Demolding film
By combining low molecular weight organosilicon and Si-H-based aqueous coating compositions with polyvinyl alcohol resins, the problem of balancing peelability and wettability in the release layer is solved, achieving efficient and uniform release layer coating and reducing manufacturing costs.
Patent Information
- Application Number
- CN202380031171.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-29
- Filing Date
- 2023-03-24
- Publication Date
- 2024-11-15
AI Technical Summary
Existing release films face challenges in balancing the peelability and wettability of the release layer. Furthermore, organic solvent-based coating compositions are unsuitable for online coating, resulting in high manufacturing costs and complex processes. Meanwhile, silicone-based waterborne coating compositions are prone to generating aggregates during coating, affecting the surface shape.
Using low molecular weight organosilicon and organosilicon containing Si-H groups as water-based coating compositions, a release layer is formed through an addition reaction. Combined with polyvinyl alcohol-based resin, the composition of the release layer is optimized to improve peelability and wettability, and the cost is reduced through an online coating process.
It achieves good peelability and wettability of the release layer, high coating uniformity, reduces manufacturing costs and foreign matter generation, and improves reusability.
Smart Images

Figure BDA0005063744860000041 
Figure BDA0005063744860000042 
Figure BDA0005063744860000051
Abstract
Description
Technical Field
[0001] The present invention relates to a release film having a base film and a release layer, and relates to a release film useful as a film for various processes. Background Art
[0002] In the past, release films based on polyester films or the like had high heat resistance and mechanical properties and were used as process films for forming resin sheets such as adhesive sheets, cover films, ceramic slurries, and polymer electrolyte membranes. In addition, as release layers of release films, since they have good heat resistance and peelability, various release layers formed from coating compositions containing silicone have been proposed (e.g., Patent Documents 1 to 7).
[0003] Patent Documents 1 and 2 propose release films in which a release layer is formed using a coating composition containing polysiloxane having an unsaturated group, polysiloxane having a Si—H group, a platinum group metal catalyst, and an organic solvent.
[0004] However, this technology has a problem that it is not suitable for a coating method during the stretching film formation of a substrate film (hereinafter referred to as "online coating") because an organic solvent is formed as a coating composition. In other words, since an organic solvent is used alone as a solvent for the coating composition, a large-scale explosion-proof device is required for the film-forming stretching equipment, which consumes initial installation costs and complicates operation, thereby increasing the manufacturing cost.
[0005] On the other hand, as a technology suitable for in-line coating, a release film using an aqueous coating composition to form a release layer, the aqueous coating composition comprising an alkenyl-containing silicone and an Si-H-containing silicone is proposed in Patent Document 3. In addition, as an example, a release film using an alkenyl-containing silicone with a number average molecular weight of 25,000 and an Si-H-containing silicone with a number average molecular weight of 4,500 to form a release layer is disclosed.
[0006] In addition, Patent Document 4 proposes a release film which uses a film containing SiO 4 / 2 The present invention discloses a mold release film in which a mold release layer is formed by using an aqueous coating composition of an alkenyl-containing silicone having a Q unit and an Si-H-containing silicone. In addition, as an example, a mold release film is disclosed in which a mold release layer is formed by using an alkenyl-containing silicone having a Q unit and a number average molecular weight of 25,000 and an Si-H-containing silicone having a number average molecular weight of 4,500.
[0007] As described above, conventionally, when forming a release layer, a relatively high molecular weight polysiloxane containing an unsaturated group is generally used in order to facilitate formation of a helical structure of polydimethylsiloxane on the coating surface. This also applies to the case of using an organic solvent-based coating composition (e.g., Patent Documents 1 to 2).
[0008] On the other hand, Patent Document 5 proposes a release film obtained by using polyvinyl alcohol as a primer layer of a release layer of a silicone resin. The primer layer and the release layer are applied in different steps, and two coatings are required to produce the release film. Usually, after applying the primer layer, the film is wound up in the form of a film roll, and then the film roll is unwound at another processing site and coated with a release layer, which increases the number of management items, complicates the manufacturing process, and is inefficient.
[0009] In addition, Patent Document 6 proposes a technique for forming a release layer by adding a polyvinyl alcohol-based resin to an aqueous coating composition containing an addition reaction type silicone in order to adjust the releasability of the release layer. However, as the addition reaction type silicone, a silicone with a relatively high molecular weight is used, as in other patent documents.
[0010] Prior art literature
[0011] Patent Literature
[0012] Patent Document 1: Japanese Patent Application Publication No. 2003-292894
[0013] Patent Document 2: Japanese Patent Application Publication No. 2003-292895
[0014] Patent Document 3: Japanese Patent No. 6077327
[0015] Patent Document 4: Japanese Patent Application Publication No. 2021-11081
[0016] Patent Document 5: Japanese Patent Application Publication No. 2000-289168
[0017] Patent Document 6: Japanese Patent No. 5319329
[0018] Patent Document 7: International Publication No. WO2017 / 200056 Summary of the invention
[0019] Problem that the invention aims to solve
[0020] However, in recent years, there is a trend of thinner ceramic green sheets and other components formed on the release layer of the release film, and it is difficult to achieve both release properties and wettability to ceramic slurry, etc. on the release layer surface. In other words, if the chemical composition of the release layer is changed to improve wettability, there is a problem of reduced release properties.
