Polyester resin composition for film containing titanium-

By using a combination of titanium chelate catalyst and phosphorus compound in polyester resin, the electrostatic application and transparency problems in the preparation of films of polyester resin are solved, and the environmental pollution and scarcity of the catalyst are reduced, thus achieving high Film preparation of polymerization and thermal stability.

CN118974140APending Publication Date: 2024-11-15TORAY ADVANCED MATERIALS KOREA INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380020574.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-02-07
Filing Date
2023-01-11
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

When preparing films, existing polyester resins have problems such as low electrostatic application, uneven thickness, reduced transparency, and environmental pollution and scarcity during catalyst use, especially the toxicity and scarcity of antimony and germanium compounds catalysts. Titanium system Catalysts may cause polyester coloring and unstable melt thermal stability.

Method used

The composition containing polyester resin, titanium chelate catalyst, fixative and phosphorus compound is used to satisfy the specific content relationship and chemical formula, and the reaction product of titanium alkoxide and α-hydroxycarboxylic acid is used as the catalyst, and the Adjust the titanium, phosphorus and magnesium content to improve polymerization and thermal stability, while adding blue and red dyes as complementing agents to improve transparency.

Benefits of technology

Polyester polycondensation reaction is carried out at low temperatures to improve the thermal stability and polymerization of the polyester resin, reduce foreign matter content, ensure the uniformity and transparency of the film, and reduce the metal content of the catalyst, avoid environmental pollution, and improve the electrostatic clinging of the film and productivity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004981014020000031
    Figure BDA0004981014020000031
  • Figure BDA0004981014020000032
    Figure BDA0004981014020000032
  • Figure BDA0004981014020000041
    Figure BDA0004981014020000041
Patent Text Reader

Abstract

The present invention can perform a polycondensation reaction of a polyester at a low temperature, exhibits a high degree of polymerization while improving thermal stability of a polyester resin, minimizes a terminal group (carboxyl group), can prepare a polyester resin having a low content of foreign matter, has excellent electrostatic imparting properties and low melt resistivity, and can produce a thin film with excellent electrostatic imparting properties even at a high rotational speed. And a gap between the surface of the roller and the sheet-shaped article is not formed, the film with uniform thickness is prepared, and the film with high transparency can be prepared due to small foreign matter content.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a polyester composition for film and a polyester resin for film prepared therefrom. Background Art

[0002] Polyester means a polymer obtained by polycondensation of a compound formed by generating an ester between a carboxyl group and a hydroxyl group. Generally, polyester obtained by polymerizing terephthalic acid and ethylene glycol has excellent mechanical and chemical properties, and thus has high industrial value and is widely used in fibers, films, sheets, hollow molded bodies, and the like.

[0003] In particular, films using polyester resins have excellent properties such as mechanical properties, thermal properties, chemical resistance, and electrical properties, and are therefore widely used in various industrial fields such as magnetic recording media, capacitors, optics, and general industry.

[0004] However, in order to produce a film using such a polyester resin, there is a possibility that the following process problems will occur.

[0005] First, in order to use polyester resin to prepare film, it is necessary to use an electrostatic casting method that applies high voltage to make the sheet film close to a rotating cooling drum. The electrostatic applicability of polyester resin is low, which may reduce the adhesion between the above-mentioned film and the drum, which may reduce the thickness uniformity, transparency, surface smoothness and other physical properties of the film itself.

[0006] Secondly, in order to mold a film made of polyester resin, it is necessary to perform melt extrusion molding at a temperature above the melting point of 250 to 300°C. Therefore, even a small amount of oxygen flowing in during high-temperature processing may produce a large amount of foreign matter caused by oxidative decomposition, which reduces the transparency of the film. In order to compensate for the disadvantages of polyester resin, various catalysts are generally used in the polycondensation reaction of polyester resin, and antimony compounds or germanium compounds are mostly used on an industrial scale.

[0007] However, polyester resins produced by polycondensation using antimony compounds as catalysts have a characteristic black color, which raises concerns about toxicity and environmental pollution. Polyester resins produced by polycondensation using germanium compounds as catalysts are difficult to mass-produce industrially due to the scarcity of germanium itself. As an alternative, titanium (Ti)-based catalysts are introduced, which can overcome the problems of the above-mentioned antimony and germanium catalysts, but when used as polyester polycondensation catalysts, there may be problems such as yellowing of the polyester itself and unstable melt thermal stability. In particular, when titanium-based compound catalysts are used in films, the formation of particles such as byproducts cannot be suppressed, which affects the lubricity and smoothness of the film, and may eventually lead to film rupture.

[0008] Therefore, there is an urgent need to develop a catalyst that can improve the above-mentioned process problems of polyester resins and solve the unique problems of titanium-based compound catalysts instead of antimony compounds and germanium compounds. Summary of the invention

[0009] Technical issues

[0010] The present invention has been conceived to overcome the above-mentioned problems, and its purpose is to provide a polyester resin composition for preparing a film of a polyester resin having a low foreign matter content, which can carry out a polycondensation reaction of polyester at a low temperature, improve the thermal stability of the polyester resin, and minimize the terminal group (carboxyl group) due to a high degree of polymerization.

[0011] Furthermore, another object of the present invention is that the polyester resin according to the present invention has excellent electrostatic applicability and low melt resistivity. When it is used to prepare a film, no gap is formed between the roller surface and the sheet-like article even at a fast rotation speed, providing a uniform and highly transparent film.

[0012] Solutions to the problem

[0013] The present invention for solving the above-mentioned problems is a polyester resin composition for film, comprising a polyester resin, a titanium chelate catalyst, a fixing agent and a phosphorus compound, all of which satisfy the following relations (1) to (3).

[0014] (1) M = 1 to 150 ppm

[0015] (2) T = 5 to 45 ppm

[0016] (3) R = 0.01 to 10 MΩ cm

[0017] In this case, the above M means the total content of metal components other than phosphorus (P) in the polyester resin composition, the above T means the content of titanium based on the titanium element, and the above R means melt resistivity.

