Curable polymer, curable composition, prepreg, laminate, metal-clad laminate, and wiring substrate
By using a combination of homopolymers or copolymers with specific structural units and inorganic filler materials, the problems of high dielectric loss tangent (Df) and insufficient glass transition temperature (Tg) of wiring substrates under high frequency conditions have been solved, resulting in wiring substrate materials with low loss and high reliability.
Patent Information
- Application Number
- CN202380034243.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-04-28
- Filing Date
- 2023-04-10
- Publication Date
- 2024-11-15
AI Technical Summary
In the prior art, the curable polymers used to manufacture wiring substrates have a high dielectric loss tangent (Df) under high frequency conditions, which makes it difficult to meet the requirements of high-speed and high-capacity communication. At the same time, the glass transition temperature (Tg) is insufficient, which makes it impossible to guarantee reliability in high-temperature environments.
Curable polymers containing specific structural units (UX) are used, combined with inorganic fillers and flame retardants, and formed into prepreg blanks, metal-clad laminates and wiring substrates by thermosetting or active energy radiation curing, thereby optimizing dielectric loss and glass transition temperature.
It effectively reduces the dielectric loss tangent (Df) under high-frequency conditions and increases the glass transition temperature (Tg), making it suitable for wiring substrates in high-frequency signal transmission and high-temperature environments, reducing transmission loss and improving reliability.
Smart Images

Figure CN118974120A_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to a curable polymer, a curable composition, a prepreg, a laminate, a metal-clad laminate, and a wiring substrate. Background Art
[0002] In applications such as electrical equipment and electronic equipment, a wiring substrate (also referred to as a printed wiring board) is used. Wiring substrates can be manufactured as follows, for example. The fiber substrate is impregnated in a curable composition comprising a curable polymer and additives such as a flame retardant and an inorganic filler (also referred to as a filler) added as needed, and the curable composition is (semi) cured to make a prepreg. One or more prepregs are sandwiched between a pair of metal foils, and the first temporary laminate obtained is heated and pressurized to thereby make a metal-clad laminate. Using the metal foil located at the outermost surface of the metal-clad laminate, conductor patterns such as wiring (also referred to as circuit patterns) are formed. The metal foil on the outermost surface can be configured only on the single-sided side of the first temporary laminate.
[0003] Furthermore, one or more prepregs are laminated on the obtained wiring substrate, the obtained product is sandwiched between a pair of metal foils, the obtained second temporary laminate is heated and pressurized, and a conductor pattern such as wiring is formed using the metal foil located on the outermost surface, thereby being able to manufacture a multilayer wiring substrate (also called a multilayer printed wiring board). The outermost metal foil may be arranged only on one side of the second temporary laminate.
[0004] The heated and pressed material of the prepreg includes a fiber base material, a resin, an inorganic filler, etc., and is also called a composite base material. In a wiring board, the composite base material functions as an insulating layer.
[0005] The resin contained in the prepreg is a (semi-)cured product of the curable composition, and the resin contained in the composite base material is a cured product of the curable composition.
[0006] Prior art literature
[0007] Non-patent literature
[0008] Non-patent literature 1: Organic Synthetic Chemistry, Vol. 27, No. 9, 1969, 858-862.
[0009] Non-patent document 2: Macromolecules, Vol. 32, No. 17, 1999, 5495-5500.
[0010] Non-patent document 3: Polymer, 59, 2015, 252-259.
[0011] Non-patent document 4: Macromolecules, Vol. 32, No. 19, 1999, 6082-6087. Summary of the invention
[0012] Problems to be solved by the invention
[0013] Conventionally, as a curable polymer for use in prepregs for producing wiring boards, a polyphenylene ether (modified PPE) oligomer having polymerizable functional groups at both ends (see formula (PPE-o) described later) has been widely used.
[0014] In recent years, in applications such as mobile electronic devices, communication speeds and capacity have been increasing, and signals have been increasing in frequency. For wiring substrates used in such applications, it is required to reduce transmission loss in the high-frequency region. Transmission loss mainly includes conductor loss caused by the surface resistance of metal foil and dielectric loss tangent (D f ) caused by dielectric loss. Therefore, the resin contained in the composite substrate of the wiring substrate used in the above applications is required to reduce the dielectric loss in the high frequency region. Usually, the dielectric loss tangent (D f ) depends on the frequency. If the material is the same, the higher the frequency, the higher the dielectric loss tangent (D f ) is larger. For the resin contained in the composite matrix, the dielectric loss tangent (D f ) is preferably low.
[0015] The dielectric loss tangent (D) of the polyphenylene ether (PPE) resin as the cured product of the modified polyphenylene ether (modified PPE) oligomer at 10 GHz is f ) is about 0.002 to about 0.003.
[0016] It is expected that in the future, the communication speed and capacity will continue to develop, so it is necessary to make the dielectric loss tangent (D f ) further reduces the material.
[0017] The wiring board is sometimes used in a relatively high temperature environment. In order to ensure the reliability of the wiring board even in this case, the resin contained in the prepreg and the composite base material preferably has a sufficiently high glass transition temperature (Tg).
[0018] As related technologies of the present disclosure, Non-Patent Documents 1 to 4 can be cited.
[0019] The synthesis of a part of the curable polymer of the present disclosure is reported in Non-Patent Documents 1 to 4. However, there is no description of the use of prepregs, metal-clad laminates, and wiring boards, nor is there any description of dielectric properties.
[0020] The present disclosure is made in view of the above situation, and an object of the present disclosure is to provide a curable polymer and a curable composition comprising the curable polymer, wherein the curable polymer can obtain a dielectric loss tangent (D f ) is sufficiently low and the glass transition temperature (Tg) is sufficiently high.
[0021] Means used to solve problems
[0022] The present disclosure provides the following curable polymer, curable composition, prepreg, laminate, metal-clad laminate, and wiring board.
[0023] [1] A curable polymer, wherein the curable polymer is a homopolymer or a copolymer comprising one or more structural units (UX) represented by the following formula, and is used for producing a prepreg, a metal-clad laminate or a wiring board,
[0024]
[0025] (In the above formula, X is a single bond or an oxygen atom. The benzene ring may have a substituent other than those listed above. n is an integer greater than 0).
[0026] [2] The curable polymer according to [1], wherein the curable polymer is a copolymer comprising one or more structural units (UX) and one or more structural units (UY) derived from a monovinyl aromatic compound.
[0027] [3] The curable polymer according to [1] or [2], wherein the content of the one or more structural units (UX) is 1 mol % to 90 mol % based on 100 mol % of the total amount of all structural units.
[0028] [4] The curable polymer according to [1] or [2], wherein X is a single bond.
[0029] [5] The curable polymer according to [1] or [2], wherein n is 1 to 18.
[0030] [6] A curable composition comprising the curable polymer according to [1] or [2].
[0031] [7] The curable composition according to [6], further comprising another curable compound having one or more polymerizable functional groups.
[0032] [8] A prepreg comprising: a fiber base material; and a semi-cured product or a cured product of the curable composition according to [6].
[0033] [9] A laminate comprising: a substrate; and a curable composition layer comprising the curable composition according to [6].
[0034]
[10] A laminate comprising: a substrate; and a (semi-)cured material-containing layer comprising a semi-cured material or a cured material of the curable composition according to [6].