[0021] It should be noted that Patent Document 7 proposes a release film that uses an organic solvent-based coating composition to form a release layer. The organic solvent-based coating composition contains polydimethylsiloxane with a vinyl group having a molecular weight of 500 to 30,000 and polydimethylsiloxane with a Si-H group having a molecular weight of 150 to 10,000. However, it does not suggest that the composition can achieve both releasability and wettability. In addition, since the composition belongs to an organic solvent system, it is not suitable for online coating.
[0022] Furthermore, according to the research conducted by the present inventors, it has been found that when a silicone-based release film is recycled and used as a raw material for a base film, foreign matter larger than a specific size may be generated depending on the composition of the release layer, making it unsuitable for recycling.
[0023] According to other studies by the present inventors, when a release layer is formed using a silicone-based aqueous coating composition, the influence of aggregates generated during the application of the release layer on the surface shape is likely to become a problem in terms of thinning of ceramic green sheets and the like.
[0024] Therefore, an object of the present invention is to provide a release film that can easily achieve both releasability and wettability of a release layer and has excellent coating uniformity and recyclability of the release layer.
[0025] Solutions for solving problems
[0026] The present inventors have conducted intensive studies to solve this problem and have found that the above-mentioned problem can be solved by forming a release layer using an aqueous coating composition using silicone having a molecular weight lower than that of conventional silicones, thereby completing the present invention. That is, the present invention includes the following contents.
[0027] [1] A release film comprising a base film and a release layer, wherein the release layer is formed by reacting and curing an aqueous coating composition,
[0028] The aqueous coating composition comprises an alkenyl-containing organosilicon and a Si—H-containing organosilicon, wherein the alkenyl-containing organosilicon has two or more alkenyl groups in the molecule and optionally has SiO 4 / 2 The Q unit shown in FIG. 1 has a number average molecular weight of 1,000 or more and less than 10,000, and the Si-H group-containing silicone has two or more Si-H groups in the molecule and has a number average molecular weight of 1,000 or more and 5,000 or less.
[0029] [2] The release film according to [1], wherein the aqueous coating composition contains a polyvinyl alcohol-based resin.
[0030] [3] The release film according to [2], wherein the polyvinyl alcohol-based resin has a viscosity of 5 mPa·s to 50 mPa·s when a 4 mass % aqueous solution is measured at 20°C, and a saponification degree of 85 mol % to 99 mol %.
[0031] [4] The release film according to any one of [1] to [3], wherein the alkenyl group-containing silicone has SiO 4 / 2 The Q unit shown.
[0032] [5] The release film according to any one of [1] to [4], wherein the alkenyl group-containing silicone is represented by the following general formula (I).
[0033]
[0034] (In the general formula (I), R 1 are optionally the same or different, and are alkenyl groups having 2 to 8 carbon atoms, or monovalent hydrocarbon groups having 1 to 16 carbon atoms including alkyl groups or aryl groups, and [SiO] b1 The silicon atom bonded R 1 At least one of them is an alkenyl group having 2 to 8 carbon atoms; R 2 are optionally the same or different, and are monovalent hydrocarbon groups having 1 to 16 carbon atoms, including alkyl groups or aryl groups; 1 They may be the same or different and are represented by the general formula (Ia).
[0035]
[0036] (In the general formula (Ia), R 1 R of the general formula (I) 1 The same, and R 1 Optional: same or different.)
[0037] Including Y 1 In the general formula (I) as a whole, when all silicon atoms including the terminal are set to 100 mol%, a1 is 50 mol% or more and 98 mol% or less, b1 is 0 mol% or more and 10 mol% or less, c1 is 0 mol% or more and 30 mol% or less, and d1 is 0 mol% or more and 50 mol% or less. 1 In the general formula (I), R 1 Two or more of them are alkenyl groups having 2 or more and 8 or less carbon atoms.)
[0038] [6] The release film according to any one of [1] to [5], wherein the Si-H group-containing silicone is represented by the following general formula (II).
[0039]
[0040] (In the general formula (II), R 3 They are optionally the same or different and are monovalent hydrocarbon groups having 1 to 16 carbon atoms, including alkyl or aryl groups. When a2+b2 is 100 mol%, a2 is 30 mol% to 90 mol%, and b2 is 10 mol% to 70 mol%.
[0041] [7] The release film according to any one of [1] to [6], wherein the aqueous coating composition contains 1 part by mass or more and 50 parts by mass or less of the Si—H group-containing silicone per 100 parts by mass of the alkenyl group-containing silicone.
[0042] [8] The release film according to any one of [1] to [7], wherein the release layer is formed by coating the aqueous coating composition on a substrate film before the crystal orientation is completed, stretching the substrate film in at least one direction, and then performing a heat treatment to complete the crystal orientation.
[0043] [9] The release film according to any one of [1] to [8], wherein the base film is a polyester film.