[0018] Furthermore, according to one embodiment of the present invention, the composition may be a polyester resin composition for a film, characterized in that it satisfies the following relational expression (4).

[0019] (4) P / M = 0.1 to 0.6

[0020] In this case, the above-mentioned P means the amount of phosphorus element contained in the phosphorus-based compound.

[0021] Furthermore, the composition may be a polyester resin composition for a film, wherein the titanium chelate catalyst is a reaction product of titanium-(IV)-alkoxide and alpha-hydroxy carboxylic acid represented by the following chemical formula 1.

[0022] Chemical formula 1

[0023] Ti-(OR1)4

[0024] In this case, the above R1 is an alkyl group having 1 to 6 carbon atoms and its isomers.

[0025] Furthermore, the composition may be a polyester resin composition for a film, wherein the reaction product is titanium alpha-hydroxy carboxylate represented by the following chemical formula 2.

[0026] Chemical formula 2

[0027]

[0028] Furthermore, the composition may be a polyester resin composition for a film, characterized in that the phosphorus compound is represented by the following Chemical Formula 3, and preferably may be triethyl phosphate (TEP).

[0029] Chemical formula 3

[0030]

[0031] In this case, the above R6 to R8 are each independently an alkyl group having 1 to 6 carbon atoms and its isomers.

[0032] Furthermore, the composition may be a polyester resin composition for a film, wherein the fixing agent is a magnesium (Mg) compound.

[0033] Furthermore, the composition may be a polyester resin composition for a film, characterized in that it further comprises 1 to 10 ppm of a color corrector comprising blue and red dyes, based on the total weight of the polyester resin composition.

[0034] According to yet another embodiment of the present invention, a film is prepared using a polyester resin composition selected from one of the above polyester resin compositions.

[0035] Furthermore, according to another embodiment of the present invention, there is provided a method for preparing a polyester resin for film, characterized in that it comprises: step (1), preparing an esterification reactant by reacting an acidic component and a diol component; and step (2), adding a titanium chelate catalyst, a fixing agent and a phosphorus compound to the esterification reactant prepared above to prepare a polyester resin, wherein in the above step (2), the composition of the titanium chelate catalyst, the fixing agent and the phosphorus compound are combined to prepare a polyester resin having a melt resistivity of 0.01 to 10 MΩ·cm.

[0036] Furthermore, the method for preparing a polyester resin for a film is characterized in that in the above step (2), the titanium chelate catalyst, the fixing agent and the phosphorus compound are combined, and the number of carboxyl groups at the terminal of the polyester resin is 1 to 45.

[0037] Furthermore, the method can be a method for preparing a polyester resin for a film, characterized in that the titanium-based chelate catalyst is a reaction product of titanium-(IV)-alk oxide and alpha-hydroxycarboxylic acid represented by the following chemical formula 1, and the phosphorus-based compound is represented by the following chemical formula 3.

[0038] Chemical formula 1

[0039] Ti-(OR1)4

[0040] In this case, the above R1 are each independently an alkyl group having 1 to 6 carbon atoms and its isomers, and at least one of them is not hydrogen.

[0041] Chemical formula 3

[0042]

[0043] In this case, the above R6 to R8 are each independently an alkyl group having 1 to 6 carbon atoms and an isomer thereof.

[0044] Furthermore, the composition may be a polyester resin composition for a film, wherein the reaction product is titanium alpha-hydroxy carboxylate represented by the following chemical formula 2.

[0045] Chemical formula 2

[0046]

[0047] In this case, the above R2 to R5 are each independently hydrogen or an alkyl group having 1 to 6 carbon atoms and its isomers.

[0048] Effects of the Invention

[0049] The polyester resin composition using the titanium chelate catalyst according to the present invention can carry out polycondensation of polyester at low temperature, improve the thermal stability of the polyester resin while presenting a high degree of polymerization, minimize the terminal group (carboxyl group), and prepare a polyester resin with a low foreign matter content.

[0050] The polyester resin according to the present invention has excellent electrostatic applicability and low melt resistivity. When it is used to prepare a film, no gap is formed between the roller surface and the sheet-like object even at a fast rotation speed. A film with uniform thickness can be prepared, with a small foreign matter content and a high transparency. DETAILED DESCRIPTION

[0051] Best Mode for Carrying Out the Invention

[0052] The following describes the embodiments of the present invention in detail so that those skilled in the art can easily implement the present invention. The present invention can be implemented in many different forms and is not limited to the embodiments described herein.

[0053] As mentioned above, conventional polyester resins are generally widely used due to their excellent chemical resistance, but the film production process using them has problems due to the physical properties unique to polyester resins, and catalysts have been introduced to improve these problems. However, the catalysts introduced in the past have difficulties in industrial production in terms of color tone, productivity, environmental pollution, and economy.

[0054] In view of this, the present invention provides a polyester resin composition for film comprising a polyester resin polycondensate, a titanium chelate catalyst, a fixing agent and a phosphorus compound, all of which satisfy the following relationships (1) to (3), in order to solve the above problems.

[0055] (1) M = 1 to 150 ppm

[0056] (2) T = 5 to 45 ppm

[0057] (3) R is less than 10 MΩ·cm

[0058] In this case, the above M means the total content of metal components other than phosphorus (P) in the polyester resin composition, the above T means the content of titanium based on the titanium element, and the above R means melt resistivity.

[0059] This can improve the physical properties of the polyester resin itself and at the same time improve the uniformity and transparency of the film prepared therefrom.

[0060] Hereinafter, the present invention will be described in detail.

[0061] The polyester resin polycondensate can be prepared by an esterification reaction of an acid component and a diol component.

[0062] The polymerization of the acidic component and the diol component can be carried out under the conditions commonly used in the esterification polymerization reaction in this field. As an example, it can be achieved by stirring at 40 to 80 rpm for 150 to 240 minutes at 200 to 260° C., but is not limited thereto.