[0035]
[11] A metal-clad laminate comprising: a metal foil; and an insulating layer comprising a cured product of the curable composition according to [6].
[0036]
[12] A wiring substrate comprising: wiring; and an insulating layer comprising a cured product of the curable composition according to [6].
[0037] Effects of the Invention
[0038] According to the present disclosure, a curable polymer and a curable composition containing the curable polymer can be provided, wherein the curable polymer can obtain a dielectric loss tangent (D f ) is sufficiently low and the glass transition temperature (Tg) is sufficiently high. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] Figure 1 It is a schematic cross-sectional view of a metal-clad laminate according to a first embodiment of the present invention.
[0040] Figure 2 It is a schematic cross-sectional view of a metal-clad laminate according to a second embodiment of the present invention.
[0041] Figure 3 This is a schematic cross-sectional view of a wiring substrate according to one embodiment of the present invention. DETAILED DESCRIPTION
[0042] In this specification, (semi) curing is a general term for semi-curing and curing.
[0043] In this specification, unless otherwise specified, a "wiring substrate" includes a multilayer wiring substrate.
[0044] In this specification, unless otherwise specified, "polymer" includes homopolymers and copolymers.
[0045] In the present specification, unless otherwise specified, an "alkyl group having 3 or more carbon atoms" may be linear or branched.
[0046] In the present specification, unless otherwise specified, a compound having isomers includes all isomers.
[0047] In this specification, unless otherwise specified, the "weight average molecular weight (Mw)" is the weight average molecular weight calculated in terms of standard polystyrene obtained by gel permeation chromatography (GPC), and the "number average molecular weight (Mn)" is the number average molecular weight calculated in terms of polystyrene obtained by gel permeation chromatography (GPC).
[0048] In the present specification, in the chemical formula, Me represents a methyl group, Et represents an ethyl group, and Ph represents a phenyl group.
[0049] In this specification, the "high frequency region" is defined as a region with a frequency of 1 GHz or more.
[0050] In the present specification, unless otherwise specified, "to" indicating a numerical range is used to mean that the numerical values described before and after it are included as the lower limit and the upper limit.
[0051] Hereinafter, embodiments of the present invention will be described.
[0052] [Curing polymer]
[0053] The curable polymer of the present disclosure is a homopolymer or a copolymer including a structural unit (UX) represented by the following formula, and is used for producing a prepreg, a metal-clad laminate, or a wiring board.
[0054]
[0055] The above formula is also called formula (UX).
[0056] In formula (UX), X is a single bond or an oxygen atom, preferably a single bond.
[0057] n is an integer greater than or equal to 0. The benzene ring may have a substituent other than the substituent (SX) represented by the following formula.
[0058]
[0059] When the curable polymer of the present disclosure is a copolymer, the curable polymer of the present disclosure may be a copolymer including a plurality of structural units (UX) or a copolymer including one or more structural units (UX) and one or more other structural units.
[0060] From the viewpoint of increasing the glass transition temperature (Tg) of the cured product of the curable polymer of the present disclosure, the other structural unit is preferably a structural unit (UY) derived from a monovinyl aromatic compound.
[0061] The monovinyl aromatic compound is a compound having a structure in which one polymerizable vinyl group is linked to an aromatic ring. The polymerizable vinyl group may be a substituent of the aromatic ring or a vinyl group contained in a cyclopentadiene ring condensed with the aromatic ring.
[0062] For example, the following can be listed: styrene and vinylnaphthalene; methylstyrene, ethylstyrene, and tert-butylstyrene, etc., alkyl-substituted styrenes on the ring; alkyl-substituted vinylnaphthalene on the ring; other alkyl-substituted aromatic vinyl compounds on the ring; dimethylstyrene, etc., dialkyl-substituted styrenes on the ring; other dialkyl-substituted aromatic vinyl compounds on the ring; α-alkyl-substituted styrenes such as α-methylstyrene; other α-alkyl-substituted aromatic vinyl compounds; β-alkyl-substituted styrenes such as β-methylstyrene; other β-alkyl-substituted aromatic vinyl compounds; indene, acenaphthylene; their derivatives such as substitutions and modifications; etc.
[0063] When the monovinyl aromatic compound has structural isomers, any of the ortho-isomer, the meta-isomer and the para-isomer may be used.
[0064] Examples of the structural unit (UY) include structural units represented by the following formulae (UY-1) to (UY-5).
[0065]
[0066]
[0067] The inventors of the present disclosure have conducted research and found that the dielectric loss tangent (D ) of a (semi-)cured product of a curable composition under high frequency conditions can be sufficiently reduced by using the curable polymer of the present disclosure. f ).
[0068] In the curable polymer disclosed in the present invention, the content of one or more structural units (UX) is not particularly limited relative to the total amount of all structural units (100 mol %). The inventors of the present application have conducted research and found that when the conditions other than the content of the structural unit (UX) are set to be the same for comparison, when the content of the structural unit (UX) increases, the dielectric loss tangent (D) of the (semi-)cured material of the curable composition under high frequency conditions increases. f ) tends to become relatively higher.
[0069] Compared with a homopolymer or copolymer containing only one or more structural units (UX) as structural units, a copolymer containing one or more structural units (UX) and one or more other structural units (preferably structural units (UY) derived from a monovinyl aromatic compound) has the ability to more effectively reduce the dielectric loss tangent (D ) of the (semi-)cured product of the curable composition under high frequency conditions.f ) tendency.
[0070] The curable polymer of the present disclosure is preferably a copolymer comprising one or more structural units (UX) and one or more structural units (UY) derived from a monovinyl aromatic compound, because the dielectric loss tangent (Df) of the (semi-)cured product of the curable composition under high frequency conditions can be effectively reduced.
[0071] In the curable polymer of the present invention, the content of one or more structural units (UX) is preferably 1 mol% to 90 mol%, more preferably 1 mol% to 50 mol%, particularly preferably 5 mol% to 50 mol%, and most preferably 5 mol% to 25 mol%, relative to 100 mol% of the total amount of all structural units, because it can effectively reduce the dielectric loss tangent (D) of the (semi-)cured product of the curable composition under high frequency conditions. f ).
[0072] In the structural unit (UX), the substitution position of the substituent (SX) on the benzene ring may be any of the ortho, meta and para positions. From the viewpoint of the ease of synthesis of the monomer and the ease of synthesis of the curable polymer disclosed herein, the substitution position is preferably the para position.
[0073] The benzene ring in the structural unit (UX) may have other substituents other than the above-mentioned substituents (SX). Examples of other substituents that the benzene ring may have include alkyl groups and aryl groups having 1 to 18 carbon atoms, and from the viewpoint of raw material availability, methyl, ethyl, propyl, butyl, hexyl, octyl, phenyl, and tolyl are preferred. The benzene ring in the structural unit (UX) preferably has no substituents other than the above-mentioned substituents (SX).
[0074] In the structural unit (UX), n is an integer of 0 or more, preferably 1-18, more preferably 1-12, and particularly preferably 1-8.
[0075] The curable polymer disclosed herein may be either thermosetting or active energy ray curable. Active energy ray curable polymers are polymers that are cured by irradiation with active energy rays such as ultraviolet rays and electron beams. In applications such as metal-clad laminates and wiring substrates, thermosetting polymers are preferred.