[0044]
[10] The release film according to any one of [1] to [9], wherein the release film is a release film for a laminated ceramic capacitor or a release film for a resin sheet.
[0045] Effects of the Invention
[0046] According to the present invention, it is possible to provide a release film in which both the releasability and wettability of the release layer can be easily achieved and the coating uniformity and recyclability of the release layer are excellent.
[0047] The detailed reasons for achieving this effect are not clear, but it can be considered that the organosilicon crosslinked body obtained by the reaction of organosilicones with lower molecular weights can easily form a dense three-dimensional structure, so it is easy to maintain hardness even in contact with an organic solvent, and can reduce the adhesion when the laminate coated and cast on the surface of the release layer is peeled off. It can also be considered that the organosilicon crosslinked body with a dense three-dimensional structure is not easy to form a helical structure such as polydimethylsiloxane, which will also affect the surface free energy of the surface of the release layer, and therefore, it is easy to show moderate wettability to the laminate. It can also be considered that when the aqueous coating composition contains a polyvinyl alcohol-based resin, by containing a polyvinyl alcohol-based resin, it is possible to maintain the release layer's releasability and improve its wettability.
[0048] Furthermore, it can be considered that by reducing the molecular weight of the organosilicon contained in the water-based coating composition, the stability and uniformity of the coating film are increased, and it is difficult to generate aggregates in the release layer, thereby improving the coating uniformity. In addition, it can be considered that when the coating film is remelted during reuse, it is easy to disperse each other in the remelted matrix film resin because it is a highly uniform coating film, and thus it is difficult to generate foreign matter.
[0049] It is considered that, in particular, when the alkenyl group-containing silicone has a Q unit, it is easier to form a dense three-dimensional structure, and it is easier to achieve both the releasability and wettability of the release layer. DETAILED DESCRIPTION
[0050] Hereinafter, the present invention will be described in detail.
[0051] [Release film]
[0052] The release film of the present invention comprises a substrate film (hereinafter sometimes referred to as "substrate") and a release layer, wherein the release layer is formed by reacting and curing an aqueous coating composition. As described in detail later, the aqueous coating composition contains two types of silicones that can react with each other, so it is not easy to identify the structure of the obtained polymer and determine the claims based on it, which may be impractical. Therefore, the release film of the present invention is determined in the form of a product claim characterized by a method.
[0053] [Mold release layer]
[0054] The release layer is obtained by reacting and curing the aqueous coating composition. The aqueous coating composition comprises an alkenyl-containing organosilicon and an Si—H-containing organosilicon, wherein the alkenyl-containing organosilicon has two or more alkenyl groups in the molecule and optionally has SiO 4 / 2 The aqueous coating composition contains a Q unit as shown, and the number average molecular weight is greater than 1000 and less than 10000, and the organic silicon containing a Si-H group has two or more Si-H groups in the molecule, and the number average molecular weight is greater than 1000 and less than 5000. In addition, the aqueous coating composition optionally contains a polyvinyl alcohol-based resin. Each constituent component is described in detail below.
[0055] (Silicone containing olefin groups)
[0056] As the alkenyl group-containing organosilicon, there can be used organosilicon having two or more alkenyl groups in the molecule and having SiO 4 / 2 The alkenyl-containing organosilicon of the Q unit shown in the figure and / or the organosilicon having two or more alkenyl groups in the molecule but not having SiO 4 / 2 The Q unit shown is an alkenyl-containing organosilicon.
[0057] As the alkenyl group-containing organosilicon having a Q unit, any organosilicon having two or more alkenyl groups in the molecule and having SiO 4 / 2 The compound having a Q unit as shown and a siloxane bond in the main chain may be any compound, but preferably a polyorganosiloxane having an alkenyl group at the terminal and / or side chain. In addition, from the perspective of easy exfoliation and easy adjustment of the amount of alkenyl groups in one molecule, a copolymer containing a dialkylsiloxane unit or an alkylphenylsiloxane unit is preferred. It is preferred that the silicon atom at the terminal has an alkenyl group, but it may also be a trialkylsilane structure such as trimethylsilane.
[0058] As the alkenyl-containing organosilicon without Q unit, any compound may be used as long as it has two or more alkenyl groups in the molecule and a siloxane bond in the main chain, and polyorganosiloxane having alkenyl groups at the terminal and / or side chain is preferred. In addition, from the perspective of easy exfoliation and easy adjustment of the amount of alkenyl groups in one molecule, a copolymer containing a dialkylsiloxane unit or an alkylphenylsiloxane unit is preferred. It is preferred that the silicon atom at the terminal has an alkenyl group, but it may also be a trialkylsilane structure such as trimethylsilane.
[0059] In any organosilicon containing alkenyl groups, alkenyl groups may be introduced into any of a single terminal, both terminals, or a side chain, preferably at least into any terminal, more preferably into both terminals of the main chain. There are 2 or more alkenyl groups in the molecule, preferably 2 or more and 20 or less, more preferably 2 or more and 10 or less.