[0063] On the other hand, the acidic component contains terephthalic acid and may contain an aromatic polyvalent carboxylic acid having 6 to 14 carbon atoms or an aliphatic polyvalent carboxylic acid having 2 to 14 carbon atoms or a sulfonic acid metal salt other than terephthalic acid.

[0064] The aromatic polyvalent carboxylic acid having 6 to 14 carbon atoms is an acidic component for preparing polyester, and any known one can be used without limitation. Preferably, it can be one or more selected from the group consisting of dimethyl terephthalate, isophthalic acid and dimethyl isophthalate, and more preferably, it can be isophthalic acid in terms of reaction stability with terephthalic acid, easy handling and economy.

[0065] Furthermore, an aliphatic polyvalent carboxylic acid having 2 to 14 carbon atoms is an acidic component used to prepare polyester, and known ones can be used without limitation. However, as a non-limiting example, it can be one or more selected from the group consisting of oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, suberic acid, citric acid, pimelic acid, azelaic acid, sebacic acid, nonanoic acid, decanoic acid, dodecanoic acid and hexadecanoic acid.

[0066] Furthermore, the metal sulfonate may be sodium 3,5-dimethoxybenzenesulfonate.

[0067] Next, the diol component which is one of the monomers of the esterification reaction product will be described.

[0068] The above-mentioned diol components may independently include aliphatic diol components and polyethylene glycol having 2 to 14 carbon atoms. As the aliphatic diol component, specifically, it can be selected from the group consisting of ethylene glycol, diethylene glycol, neopentyl glycol, 1,3-propylene glycol, 1,4-butylene glycol, 1,6-hexanediol, propylene glycol, trimethyl glycol, tetramethylene glycol, pentamethyl glycol, hexamethylene glycol, heptamethylene glycol, octamethylene glycol, nonamethylene glycol, decamethylene glycol, undecamethylene glycol, dodecamethylene glycol and tridecamethylene glycol, but is not particularly limited. Preferably, it can be selected from the group consisting of ethylene glycol, diethylene glycol, neopentyl glycol, 1,3-propylene glycol, 1,4-butylene glycol and 1,6-hexanediol.

[0069] Then, the titanium chelate catalyst means a titanium chelate compound with titanium as the central atom and other substances bonded around it. For this titanium chelate compound, it is stable even in the presence of water molecules, so it will not be deactivated even if added before the esterification reaction in which water is attached in large quantities, so the ester reaction and polycondensation reaction can be shortened more than before, and the coloring caused by yellowing can be suppressed. In addition, titanium alkoxides are water-insoluble substances in the past, and when applied to the process, there is a problem of being difficult to handle. The titanium chelate catalyst suitable for the present invention is a water-soluble substance, which has the advantages of being stable in the presence of water molecules and being highly active during polymerization reactions.

[0070] The titanium chelate catalyst may contain 10 to 15 ppm in terms of the obtained atom, which makes the thermal stability and color tone better, and is therefore preferred. When the content is less than 10 ppm in terms of the titanium atom, it may be difficult to properly promote the esterification reaction, and when it is greater than 15 ppm, the reactivity is promoted, but there may be a problem of coloration.

[0071] Such titanium chelate catalysts may be commonly used, and as the titanium compound, may have one or more substituents selected from the group consisting of alkoxy, phenoxy, acylation, amino and hydroxyl groups. For example, tetraalkoxy groups such as tetraethanolate, tetrapropoxide, tetraisopropoxide, tetrabutoxy, tetra-2-ethylhexaoxide, B-diketone functional groups, hydroxy polyvalent carboxylic acid functional groups such as lactic acid, malic acid, tartaric acid, salicylic acid, citric acid, ketoester functional groups such as methyl acetoacetate and ethyl acetoacetate may be cited. As the phenoxy group, for example, phenoxy, cresol salt, etc. may be cited. As the acylation group, for example, tetraacylation groups such as lactate and stearate, phthalic acid, trimellitic acid, trimesic acid, hemimeric acid, pyrophosphate, oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, sebacic acid, maleic acid, phthalic acid, cyclohexanedicarboxylic acid or a polyvalent carboxylic acid functional group thereof, ethylenediaminetetraacetic acid, nitriletripropionic acid, carboxyiminodiacetic acid, carboxymethyliminodipropionic acid, diethylenetriaminoacetic acid, triethylenetetraaminohexaacetic acid, iminodiacetic acid, iminodipropionic acid, hydroxyethyliminodiacetic acid, hydroxyethyliminodipropionic acid, methoxyethyliminodiacetic acid, etc. can be used, but are not limited thereto.

[0072] The reaction product of titanium alkoxide (titanium-(IV)-alkoxide) and alpha-hydroxy carboxylic acid represented by the following chemical formula 1 is preferred, which is advantageous in terms of polymerization reaction. That is, titanium alkoxide is a water-insoluble substance in the past, and when applied to the process, there is a problem of difficulty in handling, but the titanium chelate compound applicable to the present invention is a water-soluble substance, which has the advantages of being stable even in the presence of water molecules and having high activity during polymerization reaction.

[0073] Chemical formula 1

[0074] Ti-(OR1)4

[0075] In this case, the above R1 is hydrogen or an alkyl group having 1 to 6 carbon atoms and its isomers, at least one of which is not hydrogen.

[0076] At this time, the reaction product may be titanium alpha-hydroxy carboxylate represented by the following Chemical Formula 2.

[0077] Chemical formula 2

[0078]

[0079] In this case, the above R2 to R5 are each independently hydrogen or an alkyl group having 1 to 6 carbon atoms.