[0076] The curable polymer of the present disclosure containing one or more structural units (UX) can be produced by homopolymerizing or copolymerizing one or more monomers (MX) represented by the following formula, or can be produced by copolymerizing one or more monomers (MX) represented by the following formula and one or more other monomers copolymerizable therewith (preferably one or more other monomers containing one or more monovinyl aromatic compounds).
[0077] In other words, the curable polymer of the present disclosure is: a homopolymer or copolymer of one or more monomers (MX); or a copolymer of one or more monomers (MX) and one or more other monomers copolymerizable therewith (preferably one or more other monomers including one or more monovinyl aromatic compounds).
[0078]
[0079] The above formula is also referred to as formula (MX).
[0080] In formula (MX), X is a single bond or an oxygen atom, preferably a single bond. The benzene ring may have a substituent other than the above. n is an integer greater than 0. Preferably n is the same as in formula (UX).
[0081] As the polymerization method, chain polymerization is preferred. Examples of chain polymerization include cationic polymerization, anionic polymerization, and radical polymerization, and cationic polymerization is preferred.
[0082] The monomer (MX) can be synthesized by a known method using chloroalkylstyrene such as chloromethylstyrene (CMS) as a starting material. The monomer (MX) is preferably a modified product of CMS obtained by using chloromethylstyrene (CMS) as a starting material.
[0083] The following is a first example of a reaction route for synthesizing a monomer (MX) using chloromethylstyrene (CMS) as a starting material and a reaction route for polymerization using the obtained monomer (MX). In this example, in the monomer (MX), X is a single bond, the substitution position of the substituent (SX) on the benzene ring is the para position, and n = 1. In this example, copolymerization of the obtained monomer (MX) with styrene as a monovinyl aromatic compound is shown.
[0084]
[0085] The following is a second example of a reaction route for synthesizing a monomer (MX) using chloromethylstyrene (CMS) as a starting material and a reaction route for polymerization using the obtained monomer (MX). In this example, in the monomer (MX), X is an oxygen atom, the substitution position of the substituent (SX) on the benzene ring is the para position, and n = 1. In this example, copolymerization of the obtained monomer (MX) with styrene as a monovinyl aromatic compound is shown.
[0086]
[0087] Examples of the curable polymer of the present disclosure include homopolymers represented by the following formulae (MC-11) and (MC-12).
[0088]
[0089]
[0090] In formula (MC-11) and (MC-12), m represents the number of moles of the structural unit, and m>0. m is preferably 5 to 250, and more preferably 10 to 200. It should be noted that m in these formulas has nothing to do with m in formula (MX) and (SX).
[0091] Examples of the curable polymer of the present disclosure include copolymers represented by the following formulae (MC-21) to (MC-30): The arrangement of the structural units in the copolymer may be any of an alternating arrangement, a block arrangement, and a random arrangement.
[0092]
[0093]
[0094]
[0095] In formulae (MC-21) to (MC-30), m and n represent the number of moles of each structural unit, and m>0, n>0. It should be noted that n in these formulae has nothing to do with m and n in formulae (MX) and (SX).
[0096] When the total molar number of m and n is 100 mol %, the molar fraction of m is preferably 1 mol % to 90 mol %, more preferably 5 mol % to 50 mol %, and the molar fraction of n is preferably 10 mol % to 99 mol %, more preferably 50 mol % to 95 mol %.
[0097] The molecular weight of the curable polymer disclosed herein is not particularly limited. The number average molecular weight (Mn) is preferably 1,000 to 20,000, more preferably 1,000 to 5,000. The weight average molecular weight (Mw) is preferably 2,000 to 100,000, more preferably 3,000 to 40,000.
[0098] The curable polymer of the present disclosure can have a structure not containing polar atoms in the main chain, unlike a modified polyphenylene ether (modified PPE) oligomer having polymerizable functional groups at both ends.
[0099] The curable polymer of the present disclosure may have a structure containing no polar atoms or few polar atoms. In the curable polymer of the present disclosure, it is preferred that X is a single bond and contains no polar atoms.
[0100] By using the curable polymer of the present disclosure that does not contain polar atoms or contains a small amount of polar atoms, it is possible to effectively reduce the dielectric loss tangent (D f ) of resin.
[0101] The curable polymer disclosed herein may be either thermosetting or active energy ray curable. Active energy ray curable polymers are polymers that are cured by irradiation with active energy rays such as ultraviolet rays and electron beams. In applications such as metal-clad laminates and wiring substrates, thermosetting polymers are preferred.
[0102] [Curable composition]
[0103] The curable composition of the present disclosure contains one or more curable polymers of the present disclosure.
[0104] The curable composition of the present disclosure may contain one or more other curable compounds having one or more polymerizable functional groups, as necessary.
[0105] As for the curable polymer of the present disclosure, the resin obtained when cured alone is hard and brittle, depending on the molecular structure, and is sometimes not practical for use as a prepreg, a metal-clad laminate, or a wiring substrate. In this case, by using other suitable curable compounds in combination, the brittleness of the obtained resin can be improved to a level that is practical for use as a prepreg, a metal-clad laminate, or a wiring substrate.
[0106] By using the curable polymer of the present disclosure in combination with another appropriate curable compound, the glass transition temperature (Tg) of the (semi-)cured product of the curable composition may be increased.
[0107] The curable composition of the present disclosure may further contain one or more optional components as necessary.
[0108] The curable composition of the present disclosure may be thermosetting or active energy ray-curable. In applications such as metal-clad laminates and wiring boards, thermosetting is preferred.
[0109] The other curable compound may be a monofunctional compound having one or more polymerizable functional groups, or may be a polyfunctional compound having two or more polymerizable functional groups.
[0110] Examples of the polymerizable functional group include a group having a polymerizable carbon-carbon unsaturated bond, an epoxy group, an isocyanate group, a hydroxyl group, a mercapto group, an amino group, a urea group, a carboxyl group, a sulfonic acid group, an acyl chloride group, and a chlorine atom. Examples of the group having a polymerizable carbon-carbon unsaturated bond include a vinyl group, an allyl group, a diene group, a (meth)acryloyloxy group, and a (meth)acryloylamino group.
[0111] As other curable compounds, for example, when cured alone, curable compounds that become the following resins can be listed, and the resins are polyphenylene ether resin (PPE), bismaleimide resin, epoxy resin, fluorine-containing resin, polyimide resin, olefin resin, polyester resin, polystyrene resin, hydrocarbon elastomer, benzophenone resin, Oxazine resins, active ester resins, cyanate resins, butadiene resins, hydrogenated or unhydrogenated styrene butadiene resins, vinyl resins, cycloolefin polymers, aromatic polymers, and divinyl aromatic polymers.
[0112] Examples of the form of other curable compounds include monomers, oligomers, and prepolymers.
[0113] Examples of other curable compounds include modified polyphenylene ether (modified PPE) oligomers represented by the following formula (PPE-o) and having polymerizable functional groups at both ends.
[0114]
[0115] The m and n in the formula (PPE-o) have nothing to do with the m and n in the formulas (MX), (SX), (MC-11), (MC-12), (MC-21) to (MC-30).