[0060] In the case of an alkenyl-containing organosilicon having a Q unit, as SiO 4 / 2 The content of the Q unit shown is preferably 0.5 mol% to 30 mol% when all silicon atoms including the terminal in the molecule are 100 mol%, and more preferably 0.5 mol% to 20 mol%. If the content of the Q unit is 0.5 mol% or more, it is easy to form a dense release layer with high cohesive force, and it is easy to take into account the release property and wettability of the release layer. If the content of the Q unit is 30 mol% or less, it is easy to suppress excessive dense structure and suppress the brittleness of the coating film.
[0061] Examples of the alkenyl group-containing organosilicon include organopolysiloxane represented by the following general formula (I).
[0062]
[0063] (In the general formula (I), R 1 are optionally the same or different, and are alkenyl groups having 2 to 8 carbon atoms, or monovalent hydrocarbon groups having 1 to 16 carbon atoms including alkyl groups or aryl groups, and [SiO] b1 The silicon atom bonded R 1At least one of them is an alkenyl group having 2 to 8 carbon atoms; R 2 are optionally the same or different, and are monovalent hydrocarbon groups having 1 to 16 carbon atoms, including alkyl groups or aryl groups; 1 They may be the same or different and are represented by the general formula (Ia).
[0064]
[0065] (In the general formula (Ia), R 1 R of the general formula (I) 1 The same, and R 1 Optional: same or different.)
[0066] Including Y 1 In the general formula (I) as a whole, when all silicon atoms including the terminal are set to 100 mol%, a1 is 50 mol% or more and 98 mol% or less, b1 is 0 mol% or more and 10 mol% or less, c1 is 0 mol% or more and 30 mol% or less, and d1 is 0 mol% or more and 50 mol% or less. 1 In the general formula (I), R 1 Two or more of them are alkenyl groups having 2 or more and 8 or less carbon atoms.)
[0067] In the general formula (I), when c1 is 0 mol%, that is, in the case of an alkenyl group-containing organosilicon having no Q unit, examples of the alkenyl group-containing organosilicon include organopolysiloxanes represented by the following general formula (I′).
[0068]
[0069] With [SiO] a1 The silicon atom bonded R 2 It may be a monovalent hydrocarbon group including an alkyl group or an aryl group, and is preferably a monovalent hydrocarbon group having 1 to 16 carbon atoms selected from alkyl groups or aryl groups, more preferably a methyl group or a phenyl group, and still more preferably a methyl group.
[0070] With [SiO] b1 The silicon atom bonded R 1 It is an alkenyl group having 2 to 8 carbon atoms, or a monovalent hydrocarbon group containing an alkyl group or an aryl group, and at least one of them may be an alkenyl group having 2 to 8 carbon atoms, and preferably an alkenyl group having 2 to 8 carbon atoms, or a monovalent hydrocarbon group having 1 to 16 carbon atoms selected from an alkyl group or an aryl group. 1 When it is a hydrocarbon group other than an alkenyl group, a methyl group or a phenyl group is more preferred, and a methyl group is further preferred.
[0071] With [SiO] d1The silicon atom bonded R 1 It may be an alkenyl group having 2 to 8 carbon atoms or a monovalent hydrocarbon group including an alkyl group or an aryl group, preferably an alkenyl group having 2 to 8 carbon atoms or a monovalent hydrocarbon group having 1 to 16 carbon atoms selected from an alkyl group or an aryl group, and more preferably a monovalent hydrocarbon group having 1 to 16 carbon atoms selected from an alkyl group or an aryl group. 1 When it is a hydrocarbon group other than an alkenyl group, a methyl group or a phenyl group is more preferred, and a methyl group is further preferred.
[0072] The two ends of the main chain are R 1 Also bonded to [SiO] b1 The R on the silicon atom shown in 1 Similarly, as a preferred structure, an alkenyl group having 2 to 8 carbon atoms is particularly preferred because when the terminal alkenyl group reacts with the Si-H group, steric hindrance is small and the peeling property is easily improved.
[0073] In the general formula (Ia), R bonded to the terminal silicon atom 1 Also bonded to [SiO] b1 The R on the silicon atom shown in 1 Similarly, as a preferred structure, an alkenyl group having 2 to 8 carbon atoms is preferred because the cohesive force of the release layer is improved and the release property of the material through a process such as an organic solvent is improved.
[0074] As R 1 Examples of the alkenyl group having 2 to 8 carbon atoms include vinyl, allyl, butenyl, pentenyl, and hexenyl. Among these, vinyl is particularly preferred.
[0075] Including Y 1 In the whole of the general formula (I), when all silicon atoms including the terminal are set to 100 mol%, a1 is 50 mol% or more and 98 mol% or less, preferably 70 mol% or more and 98 mol% or less. In addition, b1 is 0 mol% or more and 10 mol% or less, preferably 0 mol% or more and 5 mol% or less. c1 is 0.5 mol% or more and 30 mol% or less, preferably 0.5 mol% or more and 20 mol% or less. d1 is 0 mol% or more and 50 mol% or less, preferably 0 mol% or more and 30 mol% or less.