[0080] In particular, the use of the above-mentioned chemical formula 2 as the titanium chelate catalyst according to the present invention is most preferred when maximizing the effects of low process temperature, high polymerization degree, heat resistance, minimization of terminal groups, etc. When the polyester polycondensation reaction is carried out using other known titanium-based polyester catalysts instead of the titanium-based chelate catalyst represented by chemical formula 2 according to the present invention, there may be problems such as yellowing of the polyester itself and unstable melt heat stability.

[0081] The same is true for films. When films are prepared by using other well-known titanium-based polyester catalysts instead of using the polyester resin prepared by the titanium-based chelate catalyst represented by Chemical Formula 2 according to the present invention, the particle formation of by-products etc. cannot be suppressed, which affects the lubricity and smoothness of the film, and may eventually lead to film rupture.

[0082] The titanium α-hydroxycarboxylate represented by the above chemical formula 2 is more stable in the presence of water molecules than conventional titanium chelate catalysts, and thus does not deactivate even when added before the esterification reaction where a large amount of water is attached, so that the esterification reaction and polycondensation reaction can be carried out in a shorter time than before, thereby suppressing coloration caused by yellowing. In addition, the polymerization reaction can be carried out at a low temperature, and the heat resistance of the polyester resin can be improved while presenting a high degree of polymerization, minimizing the terminal group (carboxyl group), and preparing a polyester resin with a low foreign matter content.

[0083] However, in order to obtain the intended effect, the present invention needs to use the above-mentioned titanium chelate. When the titanium chelate forms a coordination bond or reacts with other types of compounds, the intended heat resistance and high degree of polymerization cannot be obtained, and the number of end groups increases, and there may be a problem of reduced physical properties due to foreign matter content. Moreover, when the titanium chelate catalyst according to the present invention is applied, the metal content can be greatly reduced to less than 1 / 10 compared with the previous (Sb catalyst), showing excellent melt resistivity.

[0084] Then, the above-mentioned fixing (pinning) agent performs the function of suppressing the formation of foreign matter when the polyester undergoes polycondensation reaction, increasing the degree of polymerization and reducing the melt resistivity. In the present invention, commonly used fixing agents can be used without particular limitation, but preferably, metal-based fixing agents can be used, more specifically, alkali metal compounds, alkaline earth metal compounds, manganese compounds, cobalt compounds, zinc compounds, etc., which have large electrostatic activity and are therefore preferred. As their specific examples, magnesium acetate, sodium acetate, calcium acetate, lithium acetate, calcium phosphate, magnesium oxide, magnesium hydroxide, magnesium alcohol, manganese acetate, zinc acetate, etc. can be used, and one or more of them can be mixed and used. More preferably, it can be a magnesium (Mg)-based compound.

[0085] At this time, the fixing agent can be included in the polyester resin composition at 10 to 100 ppm based on the element used. If the fixing agent content is less than 10 ppm, when casting the film, the sheet-type article and the cooling drum do not produce high adhesion, resulting in uneven film thickness, and the speed cannot be increased during casting, thereby reducing the film preparation efficiency. If the fixing agent content is greater than 100 ppm, the metal content becomes more, resulting in this part being a disadvantage when preparing the film, and problems such as poor appearance that are not conducive to products and processes may occur. More preferably, it can be included at 20 to 80 ppm.

[0086] Then, the phosphorus compound is contained in the polyester resin composition of the present invention and functions as a heat stabilizer during the polycondensation process.

[0087] As the above-mentioned phosphorus compound, phosphoric acid, phosphorous acid, phosphonic acid and their derivatives may be mentioned. As specific examples, phosphoric acid, trimethyl phosphate, tributyl phosphate, triphenyl phosphate, monomethyl phosphate, dimethyl phosphate, monobutyl phosphate, dibutyl phosphate, phosphorous acid, trimethyl phosphite, tributyl phosphite, methylphosphonic acid, dimethyl methylphosphonic acid, dimethyl ethylphosphonic acid, ethyl diethylphosphonoacetate, dimethyl phenylphosphonic acid, diethyl phenylphosphonic acid, phenylphosphonic acid and the like may be mentioned. Preferably, among them, diethylphosphonoacetate and trimethyl phosphate may be mentioned. More preferably, the above-mentioned phosphorus compound may be represented by the following Chemical Formula 3. More preferably, it may be triethyl phosphate (TEP, Triethyl phosphate).

[0088] When the phosphorus compound represented by the following chemical formula 3 according to the present invention is used, the activity of the titanium catalyst as a heat stabilizer is more favorable than when the above-mentioned known phosphorus compounds are used. When other known phosphorus compounds are used instead of the phosphorus compound represented by the following chemical formula 3, the purpose of the present invention of improving the heat resistance of the polyester resin and minimizing the melt resistivity cannot be achieved.

[0089] Chemical formula 3

[0090]

[0091] In this case, the above R6 to R8 are each independently hydrogen or an alkyl group having 1 to 6 carbon atoms and its isomers, and at least one of them is not hydrogen.

[0092] In the above chemical formula 3 of the present invention, the above PO 4- The base can easily form a complex through coordination bonds on various metals, thereby realizing a high molecular weight complex. The appropriate equivalent ratio of the metal catalyst and phosphorus is an important factor in forming reactants and improving the melt resistivity. That is, the lower the equivalent ratio of phosphorus to metal, the lower the melt resistivity, so the design can be appropriately changed in consideration of the above effects.

[0093] The phosphorus compound may contain 10 to 30 ppm of phosphorus atoms relative to the mass of the polyester resin composition finally obtained. When the phosphorus compound content is less than 5 ppm relative to the mass of the polyester resin composition, it cannot fully function as a heat stabilizer, which may cause the heat resistance of the polyester resin to decrease. On the contrary, when the phosphorus compound content is greater than 30 ppm, the melt resistivity value is large, which hinders the applicability as a film, and a large amount of highly insoluble foreign matter may be generated, which may affect the transparency.

[0094] On the other hand, the polyester resin composition for film of the present invention must satisfy all of the following relations (1) to (3) in order to achieve its purpose.

