass has a shielding layer, and a HUD display area used in a head-up display is at a distance of 20 mm or more from an edge of the shielding layer.
[0207] This international application claims the benefit of priority based on Japanese Patent Application No. 2022-055748 filed on March 30, 2022, and the entire contents of Japanese Patent Application No. 2022-055748 are incorporated herein by reference.
[0208] Explanation of symbols
[0209] 1HUD system
[0210] 10,10A,10B laminated glass
[0211] 11 First Glass Plate
[0212] 12 Second Glass Plate
[0213] 13Intermediate film
[0214] 14 shielding layer
[0215] 15P polarized reflective film
[0216] 50 Light Sources
[0217] 60First optical system
[0218] 70 Image display element
[0219] 80 Second optical system
[0220] 90 concave mirror.
Claims
1. A laminated glass comprising a first glass plate, a second glass plate, and an intermediate film located between the first glass plate and the second glass plate and bonding the first glass plate and the second glass plate together, A projection assumption area used in a head-up display and into which P-polarized light can be incident from the first glass plate side is defined in a portion of the laminated glass, and a P-polarized light reflecting film is provided in the projection assumption area. The residual stress Δσ [MPa] in the projection assumption region satisfies the inequality obtained by combining the following equations (1), (2) and (3) with Rp, Ts and t as variables: ((1-Rp)×X×Ts 2 ×Rs) / Rp≤0.1……(1) X=sinδ……(2) Δσ=δ / 2π×λ / C / t……(3) in, When the P polarized light enters the projected assumed area of the laminated glass from the first glass plate side at an incident angle of 57 degrees, the P polarized light reflectivity of the laminated glass is Rp, the P polarized light transmittance is (1-Rp), the polarization conversion factors of the first glass plate and the second glass plate are X, the S polarized light transmittance of the laminated glass is Ts, the S polarized light reflectivity of the outer main surface of the second glass plate is Rs, the phase difference generated inside the first glass plate and the second glass plate is δ; and the circumference is π, the wavelength λ of the P polarized light is 555 [nm], the photoelastic coefficient C is 2.8 [nm / mm / Mpa], and the total thickness of the first glass plate and the second glass plate is t [mm].
2. The laminated glass according to claim 1, wherein: The residual stress Δσ is below 1 MPa.
3. The laminated glass according to claim 1 or 2, wherein: The residual stress Δσ is below 0.7 MPa.
4. The laminated glass according to claim 1 or 2, wherein: The P-polarized light reflectivity Rp is greater than or equal to 10% and less than or equal to 25%.
5. The laminated glass according to claim 1 or 2, wherein: The P-polarized light reflective film is provided on the outer main surface of the first glass plate.
6. The laminated glass according to claim 1 or 2, wherein: The S-polarized light transmittance Ts of the laminated glass when the incident angle of the laminated glass entering the projection assumed area is 57 degrees is less than or equal to 80%.
7. The laminated glass according to claim 1 or 2, wherein: The visible light transmittance of the first glass plate is greater than the visible light transmittance of the second glass plate.
8. The laminated glass according to claim 1 or 2, wherein: The total thickness of the projected assumed area is below 4.6 mm.
9. The laminated glass according to claim 1 or 2, wherein: The thickness of the first glass plate in the projection assumed area is 1.8 mm or less.
10. The laminated glass according to claim 1 or 2, wherein: The S-polarized light transmittance Ts of the laminated glass when the incident angle of the laminated glass entering the projection assumed area is 57 degrees is less than or equal to 75%.
11. The laminated glass according to claim 1 or 2, wherein: The thickness of the second glass plate in the projection assumed area is greater than or equal to 1.9 mm.
12. The laminated glass according to claim 1 or 2, wherein: The visible light transmittance of either the first glass plate or the second glass plate in the projection assumed area is 87% or less.
13. The laminated glass according to claim 1 or 2, wherein: The difference in visible light transmittance between the first glass plate and the second glass plate in the projection assumed area is greater than or equal to 3%.
14. The laminated glass according to claim 1 or 2, wherein: The difference in plate thickness between the first glass plate and the second glass plate in the projection assumed area is 0.1 mm or more.
15. The laminated glass according to claim 1 or 2, wherein: The transmittance of the intermediate film in the projection assumed area is greater than or equal to 90%.
16. The laminated glass according to claim 1 or 2, wherein: The laminated glass has a shielding layer, and a HUD display area used in a head-up display is more than 20 mm away from an edge of the shielding layer.
Citation Information
Patent Citations
Laminated glass for vehicle
CN101038349A
Array substrate and display device
CN103680328A
Head up display system
CN104267499A
Polarization optimized heads-up display
WO2021064498A1
Head-up display system
WO2021145387A1
Cited By
Head-up display glass, laminated glass, head-up display system, and vehicle
WO2026179937A1