[0076] [SiO] a1 With [SiO] b1 When the total amount of the structural units of [SiO] is 100 mol%, from the viewpoint of localizing the hydrocarbon groups on the coating film surface in order to improve the peeling property, [SiO] a1The content of the structural units is preferably in the range of 90 mol % to 100 mol %, and more preferably in the range of 95 mol % to 100 mol %.
[0077] The number average molecular weight of the alkenyl-containing silicone is preferably 1000 or more and less than 10000, more preferably 3000 or more and less than 10000. If the number average molecular weight is 1000 or more, the hydrocarbon group is easily localized on the surface of the coating film to obtain sufficient peeling properties. On the other hand, if the number average molecular weight is less than 10000, there is a tendency that the emulsification characteristics of the emulsified water-based coating composition become good and the uniform coating property is also good.
[0078] (Silicon containing Si-H group)
[0079] As the organosilicon containing Si-H groups, any compound can be used as long as it has two or more Si-H groups (i.e., two or more hydrogen atoms directly bonded to Si atoms) in the molecule and has a siloxane bond in the main chain, and polyorganosiloxane having Si-H groups in the side chain is preferred. In addition, from the perspective of easy exfoliation and easy adjustment of the amount of Si-H groups in one molecule, a copolymer containing a dialkylsiloxane unit or an alkylphenylsiloxane unit is preferred. The terminal silicon atom may have a Si-H group, and preferably a trialkylsilane structure such as trimethylsilane.
[0080] Examples of the Si-H group-containing organosilicon include organohydrogenpolysiloxane represented by the following general formula (II).
[0081]
[0082] (In the general formula (II), R 3 They are optionally the same or different and are monovalent hydrocarbon groups having 1 to 16 carbon atoms, including alkyl or aryl groups. When a2+b2 is 100 mol%, a2 is 30 mol% to 90 mol%, and b2 is 10 mol% to 70 mol%.
[0083] As long as [SiO] a2 A hydrogen atom (hydrogen radical) is bonded to the silicon atom shown in 3 It may be a monovalent hydrocarbon group including an alkyl group or an aryl group, and is preferably a monovalent hydrocarbon group having 1 to 16 carbon atoms selected from alkyl groups or aryl groups.
[0084] With [SiO] b2 R bonded to the terminal Si atom 3 It may be a monovalent hydrocarbon group including an alkyl group or an aryl group, and is preferably a monovalent hydrocarbon group having 1 to 16 carbon atoms selected from alkyl groups or aryl groups.
[0085] About any R3 , more preferably, the case where the number of carbon atoms of the alkyl or aryl group is smaller, the stereo hindrance is smaller, and the cross-linking reaction is easy to proceed. In addition, it is also preferred from the viewpoint of fluidity and uniformity of the reaction structure in the release layer. Therefore, as the alkyl group, methyl, ethyl, propyl, butyl, etc. are preferred, and as the aryl group, phenyl, tolyl, etc. are preferred.
[0086] If [SiO] a2 With [SiO] b2 The total amount of the structural units is 100 mol %, and as [SiO] a2 The range of the structural unit is preferably 30 mol% or more and 90 mol% or less, and more preferably 40 mol% or more and 80 mol% or less. If [SiO] a2 The structural unit of [SiO] is 30 mol% or more, so that the crosslinking reaction sites become sufficient, the cohesive force of the release layer becomes large, and the scratch resistance and solvent resistance of the release layer are also good, so it is preferred. a2 The structural unit of is preferably 90 mol % or less because Si—H groups are less likely to remain in the release layer, the activity of the release layer surface is less likely to increase, and good releasability is maintained.
[0087] The number average molecular weight of the Si-H group-containing silicone in the present invention is preferably 1000 or more and 5000 or less, and more preferably 3000 or more and 5000 or less. If the number average molecular weight is 1000 or more, sufficient peeling properties are easily obtained. On the other hand, if the number average molecular weight is 5000 or less, there is a tendency that the emulsification characteristics of the emulsified aqueous coating composition become good and the coating uniformity also becomes good. In addition, the cross-linking reaction is easy to proceed effectively, the residual Si-H groups in the release layer decrease, and the peeling properties become good.
[0088] In the aqueous coating composition, relative to 100 parts by mass of the organosilicon containing alkenyl, it is preferred to include more than 1 part by mass and less than 50 parts by mass of the organosilicon containing Si-H groups, more preferably more than 2 parts by mass and less than 40 parts by mass, and further preferably more than 3 parts by mass and less than 30 parts by mass. If the content of the organosilicon containing Si-H groups is more than 1 part by mass, the crosslinking reaction sites become sufficient, it is easy to form a dense crosslinking structure, and the release layer property is improved, so it is preferred. If the content of the organosilicon containing Si-H groups reaches less than 50 parts by mass, the Si-H groups in the release layer are not easy to remain, the activity of the surface of the release layer is not easy to rise, and the stripping property is well maintained, so it is preferred.