[0095] (1) M = 1 to 150 ppm

[0096] (2) T = 1 to 40 ppm

[0097] (3) R is less than 10 MΩ·cm

[0098] In this case, the above M means the total content of metal components other than phosphorus (P) in the polyester resin composition, the above T means the content of titanium based on the titanium element, and the above R means melt resistivity.

[0099] The above relationship (1) is explained. The total content of the metal component (M) refers to (defined as) the concept of metal components included in the metal components and impurities of the final product. That is, the total content of the metal component (M) means all metal components except phosphorus in the polyester resin composition, for example, it can be the sum of the titanium metal content, magnesium content, etc. contained in the composition.

[0100] This metal component can react with bis(2-hydroxyethyl)terephthalate (BHT) generated in the polyester polymerization process to form compounds such as BHT TP Complex. and BHT-Metal-P, or react with titanium used as a catalyst to form foreign matter. Such foreign matter acts as a defect in the prepared polyester resin, which can reduce cleanliness and physical properties.

[0101] Therefore, the above metal component is contained in 0.01 to 150 ppm. When it is greater than 150 ppm, a large amount of foreign matter is formed in the polyester resin, the degree of polymerization becomes significantly lower, it is difficult to achieve viscosity and the required chemical / physical properties, and the metal may precipitate or form a complex in the resin, resulting in internal defects. Therefore, the transparency of the film prepared thereby may be reduced, resulting in haze. More preferably, considering the effect of the metal chelating agent of phosphorus described later, the metal component can be contained in 0.01 to 100 ppm.

[0102] Next, relational expression (2) will be described.

[0103] The titanium content (T) is contained in the polyester resin composition at 1 to 40 ppm based on the titanium element. When the content is less than 1 ppm in terms of titanium atoms, it may be difficult to properly promote the esterification reaction, and when it is greater than 40 ppm, the reactivity is promoted but there may be a problem of coloration.

[0104] In the past, titanium alkoxides were water-insoluble substances, which were difficult to handle when used in the process. The catalyst used in the present invention is a water-soluble substance, which has the advantages of being stable even in the presence of water molecules and having high activity during polymerization. In this regard, it is preferably included in an amount of 1 to 15 ppm, and more preferably, it can be included in an amount of 10 to 25 ppm to exhibit the best catalyst activity while reducing the metal component.

[0105] Next, the above-mentioned melt resistivity (R) expressed by relational expression (3) will be described.

[0106] Melt resistivity is one of the physical properties of polyester resins. It means a physical property confirmed as an indicator of electrostatic adhesion when a polyester resin is formed into a film by electrostatic adhesion casting to prepare a film. The smaller the value, the better the electrostatic adhesion, and a film of uniform thickness can be obtained during the casting process, which can affect the rotation speed and increase the production speed.

[0107] At this time, the polyester resin composition according to the present invention can present a melt resistivity of 0.01 to 10MΩ·cm. When the melt resistivity is greater than 10MΩ·cm, static electricity is not fully released from the surface of the sheet (film), and good electrostatic adhesion cannot be presented. That is, during the casting process, bubbles are generated between the rotating cooling drum and the sheet, and a film of uniform thickness cannot be obtained, which may affect the yield caused by the reduction in production speed. In addition, when the melt resistivity is below 0.01MΩ·cm, there is a problem of reduced adhesion when casting the film, resulting in poor casting. Therefore, as a range that exhibits good electrostatic adhesion without reducing the physical properties of the film, it is more preferred that a melt resistivity of 0.1 to 3MΩ·cm can be presented.

[0108] Then, the polyester resin composition for film according to one embodiment of the present invention may further include a color correcting agent to improve the optical properties of the film. In this case, the color correcting agent containing blue and red dyes may be included in an amount of 1 to 10 ppm based on the total weight of the polyester resin composition.

[0109] As the above-mentioned color-correcting agent, those known in the field of fiber can be added, and non-limiting examples thereof include dyes for coloring with original solution, pigments, vat dyes, disperse dyes, organic pigments, etc. However, preferably, a mixture of blue and red dyes can be used. This is because the cobalt compounds commonly used as color-correcting agents are highly harmful to the human body, and are therefore not preferred. On the contrary, a color-correcting agent mixed with blue and red dyes is harmless to the human body, and is therefore preferred. Moreover, when a blue and red dye are used in combination, the color tone can be subtly controlled. As an example, the above-mentioned blue dye can include solvent blue 104, solvent blue 122, solvent blue 45, etc., and as an example, the above-mentioned red dye can include solvent red 111, solvent red 179, solvent red 195, etc.

[0110] When the content of the color correcting agent in the composition is greater than 10 ppm, there may be problems such as reduced dispersibility, generation of foreign matter or scattering. On the contrary, when the content of the color correcting agent in the composition is less than 1 ppm, the yellow color peculiar to titanium is presented, and a slight difference in hue becomes a problem, which may hinder its full use in films for optical purposes, etc. Therefore, in order to balance the dispersibility and hue, the color correcting agent is more preferably contained in 2 to 8 ppm.

[0111] When the color coordinate b value of the resin caused by such a color-correcting agent is greater than 8, the color of the film is affected, and it is not suitable for optical films requiring transparency. Not only the color of the film surface, but also the color of the side of the film may change, resulting in poor appearance. Therefore, the color coordinate b value is preferably 8 or less.

[0112] On the other hand, as described above, the metal component (M) inhibits the activity of the catalyst or forms foreign matter, thereby reducing the physical properties of the polycondensed polyester resin. However, for more efficient polyester polycondensation, the use of metals such as catalysts and fixatives is essential.

[0113] At this time, in addition to the effect of being the above-mentioned heat stabilizer, phosphorus (P) can also perform the role of a metal ion chelating agent (Seque stering Agent) that reacts with the above-mentioned metal components to prevent the formation of other foreign substances. Metal ion chelating agents are mainly used to chemically act on metal ions, reduce their activity or reduce the content of impurities to increase the yield of the target compound. Therefore, as long as the optimal content ratio of metal components and phosphorus (P) is understood, the formation of foreign substances caused by metal ions can be minimized while improving the physical properties of polyester.