[0116] The X at both ends of the formula (PPE-o) are each independently a group represented by the following formula (x1) or the following formula (x2). In these formulas, “ ” indicates a bond to an oxygen atom.
[0117]
[0118] In the formula (PPE-o), m is preferably 1-20, more preferably 3-15, and n is preferably 1-20, more preferably 3-15.
[0119] The number average molecular weight (Mn) of the modified polyphenylene ether (modified PPE) oligomer is not particularly limited, but is preferably 1,000 to 5,000, and more preferably 1,000 to 4,000.
[0120] When the curable polymer of the present invention is used in combination with other curable compounds containing polar atoms in the main chain such as modified polyphenylene ether (modified PPE) oligomers as curable compounds, the amount of polar atoms contained in the (semi-)cured product of the curable composition can be reduced compared to the case where only the curable compound containing a large number of polar atoms such as modified PPE oligomers is used as the curable compound. As a result, the dielectric loss tangent (D f ).
[0121] In the curable composition of the present invention, the content of the one or more curable polymers of the present invention is preferably as large as possible relative to 100 parts by mass of the total amount of the one or more curable polymers of the present invention and the one or more other curable compounds, preferably 20 to 100 parts by mass, more preferably 30 to 100 parts by mass, particularly preferably 50 to 100 parts by mass, and most preferably 70 to 100 parts by mass, because the dielectric loss tangent (Df) of the (semi-)cured product of the curable composition under high frequency conditions can be effectively reduced.
[0122] The curable composition preferably contains one or more polymerization initiators. As the polymerization initiator, organic peroxides, azo compounds, other known polymerization initiators, and combinations thereof can be used. Specific examples include dicumyl peroxide, benzoyl peroxide, cumene hydroperoxide, 2,5-dimethylhexane-2,5-dihydroperoxide, 2,5-dimethyl-2,5-di(tert-butylperoxy)-3-hexyne, di-tert-butyl peroxide, tert-butyl cumene peroxide, α,α'-di(tert-butylperoxy)diisopropylbenzene, 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane, di-tert-butyl peroxyisophthalate, tert-butyl peroxybenzoate, 2,2-bis(tert-butylperoxy)butane, 2,2-bis(tert-butylperoxy)octane, 2,5-dimethyl-2,5-di(benzoylperoxide)hexane, bis(trimethylsilyl)peroxide, trimethylsilyltriphenylsilylperoxide, and azobisisobutyronitrile.
[0123] The curable composition may contain one or more additives as necessary. Examples of the additives include inorganic fillers (also referred to as fillers), compatibilizers, and flame retardants.
[0124] As inorganic fillers, for example, there can be listed: silicon dioxide such as spherical silica, metal oxides such as aluminum oxide, titanium oxide and mica; metal hydroxides such as aluminum hydroxide and magnesium hydroxide; talc; aluminum borate; barium sulfate; calcium carbonate, etc. More than one of these can be used. Among them, from the viewpoint of low thermal expansion, silicon dioxide, mica and talc are preferred, and spherical silica is more preferred.
[0125] The inorganic filler material may be a material surface-treated with a silane coupling agent of epoxy silane type, vinyl silane type, methacrylic silane type, or amino silane type. The timing of the surface treatment with the silane coupling agent is not particularly limited. The inorganic filler material surface-treated with the silane coupling agent may be prepared in advance, or the silane coupling agent may be added by an overall blending method when preparing the curable composition.
[0126] As flame retardants, for example, halogen flame retardants and phosphorus-containing flame retardants can be listed. More than one of these can be used. As halogen flame retardants, for example, bromine-containing flame retardants such as pentabromodiphenyl ether, octabromodiphenyl ether, decabromodiphenyl ether, tetrabromobisphenol A and hexabromocyclododecane can be listed; chlorine-containing flame retardants such as chlorinated paraffin can be listed. As phosphorus-containing flame retardants, for example, phosphate esters such as condensed phosphate esters and cyclic phosphate esters; phosphazene compounds such as cyclic phosphazene compounds; phosphinate flame retardants such as dialkylphosphinate aluminum salts; melamine flame retardants such as melamine phosphate and polyphosphate melamine; phosphine oxide compounds having a diphenylphosphine oxide group can be listed.
[0127] The curable composition may contain one or more organic solvents as required. The organic solvent is not particularly limited, and examples thereof include ketones such as methyl ethyl ketone; ethers such as dibutyl ether; esters such as ethyl acetate; amides such as dimethylformamide; aromatic hydrocarbons such as benzene, toluene and xylene; and chlorinated hydrocarbons such as trichloroethylene.
[0128] In the curable composition, the compounding composition and the solid content concentration can be appropriately designed.
[0129] The compounding composition of the curable composition can be designed so that the obtained (semi-)cured product does not become brittle and the properties such as dielectric loss tangent (Df) and glass transition temperature (Tg) of the obtained (semi-)cured product become appropriate.
[0130] In applications such as prepregs, the solid content concentration of the curable composition can be designed so that the fiber base material can be easily impregnated therein, and is preferably 50% by mass to 90% by mass.
[0131] [Prepreg]
[0132] The prepreg of the present disclosure comprises: a fiber base material; and a (semi-)cured product of the curable composition of the present disclosure.
[0133] The prepreg can be produced by impregnating a fiber base material with a curable composition and (semi-)curing the composition by thermal curing or the like.
[0134] The (semi)cured material may include: a single cured product of one curable polymer of the present disclosure; a reaction product of a plurality of curable polymers of the present disclosure; or a reaction product of one or more curable polymers of the present disclosure and one or more other curable compounds.
[0135] The (semi)cured material may contain additives such as an inorganic filler (filler) as necessary.
[0136] The material of the fiber substrate is not particularly limited, and examples thereof include inorganic fibers such as glass fiber, silica fiber, and carbon fiber; organic fibers such as aramid fiber and polyester fiber; and combinations thereof. In applications such as metal-clad laminates and wiring substrates, glass fiber is preferred. Examples of the form of the glass fiber substrate include glass cloth, glass paper, and glass mat.
[0137] The curing conditions of the curable composition can be set according to the composition of the curable composition, and are preferably semi-curing conditions (incomplete curing conditions).
[0138] For example, thermal curing by heating at 80°C to 180°C for 1 minute to 10 minutes is preferred.
[0139] In applications such as metal-clad laminates and wiring boards, it is preferred to adjust the composition of the curable composition and the curing conditions so that the resin content in the obtained prepreg is within a range of 40% by mass to 80% by mass.
[0140] [Laminated body]
[0141] The first laminate of the present disclosure includes: a substrate; and a curable composition layer including the curable composition of the present disclosure described above.
[0142] The second laminate of the present disclosure includes: a substrate; and a (semi-)cured material-containing layer including a (semi-)cured material of the curable composition of the present disclosure described above.
[0143] In the laminate of the present disclosure, the substrate is not particularly limited, and examples thereof include resin films, metal foils, and combinations thereof.
[0144] The (semi-)cured material-containing layer may be a layer containing a fiber base material and a (semi-)cured material of the curable composition of the present disclosure.
[0145] The resin film is not particularly limited, and a known resin film can be used. Examples of the constituent resin of the resin film include polyimide, polyethylene terephthalate (PET), polyethylene naphthalate, cycloolefin polymer, and polyether sulfone.