[0089] (Polyvinyl alcohol resin)
[0090] The aqueous coating composition may contain a polyvinyl alcohol resin. As such a polyvinyl alcohol resin, polyvinyl alcohol or a copolymer thereof may be used. As polyvinyl alcohol copolymers, examples include vinyl alcohol-vinyl acetate copolymers, vinyl alcohol-vinyl butyral copolymers, ethylene-vinyl alcohol copolymers, polyvinyl alcohol polymers having a silyl group in the molecule, etc. Among these, preferred vinyl alcohol-vinyl acetate copolymers and ethylene-vinyl alcohol copolymers are preferred. When the polyvinyl alcohol resin is a copolymer, the repeating unit derived from vinyl alcohol is preferably 70 mol % or more and 100 mol % or less, more preferably 85 mol % or more and 99 mol % or less.
[0091] The degree of polymerization of the polyvinyl alcohol-based resin in the present invention can be expressed by the viscosity of a 4% by mass aqueous solution at 20°C, and the viscosity is preferably 5 mPa·s or more and 50 mPa·s or less. If the viscosity is within the aforementioned numerical range, the miscibility in the aqueous coating composition is high, and a more uniform release layer is easily obtained. In other words, if the viscosity is 5 mPa·s or more, it is not easy to flow in the coating film after the release layer is formed, and it is not easy to reduce the release properties, so it is preferred. If the viscosity is 50 mPa·s or less, the viscosity of the aqueous coating composition as a whole is not easy to increase, and it is easy to apply uniformly, so it is preferred.
[0092] In addition, the polyvinyl alcohol-based resin may be mixed with the silicone before emulsification and may be used as an emulsifier.
[0093] Generally, polyvinyl alcohol is obtained by polymerizing vinyl acetate to form polyvinyl acetate, and then saponifying it, and the amount of saponification is expressed by the degree of saponification. In the present invention, the degree of saponification of the polyvinyl alcohol-based resin is preferably 85 mol% or more and 99 mol% or less. If the degree of saponification is within the aforementioned numerical range, the miscibility in the aqueous coating composition is high, and a more uniform release layer is easily obtained. In particular, if the degree of saponification is 85 mol% or more, the adhesion with the substrate is improved, and the miscibility with silicone is also good. If the degree of saponification is 99% or less, the hydrophilicity of the release layer will not become too high, it is easy to maintain the cohesive force of the release layer coating, and it is not easy for the adhesion of the release layer to deteriorate.
[0094] As the polyvinyl alcohol-based resin, a commercially available product may be used as it is. Specific examples of the commercially available product include POVAL manufactured by Kuraray Co., Ltd. and GOHSENOL manufactured by Mitsubishi Chemical Corporation.
[0095] In the release layer of the present invention, when the aqueous coating composition contains a polyvinyl alcohol resin, it is preferably contained in an amount of 20% by mass or less of the polyvinyl alcohol resin based on the release layer. As a more preferred range, it is 1% by mass or more and 15% by mass or less, and as a further preferred range, it is 1% by mass or more and 10% by mass or less. If the content of the polyvinyl alcohol resin is within the aforementioned numerical range, it is more suitable to take into account the two characteristics of miscibility with silicone and adhesion between the substrate and the release layer. In other words, if the content of the polyvinyl alcohol resin in the release layer is 1% by mass or more, the stability of the silicone emulsion in the coating liquid is easy to be good, and if it is 20% by mass or less, the release property is not easy to reduce.
[0096] (Platinum catalyst)
[0097] The cross-linking reaction between the alkenyl group-containing organosilicon and the Si—H group-containing organosilicon is an addition reaction, and in one embodiment, a platinum-based catalyst is preferably used to promote the reaction.
[0098] As the platinum-based catalyst, a known catalyst can be used, for example, platinum chloride and chloroplatinic acid. In consideration of dispersibility in silicone, the platinum-based catalyst can be 1,3-divinyl-1,1,3,3-tetramethyldisiloxane platinum (0) complex (Cast catalyst), and uniform dispersibility can be ensured by dispersing it at the same time as emulsifying the silicone.
[0099] Regarding the content of the platinum-based catalyst, it is preferably contained in a range of 10 ppm or more and 400 ppm or less relative to the total mass of the organosilicon containing alkenyl groups and the organosilicon containing Si-H groups. By setting it to such a range, the curing of the organosilicon can be fully carried out, and the generation of organosilicon aggregates can be suppressed, and a release film with excellent surface properties can be obtained. If the mass ratio of the platinum element is below the upper limit, the addition reaction of the alkenyl group and the Si-H group becomes moderate, and there is a tendency to suppress the generation of organosilicon aggregates. From this viewpoint, the content of the platinum-based catalyst is more preferably less than 300 ppm, and more preferably less than 200 ppm. In addition, if the mass ratio of the platinum element is above the lower limit, the addition reaction is fully carried out, and it is difficult to cause poor curing of the organosilicon. From this viewpoint, the content of the platinum catalyst is more preferably more than 15 ppm, and more preferably more than 20 ppm.
[0100] (Water-based solvent)
[0101] The aqueous coating composition generally contains an aqueous solvent in addition to the alkenyl-containing organosilicon and the Si-H-containing organosilicon. As the aqueous solvent, an aqueous solvent containing water is preferably used. In one embodiment, the aqueous dispersion of the alkenyl-containing organosilicon and the aqueous dispersion of the Si-H-containing organosilicon are used to prepare the aqueous coating composition. As the aqueous dispersion of each organosilicon, an aqueous emulsion is preferably used.