[0114] In this regard, according to one embodiment of the present invention, the polyester resin composition of the present invention may also satisfy the following relational formula (4).

[0115] (4) P / M = 0.1 to 0.6

[0116] When the ratio of the content of metal ions to phosphorus in the composition is greater than 0.6, the melt resistivity value becomes high, and when casting a film, the film thickness may be uneven or the casting may not be smooth. When the ratio of the content of metal ions to phosphorus in the composition is less than 0.1, phosphorus cannot fully perform the role of a metal ion chelating agent, resulting in the generation of foreign matter, etc., and the physical properties of the polyester resin itself may be reduced. In addition, the amount of phosphorus compound used is preferably 10 to 30 ppm in terms of phosphorus atoms relative to the polymer obtained after polymerization.

[0117] On the other hand, the polyester resin prepared according to one embodiment of the present invention may contain 1 to 45 terminal carboxyl groups. As described above, when the polyester resin composition according to the present invention is used, a high degree of polymerization is obtained while performing polymerization at a low temperature, and an effect of reducing polymer terminal groups (COOH) can also be obtained. This can achieve the effect of more stably performing the process and increasing the production speed.

[0118] Furthermore, the inherent viscosity of the polyester resin prepared according to one embodiment of the present invention may be 0.300 to 0.900 dl / g. When the inherent viscosity is less than 0.300 dl / g, the problem of insufficient viscosity causing a large number of bubbles to be generated during film casting due to the thin viscosity may occur, and when the inherent viscosity is greater than 0.900 dl / g, the problem of not being able to cast uniformly during casting due to the high viscosity may occur. More preferably, it may be 0.500 to 0.800 dl / g.

[0119] As described above, the polyester resin composition according to the present invention provides an optimal polyester resin for film by adjusting the content of other metal additives including the titanium-based chelate catalyst.

[0120] Next, a film produced using the above-mentioned polyester resin according to the present invention is explained.

[0121] Generally, films made of polyester have excellent properties such as mechanical properties, thermal properties, chemical resistance, and electrical properties, and are therefore widely used in industrial applications such as magnetic recording media, capacitors, optics, and general industry. Generally, polyester films are obtained by melt-extruding a polyester resin using an extruder and then biaxially stretching it in the transverse and longitudinal directions.

[0122] At this time, when the polyester film is molded, it is melted and extruded at a temperature above the melting point of the polyester resin, which is 250 to 300°C. This may cause thermal decomposition of the polyester resin. When a small amount of oxygen is mixed in, gel-type foreign matter caused by oxidative decomposition may be produced, which may act as an internal defect in the molded film.

[0123] Furthermore, when polyester resin is made into a film, an electrostatic casting method is mainly used in which a high voltage is applied to the upper surface of a sheet-like object so that the sheet-like object is closely attached to a rotating cooling drum. However, in order to increase the film-making speed, when the speed of the rotating cooling drum is increased, the close contact between the sheet-like film and the rotating cooling drum may be reduced, and the thickness uniformity or transparency of the film may be reduced, resulting in a defective film surface caused by uneven application. In particular, in recent years, a high degree of surface smoothness or thin film formation is required in films for magnetic recording media or dry film resists, and the above-mentioned gel-type foreign matter or poor electrostatic application may worsen such film surface defects or transparency, and is therefore not preferred.

[0124] In view of this, the present invention seeks to solve the conventional problems by preparing a film using a polyester resin prepared from the polyester composition for film of the present invention. To avoid repetition, the description of the polyester resin composition for film and the polyester resin prepared therefrom is omitted.

[0125] When a film is produced by an electrostatic application casting method using a polyester resin prepared from the polyester composition for film according to the above-mentioned present invention, no gap is formed between the sheet film and the rotating cooling drum, and high electrostatic adhesion is achieved, allowing uniform casting even when the rotation speed of the cooling rotating drum is increased.

[0126] That is, according to the polyester resin of the present invention, under the conditions that the above-mentioned relationship formulas (1) to (3) are satisfied, the charge amount on the film surface becomes high, the electrostatic applicability is excellent, and high electrostatic adhesion is exhibited. Even at a fast rotation speed, no gap is formed between the roller surface and the sheet film, and a uniform and highly transparent film can be prepared.

[0127] Furthermore, a high-polymer polyester resin having a low content of terminal carboxyl groups can be obtained during the polycondensation process, and has a small melt resistivity value. Even at low temperatures, film forming processing can be performed, and a film having excellent heat resistance can be prepared.

[0128] In the present invention, the polyester film can be prepared using the above-mentioned polyester composition by a conventional preparation method, for example, by melt extrusion using the conventionally known T-die method to obtain an unstretched sheet, stretching the obtained unstretched sheet to 2 to 7 times, preferably 3 to 5 times in the mechanical direction, and then stretching it 2 to 7 times, preferably 3 to 5 times in the transverse direction.

[0129] Next, a method for producing the polyester resin for a film according to the present invention is described.

[0130] The polyester resin is prepared by satisfying the following relationships (1) to (3), comprising: step (1), preparing an esterification reaction product by reacting an acid component and a diol component; and step (2), adding a titanium chelate catalyst, a fixing agent and a phosphorus compound to the esterification reaction product prepared above to prepare a polyester resin.

[0131] (1) M = 1 to 150 ppm

[0132] (2) T = 1 to 40 ppm

[0133] (3) R is less than 10 MΩ·cm

[0134] At this time, the above M means the total content of metal components other than phosphorus (P) in the polyester resin composition, the above T means the content of titanium based on the titanium element, and the above R means the melt resistivity. In order to avoid repetition, the description of the above polyester resin composition for film and the polyester resin prepared therefrom is omitted.