[0146] As the metal foil, copper foil, silver foil, gold foil, aluminum foil, and combinations thereof are preferred, and copper foil is more preferred because of low electrical resistance.
[0147] [Metal-clad laminate]
[0148] The metal-clad laminate of the present disclosure includes: a metal foil; and an insulating layer including a cured product of the curable composition of the present disclosure.
[0149] The insulating layer may be a layer including a fiber base material and a cured product of the curable composition of the present disclosure.
[0150] As the metal foil, copper foil, silver foil, gold foil, aluminum foil and combinations thereof are preferred, and copper foil is more preferred because of its low resistance. The metal foil may have a metal plating layer on the surface. The metal foil may also be a metal foil with a carrier including an ultra-thin metal foil and a carrier metal foil supporting the ultra-thin metal foil. The metal foil may be a metal foil subjected to surface treatment such as rust prevention treatment, silane treatment, surface roughening treatment and barrier formation treatment on at least one surface.
[0151] The thickness of the metal foil is not particularly limited, but is preferably 0.1 μm to 100 μm, more preferably 0.2 μm to 50 μm, and particularly preferably 1.0 μm to 40 μm in order to suitably form a conductor pattern such as wiring (also referred to as a circuit pattern).
[0152] The metal-clad laminate may be a single-sided metal-clad laminate having a metal foil on one side or a double-sided metal-clad laminate having a metal foil on both sides, but is preferably a double-sided metal-clad laminate.
[0153] The single-sided metal-clad laminate can be produced by stacking one or more of the above-mentioned prepregs and a metal foil and heating and pressurizing the obtained first temporary laminate.
[0154] The double-sided metal-clad laminate can be produced by sandwiching one or more of the above-mentioned prepregs between a pair of metal foils and heating and pressurizing the obtained first temporary laminate.
[0155] A metal-clad laminate using copper foil as the metal foil is called a copper-clad laminate (Copper Clad Laminate: CCL).
[0156] The insulating layer preferably comprises a heated and pressed product of a prepreg. The heated and pressed product of a prepreg comprises a fiber base material and a resin, and may contain one or more additives such as an inorganic filler and a flame retardant as required. The heated and pressed product of a prepreg is also called a composite base material.
[0157] The heating and pressurizing conditions of the first temporary laminate are not particularly limited, but are preferably, for example, a temperature of 170° C. to 250° C., a pressure of 0.3 MPa to 30 MPa, and a time of 3 minutes to 240 minutes.
[0158] Figure 1 and Figure 2 A schematic cross-sectional view showing a metal-clad laminate according to an embodiment of the present invention.
[0159] Figure 1 The metal-clad laminate 1 shown is a single-sided metal-clad laminate (laminate) comprising a heated and pressed product of a prepreg, and a composite substrate (layer containing a cured product) 11 comprising a cured product of the curable composition disclosed herein, on which a metal foil (metal layer) 12 is laminated on one side.
[0160] Figure 2 The metal-clad laminate 2 shown is a double-sided metal-clad laminate comprising a prepreg heated and pressed product, and metal foils (metal layers) 12 are laminated on both sides of a composite substrate (layer containing a cured product) 11 comprising a cured product of the curable composition of the present disclosure.
[0161] The metal-clad laminated plates 1 and 2 may have layers other than those described above.
[0162] The metal-clad laminates 1 and 2 may have an adhesive layer between the composite substrate (layer containing a cured product) 11 and the metal foil (metal layer) 12 to improve their adhesion. As the material of the adhesive layer, known materials can be used, and examples thereof include epoxy resins, cyanate resins, acrylic resins, polyimide resins, maleimide resins, adhesive fluorine-containing resins, and combinations thereof. As commercially available adhesive fluorine-containing resins, examples thereof include "Fluon LM-ETFE LH-8000", "AH-5000", "AH-2000", and "EA-2000" manufactured by AGC Corporation.
[0163] The thickness of the composite substrate can be appropriately designed according to the application. From the viewpoint of preventing disconnection of the wiring substrate, it is preferably 50 μm or more, more preferably 70 μm or more, and particularly preferably 100 μm or more. From the viewpoint of flexibility, miniaturization and lightness of the wiring substrate, it is preferably 300 μm or less, more preferably 250 μm or less, and particularly preferably 200 μm or less.
[0164] [Wiring board]
[0165] The wiring substrate of the present disclosure includes: wiring; and an insulating layer including a cured product of the curable composition of the present disclosure.
[0166] The wiring substrate can be manufactured by forming a conductor pattern (circuit pattern) such as wiring using a metal foil located on the outermost surface of the metal-clad laminate of the present invention. As a method for forming a conductor pattern such as wiring, there can be cited a subtractive method of etching a metal foil to form wiring, and an MSAP (modified semi-additive method) method of forming wiring on a metal foil by plating.
[0167] Figure 3 A schematic cross-sectional view showing a wiring substrate according to an embodiment of the present invention. Figure 3 The wiring substrate 3 shown is used Figure 2 The wiring board shown is obtained by forming a conductor pattern (circuit pattern) 22 such as wiring 22W on the metal foil 12 located on at least one outermost surface of the metal-clad laminate 2 of the second embodiment.
[0168] Wiring board 3 comprises a heated and pressed prepreg, and conductor patterns (circuit patterns) 22 such as wiring 22W are formed on at least one surface of composite base material (layer containing a cured product, insulating layer) 11 comprising a cured product of the curable composition of the present disclosure.
[0169] The obtained wiring substrate may be further laminated with one or more prepregs, the obtained product may be sandwiched between a pair of metal foils, the obtained second temporary laminate may be heated and pressurized, and the metal foil on the outermost surface may be used to form a conductor pattern such as wiring, thereby manufacturing a multilayer wiring substrate (also referred to as a multilayer printed wiring board). The metal foil on the outermost surface may be arranged only on one side of the second temporary laminate.
[0170] The wiring substrate of the present disclosure is suitable for use in a high-frequency region (a region with a frequency of 1 GHz or more).
[0171] In recent years, in applications such as mobile electronic devices, communication speeds and capacity have been increasing, and signals have been becoming more and more high-frequency. For wiring substrates used in such applications, it is required to reduce transmission loss in the high-frequency region. Therefore, for the resin contained in the composite base material of the wiring substrate used in the above applications, it is required to reduce dielectric loss in the high-frequency region. Usually, the dielectric loss tangent (D f ) depends on the frequency. If the material is the same, the higher the frequency, the higher the dielectric loss tangent (D f ) is larger. For the resin contained in the composite matrix, the dielectric loss tangent (D f ) is preferably low.
[0172] The wiring board is sometimes used in a relatively high temperature environment. In order to ensure the reliability of the wiring board even in this case, the resin contained in the prepreg and the composite base material preferably has a sufficiently high glass transition temperature (Tg).
[0173] When the difference between the coefficient of thermal expansion (CTE) of the prepreg or composite substrate and the metal foil is large, when the first temporary laminate comprising the prepreg and the metal foil, or the second temporary laminate comprising the composite substrate, the prepreg and the metal foil is heated and pressurized, there is a concern that the metal foil may be dislocated or peeled off. The smaller the difference between the coefficient of thermal expansion (CTE) of the prepreg or composite substrate and the metal foil, the more preferred. Usually, the coefficient of thermal expansion (CTE) of the resin is greater than that of the metal foil, so the smaller the coefficient of thermal expansion (CTE) of the prepreg and the composite substrate, the more preferred.