[0102] The release layer is formed from such an aqueous emulsion, and is formed by applying an aqueous coating composition containing the aqueous emulsion (hereinafter sometimes referred to as "aqueous coating liquid"). The aqueous coating liquid uses an aqueous solvent, and can form a release layer without using explosion-proof equipment and recovery equipment required for organic solvents in the film forming process. A small amount of organic solvent may be contained as needed.
[0103] (Other ingredients)
[0104] In one embodiment, other additives such as surfactants, coupling agents, crosslinking reaction inhibitors, antistatic agents, ultraviolet absorbers, pigments, colorants, organic or inorganic particles, lubricants, anti-blocking agents, etc. can be mixed into the aqueous coating composition within a range that does not impair the effects of the invention.
[0105] (Surfactant)
[0106] In one embodiment, in order to promote wetting of the substrate film when the release layer is provided, a surfactant is preferably added to the aqueous coating composition. As the surfactant, anionic surfactants, cationic surfactants, nonionic surfactants, etc. can be listed, and one or more of them can also be used. In order to prevent the aggregation of various silicone aqueous emulsions and not affect the curing reaction of silicone, a nonionic surfactant is preferably used as an emulsifier.
[0107] As the nonionic surfactant, the HLB value is preferably in the range of 6 or more and 18 or less, and examples thereof include at least one selected from alkylene oxide adducts such as alkylene oxide adducts of higher alcohols and / or higher fatty acids, esters of alkylene oxide adducts of higher fatty acids and alcohols, alkylene oxide adducts of alkanolamides, alkylene oxide adducts of sorbitan esters, and alkylene oxide adducts of higher fatty acid glycerides. Here, the HLB value is a value calculated by Griffin's calculation formula.
[0108] As alkylene oxides, ethylene oxide, propylene oxide, and butylene oxide can be listed. One of these can be used, or multiple can be used. When multiple types are used, they can be block or random addition forms, but the HLB value is preferably in the range of 8 or more and 18 or less, and more preferably in the range of 10 or more and 15 or less. Among these nonionic surfactants, polyoxyethylene lauryl ether, polyoxyethylene tridecyl ether, etc. can be preferably listed. As needed, two or more nonionic surfactants can be mixed. If a nonionic surfactant whose HLB value deviates from this range is used as an emulsifier for an organosilicon aqueous dispersion, the emulsifying dispersion power and the stability of the aqueous dispersion are sometimes reduced.
[0109] The surfactant is preferably used in a range of 0.1% to 20% by mass relative to the total solid content, more preferably in a range of 0.2% to 15% by mass, and further preferably in a range of 0.5% to 10% by mass. If it is above the lower limit of the range, the emulsified state becomes good, and if it is below the upper limit of the range, it is not easy to cause re-peeling.
[0110] (Cross-linking Reaction Inhibitor)
[0111] In one embodiment, in order to suppress the activity of the platinum catalyst at room temperature in the state of the aqueous coating liquid, a reaction inhibitor is preferably contained. The reaction inhibitor is preferably a reaction inhibitor with an alkynyl group. As a reaction inhibitor with an alkynyl group, as long as there is an alkynyl group, there is no particular limitation, specifically, 1-ethynyl-1-cyclohexanol, 4-ethyl-1-octyne-3-ol, 3-methyl-1-dodecyne-3-ol, 3,7,11-trimethyl-1-dodecyne-3-ol, 1,1-diphenyl-2-propyne-3-ol, 3-ethyl-6-ethyl-1-nonyne-3-ol, 3-methyl-1-pentadecane-3-ol, 2,5-dimethyl-3-hexyne-2,5-diol, 3-phenyl-1-butyne-3-ol can be exemplified. In the present invention, since it is an aqueous coating liquid, it is preferred to use the reaction inhibitor with an alkynyl group and a hydroxyl group illustrated from the balance of affinity solubility in water and coordination ability for platinum and boiling point. Alternatively, the platinum-based catalyst may be mixed with a general organopolysiloxane to be added to the aqueous coating liquid and used in the form of an aqueous emulsion.
[0112] The content of the crosslinking reaction inhibitor is preferably 5 ppm or more and 1000 ppm or less relative to the mass of the aqueous coating composition for forming the release layer, more preferably 10 ppm or more and 700 ppm or less, and further preferably 20 ppm or more and 500 ppm or less. When the content of the crosslinking reaction inhibitor is above the lower limit, there is a tendency that the storage period becomes longer, the addition curing reaction of the silicone is difficult to proceed at room temperature, and silicone aggregates are not easily generated. In addition, if the content of the crosslinking reaction inhibitor is below the upper limit, after the object material is peeled off, the silicone is not easily transferred to the object material, and the amount of the reaction inhibitor volatilized during the heat treatment is reduced, so it is not easy to cause contamination inside the oven.