[0135] In step (1), the acid component and the diol component can be reacted by esterification under known synthesis conditions in the field of polyester synthesis to obtain an esterification product. At this time, the acid component and the diol component can be added in a manner of reacting at a molar ratio of 1:1.1 to 2.0, but the present invention is not limited thereto.

[0136] In addition, the esterification reaction can be preferably performed at a temperature of 200 to 270° C. and a pressure of 1100 to 1350 Torr. If the above conditions are not met, the esterification reaction time may be prolonged or the reactivity may be reduced, and an esterified compound suitable for the polycondensation reaction may not be formed. In addition, the polycondensation reaction can be performed at a temperature of 250 to 300° C. and a pressure of 0.3 to 1.0 Torr. If the above conditions are not met, there may be problems such as delayed reaction time, reduced polymerization degree, and thermal decomposition induction.

[0137] Then, as step (2), the titanium-based chelate catalyst, the fixing agent and the phosphorus-based compound according to the present invention are added to the esterification reaction product prepared in the above step (1) to carry out polycondensation with the polyester resin.

[0138] At this time, the titanium-based chelate catalyst may be a reaction product of titanium-(IV)-alkoxide and alpha-hydroxy carboxylic acid represented by the following chemical formula 1, and the phosphorus-based compound may be represented by the following chemical formula 3. When such a titanium-based chelate catalyst is used, the reaction speed is faster than when an Sb catalyst is used, so polycondensation can be performed even at a relatively low temperature.

[0139] The reaction product may be titanium alpha-hydroxycarboxylate represented by the following Chemical Formula 2.

[0140] Chemical formula 1

[0141] Ti-(OR1)4

[0142] In this case, the above R1 is an alkyl group having 1 to 6 carbon atoms.

[0143] Chemical formula 2

[0144]

[0145] In this case, the above R2 to R5 are each independently hydrogen or an alkyl group having 1 to 6 carbon atoms.

[0146] Chemical formula 3

[0147]

[0148] Furthermore, the above R6 to R8 are each independently hydrogen or an alkyl group having 1 to 6 carbon atoms, and at least one of them is not hydrogen.

[0149] As described above, the polyester resin composition for film according to the present invention contains a titanium chelate catalyst, a fixing agent and a phosphorus compound, and proposes an optimal content ratio thereof, so that a polyester resin for film with improved production speed and yield and a film based thereon can be prepared while having excellent thermal stability and melt resistivity.

[0150] Modes for carrying out the invention

[0151] Example 1: Preparation of polyester resin

[0152] After 100% terephthalic acid (TPA) as an acid component and 100 mol% ethylene glycol (EG) as a diol component were added to an ester reaction tank, the reaction was carried out at 250°C and 1140 Torr to obtain an ester reaction product. At this time, the acid component and the diol component were added at a molar ratio of 1:1.2.

[0153] The formed ester reactant is transferred to a polycondensation reactor, and a compound represented by the following chemical formula 1-1 as a polycondensation catalyst and 20 ppm of a titanium-based chelate catalyst represented by chemical formula 2 as a reaction product of alpha-hydroxy carbo xylic acid are added, and 25 ppm (P element basis) of triethyl phosphate as a thermal stabilizer is added, and the pressure is gradually reduced to a final pressure of 0.5 Torr, and the temperature is raised to 280°C to perform a polycondensation reaction to prepare a polyester resin.

[0154] Chemical formula 1-1

[0155] Ti(OR)4

[0156] Chemical formula 2-1

[0157]

[0158] All of the above R2 to R4 are hydrogen.

[0159] Example 2 to Example 10: Preparation of polyester resin

[0160] The same method as in Example 1 was followed to prepare the products, except that the metal content or the magnesium content was changed. The results are shown in Table 2.

[0161] Example 11-Example 12: Preparation of polyester resin

[0162] The same preparation as in Example 1 was carried out except that the content of the titanium chelate catalyst was changed. The results are shown in Table 2.

[0163] Experimental Example 1: Determination of Melting Resistivity

[0164] After the polyester resin according to the embodiment and preparation example of the present invention is quantitatively added into a glass tube, it is placed in a melting bath to be melted. After shielding the portion except the electrode measurement portion with Teflon tape in a non-electrical manner, a measurement probe (electrode) is inserted into the molten polymer to transfer the charge. Press the start button of the resistance measurement software, and after stabilization for 10 minutes, the resistance value is recorded.

[0165] Experimental Example 2: Determination of intrinsic viscosity

[0166] The polyester resin prepared in the example was melted in an ortho-chlorophenol solvent at 110° C. at a concentration of 2.0 g / 25 ml for 30 minutes, then kept at 25° C. for 30 minutes, and the intrinsic viscosity was measured using an automatic viscosity measuring device connected to a CANON viscometer.

[0167] Experimental Example 3: Quantification of carboxyl end groups

[0168] The carboxyl content of the embodiment is measured according to the following method. 0.15 g of polyester powder crushed into a 20-mesh size is accurately weighed and placed in a test tube. 5 ml of benzyl alcohol is added, stirred using an ultra-small stirrer, and heated to dissolve at 210° C. for 1300 seconds. After dissolution, the test tube is immersed in 25° C. water for 6 seconds to quench it, and the content is poured into a 50 ml beaker containing 10 ml of chloroform, and 5 ml of benzyl alcohol is placed in the test tube and stirred for 60 seconds, and the remaining polyester resin solution is completely rinsed. The carboxyl content is determined by neutralizing and titrating 0.1 N sodium hydroxide benzyl alcohol solution using a microsyringe (capacity: 100 μl) using phenol red (0.1% benzyl alcohol solution) as an indicator, and the titration determination value is corrected based on the blank test result of the titration reagent, and calculated according to the following mathematical formula 1.

[0169] Mathematical formula 1: Carboxyl content (eq. / 106g polyester)

[0170] Volume of titration solution (ml) - blank test result (ml) × 0.1 × f ÷ weight of polyester sample

[0171] At this time, f is the concentration coefficient of 0.1N sodium hydroxide benzyl alcohol solution.