[0174] The inventors of the present application have conducted studies and found that the dielectric loss tangent (Df) of a (semi-)cured product of a curable composition under high frequency conditions can be sufficiently reduced by using the curable polymer of the present disclosure that contains no polar atoms or contains few polar atoms.
[0175] It was also found that the glass transition temperature (Tg) of the (semi-)cured product of the curable composition containing the curable polymer of the present disclosure was sufficiently high.
[0176] It was also found that the coefficient of thermal expansion (CTE) of the (semi-)cured product of the curable composition containing the curable polymer of the present disclosure was sufficiently low.
[0177] Furthermore, it was found that the (semi-)cured product of the curable composition containing the curable polymer of the present disclosure has good adhesion to metals such as copper foil in practical use.
[0178] By using the curable polymer disclosed in the present invention, the dielectric loss tangent (D f ) is sufficiently low and the glass transition temperature (Tg) is sufficiently high. The (semi-)cured product is suitable for use as a composite substrate and insulating layer suitable for wiring substrates used in high-frequency regions.
[0179] The dielectric loss tangent (D) of the (semi-)cured product of the curable composition disclosed herein and the composite substrate comprising the (semi-)cured product of the curable composition under high frequency conditions is f ) For example, it is preferably within the following range.
[0180] Dielectric loss tangent (D) at a frequency of 10 GHz f ) is preferably less than 0.010, more preferably less than 0.005, further preferably less than 0.003, particularly preferably less than 0.002, and most preferably less than 0.002.
[0181] Dielectric loss tangent (D) at a frequency of 10 GHz f ) can be less than 0.0019, less than 0.0017, or less than 0.0014.
[0182] Dielectric loss tangent (D) at a frequency of 10 GHz f ) is not particularly limited, and is, for example, 0.0001.
[0183] The glass transition temperature (Tg) of the (semi-)cured material of the curable composition of the present disclosure is preferably 150°C or higher, more preferably 180°C or higher, and particularly preferably 200°C or higher. The upper limit is not particularly limited, and is, for example, 300°C.
[0184] The coefficient of thermal expansion (CTE) of the (semi-)cured product of the curable composition disclosed herein and the composite substrate including the (semi-)cured product of the curable composition is preferably within the following range, for example.
[0185] The smaller the coefficient of thermal expansion (CTE), the better, preferably 70 ppm / °C or less, more preferably 60 ppm / °C or less, particularly preferably 50 ppm / °C or less, and most preferably 40 ppm / °C or less. The lower limit is not particularly limited, and is, for example, 1 ppm / °C.
[0186] Dielectric loss tangent (D f ) and the glass transition temperature (Tg) can be measured by the method described in the section [Examples] described later.
[0187] The coefficient of thermal expansion (CTE) can be measured by a known method using a commercially available thermomechanical analyzer.
[0188] As described above, according to the present disclosure, a curable polymer and a curable composition containing the curable polymer can be provided, wherein the curable polymer can obtain a dielectric loss tangent (D f ) is sufficiently low and the glass transition temperature (Tg) is sufficiently high.
[0189] The curable polymer and the curable composition containing the same disclosed in the present invention are suitable for applications such as prepregs, metal-clad laminates, and wiring boards, but can be used for any applications.
[0190] [use]
[0191] The curable polymer disclosed herein and the curable composition comprising the same are suitable for use in prepregs, metal-clad laminates, wiring boards, and the like.
[0192] The curable composition containing the curable polymer of the present disclosure is suitable as a curable composition used in applications such as prepregs, metal-clad laminates, and wiring boards.
[0193] The metal-clad laminate of the present disclosure is suitable for a wiring board or the like used in various electric devices, various electronic devices, and the like.
[0194] The wiring substrate disclosed herein is suitable for mobile electronic devices such as mobile phones, smart phones, mobile information terminals and laptop computers; antennas for mobile phone base stations and automobiles, etc.; electronic devices such as servers, routers and baseboards; wireless infrastructure; radars for collision avoidance, etc.; various sensors (for example, automotive sensors such as engine management sensors), etc.
[0195] The wiring substrate disclosed herein is particularly suitable for applications that use high-frequency signals for communication and is suitable for various applications that require reduction in transmission loss in a high-frequency region.
[0196] Example
[0197] The present invention is specifically described below with reference to examples, but the present invention is not limited thereto. Examples 11 to 13, 21, 31, 41, 51, 101 to 107, and 301 are examples, and Example 201 is a comparative example. Unless otherwise specified, the room temperature is about 25°C.
[0198] [Commercially available reagents]
[0199] In the section [Examples], commercially available catalysts and reagents were used for the reaction as they were unless otherwise specified. Commercially available solvents that had been dehydrated and deoxygenated were used.
[0200] [Evaluation Items and Evaluation Methods of Curable Polymers]
[0201] (Structure of a monomer)
[0202] Using a nuclear magnetic resonance apparatus ("AVANCE NEO400" manufactured by Bruker), 1 The structure of the synthesized monomer was identified by H-NMR measurement.
[0203] (Number average molecular weight (Mn) and weight average molecular weight (Mw))
[0204] The number average molecular weight (Mn) and weight average molecular weight (Mw) of the synthesized curable polymer were obtained by gel permeation chromatography (GPC). As a GPC device, "HLC-8320GPC" manufactured by Tosoh Corporation with a differential refractive index detector (RI detector) was used. As an eluent, tetrahydrofuran was used. As a chromatographic column, a chromatographic column obtained by connecting four columns of "TSKgel SuperHZ2000", "TSKgel SuperHZ2500", "TSKgel SuperHZ3000" and "TSKgel SuperHZ4000" (all manufactured by Tosoh Corporation) in series was used. 20 mg of resin was dissolved in 2 mL of tetrahydrofuran to prepare a sample solution. 10 μl of the sample solution was injected and the chromatogram was measured. GPC was measured using 10 standard polystyrenes with a molecular weight range of 400 to 5000000, and a standard curve representing the relationship between retention time and molecular weight was prepared. Based on the standard curve, the Mn and Mw of the curable polymer were determined.
[0205] [Evaluation Items and Evaluation Methods for Film-like Cured Products]
[0206] (Relative dielectric constant (D k ) and dielectric loss tangent (D f ))
[0207] The relative dielectric constant (D) of the evaluation sample (film-like cured product) at 10 GHz was measured by the SPDR method using a vector network analyzer (E8361C manufactured by Agilent Technologies) at room temperature. k ) and dielectric loss tangent (D f ) for determination.
[0208] (Glass transition temperature Tg)
[0209] The dynamic viscoelasticity measurement (DMA) of the evaluation sample (film-like cured product) was performed using a dynamic viscoelasticity measuring device ("DVA-200" manufactured by IT Keisoku Seigyo Co., Ltd.), and the glass transition temperature (Tg) (°C) was measured. The measurement was performed under the conditions of a frequency of 10 Hz, a heating rate of 2°C / min, and a temperature range of 25°C to 300°C.
[0210] [Synthesis Example 1] Synthesis of p-(3-butenyl)styrene
[0211] Under nitrogen atmosphere, an ether solution of allyl magnesium bromide (about 0.7 mol / L, 202 mL, 141 mmoles) was added to a 500 mL four-necked flask. The flask was cooled to 0 ° C, and a solution of 4-(chloromethyl) styrene (15.5 mL, 98.7 mmoles) in ether (35.1 mL) was added to the solution for 16 minutes, the flask was heated to room temperature, and stirred for 2.5 hours. The flask was cooled to 0 ° C, saturated aqueous ammonium chloride solution (140 mL) was added to the reaction mixture and stirred, and the organic phase was separated. Ether (100 mL) was further added to the aqueous phase, and the organic phase was separated twice. The organic phases obtained by extraction were combined, dried using sodium sulfate, and filtered, and the filtrate was concentrated under vacuum to obtain a crude product. The crude product was purified by silica gel column chromatography (mobile phase: n-hexane) to obtain 15.9 g of colorless liquid p-(3-butenyl)styrene (yield: 100%). The obtained compound was one of the monomers (MX) (X=single bond, n=1).
[0212] The reaction scheme and NMR analysis results are shown below.
[0213]
[0214] 1H-NMR (CDCl3): δ (ppm) 7.33 (d, 2H, J=8.11Hz, Ar-H), 7.14 (d, 2H, J=8.11Hz, Ar- H), 6.69 (dd, 2H, J=10.85, 17.52Hz), 5.90-5.80 (dm, 1H, J=10.13Hz), 5.70 (dd, 1H, J=0.95, 17.52Hz), 5.19 (dd, 1H, J=0.95, 10.85Hz), 5.04 (ddt, 1H, J=1.67, 3 .58, 17.17Hz), 4.99 (dm, 1H, J=10.25Hz), 2.70 (t, 2H, J=8.11Hz), 2.36 (m, 2H).
[0215] [Synthesis Example 2] Synthesis of Allyl (4-vinylbenzyl) Ether
[0216] Under nitrogen atmosphere, potassium tert-butoxide (11.7g, 103 mmoles), tetrahydrofuran (167mL) and allyl alcohol (7.00mL, 103 mmoles) were put into a 300mL four-necked bottle. At room temperature, 4-(chloromethyl)styrene (18.1mL, 115 mmoles) was added dropwise to the suspension for 8 minutes, the flask was heated to 50°C, and stirred for 1 hour. Ion exchange water (140mL) was added to the reaction mixture and stirred, and the organic phase was extracted. Ethyl acetate (140mL) was further added to the aqueous phase, and the organic phase was extracted. The organic phases obtained by extraction were combined, dried using sodium sulfate, and filtered, and the filtrate was concentrated under vacuum to obtain a crude product. The crude product was purified using silica gel column chromatography (mobile phase: n-hexane), thereby obtaining 17.1g of allyl (4-vinyl benzyl) ether (yield: 96%) of a light yellow liquid. The obtained compound is one of the monomers (MX) (X=oxygen atom, n=1).
[0217] The reaction scheme and NMR analysis results are shown below.
[0218]
[0219] 1H-NMR (CDCl3): δ (ppm) 7.39 (d, 2H, J=8.11Hz, Ar-H), 7.30 (d, 2H, J=8.11Hz, Ar -H), 6.71 (dd, 1H, J=6.68, 10.85Hz), 5.95 (ddt, 1H, J=4.11, 9.50, 18.68Hz), 5. 74 (dd, 1H, J=0.83, 17.64Hz), 5.30 (dq, 1H, J=1.67, 17.29Hz), 5.23 (dd, 1H, J=0 .83, 10.97Hz), 5.22-5.19 (m, 1H), 4.51 (s, 2H), 4.02 (dt, 2H, J=1.43, 5.60Hz).
[0220] [Example 11] Synthesis of copolymer (P11)
[0221] Under a nitrogen atmosphere, p-(3-butenyl)styrene (8.0 g, 50.6 mmol), styrene (12.0 g, 115.4 mmol), toluene (20 g, 21.7 mmol) and boron trifluoride ether complex (0.36 g, 2.6 mmol) obtained in Synthesis Example 1 were added to a 100 mL pressure-resistant reaction vessel and reacted for 5 hours at 50 ° C. After the reaction was completed, a saturated aqueous sodium bicarbonate solution was added to the polymerization solution to stop the reaction. The polymerization solution was added dropwise to a large amount of methanol to precipitate the polymer. The precipitate was recovered, washed and dried, thereby obtaining 18.9 g of a copolymer (P11) (yield: 94.7%).
[0222] [Example 12] Synthesis of copolymer (P12)
[0223] 18.9 g of a copolymer (P12) was obtained in the same manner as in Example 11 except that the amount of p-(3-butenyl)styrene was changed to 6.0 g, 38.0 mmol, and the amount of styrene was changed to 14.0 g, 134.6 mmol (yield: 94.4%).
[0224] [Example 13] Synthesis of copolymer (P13)
[0225] 18.2 g of a copolymer (P13) was obtained in the same manner as in Example 11 except that the amount of p-(3-butenyl)styrene was changed to 3.0 g and 19.0 mmol and the amount of styrene was changed to 17.0 g and 163.5 mmol (yield: 90.8%).
[0226] The reaction schemes of Examples 11 to 13 are shown below.
[0227]
[0228] [Example 21] Synthesis of copolymer (P21)
[0229] Under nitrogen atmosphere, p-(3-butene)styrene (4.0 g, 25.3 mmol), 4-tert-butylstyrene (16.0 g, 99.8 mmol), toluene (20 g, 21.7 mmol) and boron trifluoride ether complex (0.36 g, 2.6 mmol) were added to a 100 mL pressure-resistant reaction vessel and reacted for 5 hours at 50 ° C. After the reaction was completed, a saturated sodium bicarbonate aqueous solution was added to the polymerization solution to stop the reaction. The polymerization solution was added dropwise to a large amount of methanol to precipitate the polymer. The precipitate was recovered, washed and dried, thereby obtaining 18.9 g of a copolymer (P21 (yield: 94.7%).
[0230] The reaction scheme is shown below.
[0231]
[0232] [Example 31] Synthesis of copolymer (P31)
[0233] Under nitrogen atmosphere, p-(3-butenyl)styrene (3.0 g, 19.0 mmol), indene (8.4 g, 53.2 mmol), toluene (20 g, 21.7 mmol) and boron trifluoride ether complex (0.36 g, 2.6 mmol) were added to a 100 mL pressure-resistant reaction vessel and reacted for 5 hours at 50 ° C. After the reaction was completed, a saturated sodium bicarbonate aqueous solution was added to the polymerization solution to stop the reaction. The polymerization solution was added dropwise to a large amount of methanol to precipitate the polymer. The precipitate was recovered, washed and dried, thereby obtaining 19.1 g of a copolymer (P31) (yield: 95.3%).
[0234] The reaction scheme is shown below.