[0172] Experimental Example 4: Number of Internal Defects

[0173] The polyester resin according to the present invention prepared by the internal defect measurement method is melted on a slide glass to prepare a sample with a thickness of 500 μm, and the defects of a layer with a depth of 180 μm are observed under a transmitted light with a magnification of 200 times using an optical microscope, and the number of defects with a size of 1.5 μm or more in an area of ​​448 μm×336 μm is calculated by averaging the number of defects on a total of 5 microscope photos. In addition, the defect size can be measured by a microscope scale bar, and the measurement is based on the long axis of the defect.

[0174] Experimental Example 5: Determination of film haze

[0175] The polyester resin was melted by an extruder using a T-die using a Pilot film making machine and cooled using a casting drum to prepare a sheet with a thickness of 1690 μm. The prepared sheet was stretched 3 times in the transverse and longitudinal directions to prepare a 188 μm sheet, and the haze of the film was measured.

[0176] The haze measurement method is based on ASTM D-1003. Seven parts are randomly selected from two positions on the edge and one position in the center of the film, and then cut into pieces of 5 cm × 5 cm in size. The pieces are placed in a haze meter (NIPPON DENSHOKUNDH 300A) and light of 555 nm wavelength is transmitted. The average value excluding the maximum / minimum value is calculated according to the following mathematical formula 2.

[0177] Mathematical formula 2: Haze (%)

[0178] (Total scattered light / total transmitted light)×100

[0179] Table 1

[0180]

[0181] Table 2

[0182]

[0183] Referring to Table 1 and Table 2, it can be seen that all physical properties of Examples 3 and 4, which meet all numerical ranges of the present invention, are excellent. That is, it can be seen that in Examples 5 to 8, which have high metal contents, the melt resistivity is high or the internal defect test is poor. In addition, it can be seen that in Examples 11 and 12, in which the content of the titanium chelate catalyst exceeds the numerical range of the present invention, all physical properties show significantly low results.

Claims

1. A polyester resin composition for film, comprising a polyester resin polycondensate, a titanium chelate catalyst, a fixing agent and a phosphorus compound, all of which satisfy the following equations (1) to (3), characterized in that: (1) M = 1 to 150 ppm (2) T = 1 to 40 ppm (3) R is less than 10 MΩ·cm In this case, the above-mentioned M means the total content of metal components other than phosphorus (P) in the polyester resin composition. The above T means the content of titanium based on the titanium element. The above R means the melting resistivity.

2. The polyester resin composition for film according to claim 1, wherein the polyester resin composition for film satisfies the following relational expression (4), characterized in that: (4) P / M = 0.1 to 0.6 In this case, the above-mentioned P means the amount of phosphorus element contained in the phosphorus-based compound.

3. The polyester resin composition for film according to claim 1, wherein the titanium chelate catalyst is a reaction product of a titanium alkoxide and an α-hydroxycarboxylic acid represented by the following chemical formula 1, characterized in that: Chemical formula 1 Ti-(OR1)4 In this case, the above R1 are each independently hydrogen or an alkyl group having 1 to 6 carbon atoms, at least one of which is not hydrogen.

4. The polyester resin composition for film according to claim 3, wherein the reaction product is a titanium α-hydroxycarboxylate represented by the following chemical formula 2, characterized in that: Chemical formula 2 In this case, the above R2 to R5 are each independently hydrogen or an alkyl group having 1 to 6 carbon atoms.

5. The polyester resin composition for film according to claim 1, wherein the phosphorus compound is represented by the following chemical formula 3, characterized in that: Chemical formula 3 In this case, the above R6 to R8 are each independently an alkyl group having 1 to 6 carbon atoms and an isomer thereof.

6. The polyester resin composition for film according to claim 1, characterized in that: The fixing agent is a magnesium (Mg) compound.

7. The polyester resin composition for film according to claim 1, characterized in that: The polyester resin composition further comprises 1 to 10 ppm of a color-correcting agent comprising blue and red dyes, based on the total weight of the polyester resin composition.

8. A polyester resin for film, characterized in that: The polyester resin composition is prepared using the polyester resin composition selected from any one of claims 1 to 7, and has 1 to 45 terminal carboxyl groups.

9. A film, characterized in that: The film is prepared using the polyester resin as claimed in claim 8.

10. A method for preparing a polyester resin for a film, which satisfies all of the following equations (1) to (3), and the method for preparing a polyester resin for a film comprises: Step (1), preparing an esterification reaction product for reacting an acid component and a diol component; and step (2), adding a titanium chelate catalyst, a fixing agent and a phosphorus compound to the esterification reactant prepared above to prepare a polyester resin, characterized in that: (1) M = 1 to 150 ppm (2) T = 1 to 40 ppm (3) R is less than 10 MΩ·cm In this case, the above-mentioned M means the total content of metal components other than phosphorus (P) in the polyester resin composition. The above T means the content of titanium based on the titanium element. The above-mentioned R means the melting resistivity.

11. The method for preparing a polyester resin for a film according to claim 10, wherein the titanium chelate catalyst is a reaction product of a titanium alkoxide and an α-hydroxycarboxylic acid represented by the following chemical formula 1, and the phosphorus compound is represented by the following chemical formula 3, characterized in that: Chemical formula 1 Ti-(OR1)4 In this case, the above R1 is an alkyl group having 1 to 6 carbon atoms, Chemical formula 3 In this case, the above R6 to R8 are each independently an alkyl group having 1 to 6 carbon atoms and an isomer thereof.

12. The method for preparing a polyester resin for a film according to claim 10, wherein the reaction product is a titanium α-hydroxycarboxylate represented by the following chemical formula 2, characterized in that: Chemical formula 2 In this case, the above R2 to R5 are each independently hydrogen or an alkyl group having 1 to 6 carbon atoms.