[0235]
[0236] [Example 41] Synthesis of copolymer (P41)
[0237] Under nitrogen atmosphere, p-(3-butenyl)styrene (4.2 g, 26.6 mmol), 2-vinylnaphthalene (15.8 g, 102.5 mmol), toluene (20 g, 21.7 mmol) and boron trifluoride ether complex (0.36 g, 2.6 mmol) were added to a 100 mL pressure-resistant reaction vessel and reacted for 5 hours at 50 ° C. After the reaction was completed, a saturated sodium bicarbonate aqueous solution was added to the polymerization solution to stop the reaction. The polymerization solution was added dropwise to a large amount of methanol to precipitate the polymer. The precipitate was recovered, washed and dried, thereby obtaining 18.8 g of a copolymer (P41) (yield: 93.9%).
[0238] The reaction scheme is shown below.
[0239]
[0240] [Example 51] Synthesis of copolymer (P51)
[0241] Under nitrogen atmosphere, allyl (4-vinyl benzyl) ether (3.2 g, 18.4 mmol), styrene (16.8 g, 161.5 mmol), toluene (20 g, 21.7 mmol) and boron trifluoride ether complex (0.36 g, 2.6 mmol) obtained in Synthesis Example 2 were added to a 100 mL pressure-resistant reaction vessel, and reacted at 50 ° C for 5 hours. After the reaction was completed, a saturated sodium bicarbonate aqueous solution was added to the polymerization solution to stop the reaction. The polymerization solution was added dropwise to a large amount of methanol to precipitate the polymer. The precipitate was recovered, washed and dried, thereby obtaining 19.9 g of a copolymer (P41) (yield: 99.5%).
[0242] The reaction scheme is shown below.
[0243]
[0244] In Examples 11 to 13, 21, 31, 41, and 51, the monomer compositions and the physical properties of the obtained copolymers are shown in Table 1.
[0245]
[0246] [Example 101]
[0247] A curable polymer (P11), the following modified polyphenylene ether (PPE) oligomer (SA9000), dicumyl peroxide (DCP) as a radical polymerization initiator, and toluene were mixed at a mass ratio of 50:50:1:100 and stirred at room temperature to prepare a curable composition.
[0248] (SA9000) A difunctional methacrylic acid-modified PPE oligomer represented by the following formula ("SA9000" manufactured by SABIC Corporation).
[0249]
[0250] Next, the curable composition was applied onto a polyimide film having a thickness of 125 μm using an applicator (manufactured by YOSHIMITSU SEIKI CO., LTD.) to form a coating film having a thickness of 250 μm.
[0251] The coating film was heat-dried in an oven at 80° C. for 30 minutes in an air atmosphere, and then heated at 200° C. for 2 hours in a nitrogen atmosphere to thermally cure the coating film, thereby obtaining a film-like cured product with a thickness of about 100 μm.
[0252] The compounding composition of the curable composition excluding the solvent and the evaluation results of the obtained film-like cured product are shown in Table 2. The unit of the compounding amount in the table is "parts by mass".
[0253] [Examples 102~107, 201]
[0254] Except for changing the type and amount of one or more curable polymers, the same operation as in Example 101 was carried out to prepare a curable composition and produce a film-like cured product. The composition of the curable composition excluding the solvent and the evaluation results of the obtained film-like cured product are shown in Table 2.
[0255]
[0256] [Results Summary]
[0257] In Examples 101 to 106, a film-like cured product was obtained by using a curable polymer which is a copolymer including a structural unit (UX) not containing a polar atom and a structural unit (UY) derived from a monovinyl aromatic compound.
[0258] In Example 107, a film-like cured product was obtained using a curable polymer which was a copolymer including a structural unit (UX) containing a polar atom and a structural unit (UY) derived from a monovinyl aromatic compound.
[0259] In Example 201, a film-like cured product was obtained by using only a modified PPE oligomer not containing the structural unit (UX).
[0260] As for Examples 101 to 106, compared with Example 201, the dielectric loss tangent (D f In these examples, it is possible to obtain a dielectric loss tangent (Df ), and a film-like cured product having a sufficiently high glass transition temperature (Tg).
[0261] In Example 107, the dielectric loss tangent (D f ) is at the same level as Example 201, which is a practical level. In this example, the dielectric loss tangent (D f ) is sufficiently low and the glass transition temperature (Tg) is sufficiently high.
[0262] [Example 301]
[0263] The curable polymer (P11) synthesized in Example 1, the above-mentioned modified polyphenylene ether (PPE) oligomer (SA9000), diisopropylbenzene peroxide (DCP) as a free radical polymerization initiator, spherical silica as an inorganic filler, and toluene are mixed in a mass ratio of 50:50:1:100:100, and stirred at room temperature to prepare a curable polymer composition (varnish).
[0264] A glass cloth (E glass, #2116) as a fiber substrate was immersed in the obtained curable polymer composition (varnish), and then heated at 130°C for 5 minutes to semi-cure the curable polymer composition, thereby obtaining a prepreg.
[0265] Two of the obtained prepregs were stacked and sandwiched between a pair of copper foils, and the obtained temporary laminate was heated and pressed under the conditions of 200° C., 1.5 hours, and 3 MPa, thereby producing a metal-clad laminate.
[0266] The present invention is not limited to the above-described embodiments and examples, and design changes may be appropriately made without departing from the spirit and scope of the present invention.
[0267] This application claims the benefit of priority based on Japanese patent application No. 2022-074083, filed on April 28, 2022, the disclosure of which is incorporated herein in its entirety.
[0268] Description of symbols
[0269] 1, 2: metal-clad laminate, 3: wiring board, 11: composite base material, 12: metal foil, 22: conductor pattern (circuit pattern), 22W: wiring.
Claims
1. A curable polymer, wherein The curable polymer is a homopolymer or copolymer containing one or more structural units (UX) represented by the following formula, and is used for manufacturing a prepreg, a metal-clad laminate or a wiring substrate, (In the above formula, X is a single bond or an oxygen atom; the benzene ring may have a substituent other than those listed above; and n is an integer greater than 0).
2. The curable polymer according to claim 1, wherein The curable polymer is a copolymer including one or more structural units (UX) and one or more structural units (UY) derived from a monovinyl aromatic compound.
3. The curable polymer according to claim 1 or 2, wherein The content of one or more structural units (UX) is 1 mol % to 90 mol % relative to 100 mol % of the total amount of all structural units.
4. The curable polymer according to claim 1 or 2, wherein X is a single bond.
5. The curable polymer according to claim 1 or 2, wherein n is 1 to 18.
6. A curable composition, wherein: The curable composition comprises the curable polymer according to claim 1 or 2.
7. The curable composition according to claim 6, wherein The curable composition further includes another curable compound having one or more polymerizable functional groups.
8. A prepreg blank, wherein: The prepreg comprises: a fiber base material; and a semi-cured product or a cured product of the curable composition according to claim 6.
9. A laminate, wherein: The laminate comprises: a substrate; and a curable composition layer comprising the curable composition according to claim 6 .
10. A laminated body, wherein: The laminate comprises: a substrate; and a (semi)cured material-containing layer comprising a semi-cured material or a cured material of the curable composition according to claim 6 .
11. A metal-clad laminate, wherein: The metal-clad laminate comprises: a metal foil; and an insulating layer comprising a cured product of the curable composition according to claim 6 .
12. A wiring substrate, wherein: The wiring substrate includes: wiring; and an insulating layer including a cured product of the curable composition according to claim 6 .