[0113] (Coupling agent)
[0114] In one embodiment, a coupling agent may be added to the aqueous coating composition to improve the adhesion between the organosilicon component and the substrate film. The coupling agent may be, for example, a compound represented by the general formula YRSiX3, for example, a silane coupling agent. Here, Y is an organic functional group such as a vinyl group, an epoxy group, an amino group, a thiol group, etc., and Y is particularly preferably an epoxy group or a vinyl group.
[0115] R is an alkylene group such as methylene, ethylene, or propylene, or a single bond. X is a hydrolyzable group such as methoxy, ethoxy, or acetoxy, or an alkyl group, and at least one of the three Xs is a hydrolyzable group, and preferably all three Xs are hydrolyzable groups. As the hydrolyzable group, a methoxy group is preferred.
[0116] Preferred silane coupling agents include 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, vinyltriethoxysilane, vinyltriacetoxysilane, vinyltrimethoxysilane, vinyltri(2-methoxyethoxy)silane, and vinylmethyldimethoxysilane.
[0117] Other examples of coupling agents include organometallic compounds containing metals such as zirconium, titanium, and aluminum. The organometallic compounds are preferably classified as alkoxides, chelates, and acylates. Specific examples include zirconium tetraacetylacetonate, zirconium acetate, titanium acetylacetonate, triethanolamine titanate, and titanium lactate, but are not limited thereto.
[0118] Furthermore, as the coupling agent, two or more coupling agents may be used in combination, such as a silane coupling agent in which Y is an epoxy group and a silane coupling agent in which Y is a vinyl group.
[0119] In one embodiment, by adding a coupling agent, the durable adhesion between silicone as the main component of the release layer and polyester film is improved. For example, when casting a resin sheet by a solution casting method using an organic solvent, the organic solvent component sometimes penetrates into the release layer, and the release layer may be corroded, but the corrosion can be suppressed by adding a coupling agent. When casting a resin sheet by a melt casting method at high temperature, the release layer is exposed to high temperature and may be thermally degraded, but by adding a coupling agent, thermal degradation can be suppressed and the release layer can be maintained.
[0120] From the above viewpoints, the content of the coupling agent is preferably 0.1 parts by mass or more and 20 parts by mass or less, and more preferably 1 part by mass or more and 10 parts by mass or less, relative to 100 parts by mass of the total of the alkenyl group-containing silicone and the Si—H group-containing silicone contained in the release layer.
[0121] (Preparation of Silicone Aqueous Dispersion)
[0122] In one embodiment, the preparation of the aqueous emulsion can be listed as a method of using a predetermined alkenyl-containing silicone or Si-H-containing silicone, an aqueous solvent and a surfactant and emulsifying them. These components can be emulsified using a known method, for example, the following method can be listed: a method of mechanically emulsifying the predetermined silicone, surfactant and other components as required prepared in advance in an aqueous medium using a stirring device such as a homogenizer, a vacuum emulsifier (AGI HOMO MIXER), a super planetary stirrer, etc.
[0123] In addition, the particle size of the aqueous dispersion can be adjusted by adjusting the size of the stirring blade, the stirring speed and the stirring time. The average particle size of the dispersed particles of each silicone aqueous dispersion is preferably 200 nm or less, more preferably 100 nm or more and 200 nm or less.
[0124] [Base film]
[0125] The substrate film in the present invention is not particularly limited, and examples thereof include sheets or films formed of polyesters such as polyethylene terephthalate and polyethylene naphthalate, polyolefins such as polycarbonate, polyethylene and polypropylene, polystyrene triacetate, acrylics, polyimides, etc. Among them, films formed of polyesters are preferred from the viewpoint of excellent mechanical properties and heat resistance and a good balance between these properties and price. Hereinafter, the case of a polyester film will be described as an example, but in the case of using other resin films, the copolymer components, blending components, additives, film preparation methods, laminated structures, etc. are the same as follows.
[0126] (Polyester film)
[0127] The polyester constituting the polyester film used as a substrate film is not particularly limited, and a polyester generally used as a substrate for a release film can be used to form a film. Preferably, it is a crystalline linear saturated polyester formed by an aromatic dibasic acid component and a diol component, and more preferably, for example, polyethylene terephthalate, polyethylene 2,6-naphthalate, polybutylene terephthalate, poly(1,3-propylene terephthalate), or a copolymer with the constituent components of these resins as the main component. In particular, it is particularly suitable for a polyester film formed by polyethylene terephthalate. In polyethylene terephthalate, the repeating unit of ethylene terephthalate is preferably 90 mol% or more, more preferably 95 mol% or more, and other dicarboxylic acid components and diol components may also be copolymerized in small amounts. For example, from the viewpoint of cost, it is preferably manufactured only from terephthalic acid and ethylene glycol. Furthermore, known additives such as antioxidants, light stabilizers, ultraviolet absorbers, crystallizing agents, etc. may be added within the range not impairing the effects of the release film of the present invention. The polyester film is preferably a biaxially oriented polyester film because of its high elastic modulus in both directions.
[0128] The intrinsic viscosity of the polyester film is preferably 0.50 dl / g or more and 0.70 dl / g or less, and more preferably 0.52 dl / g or more and 0.62 dl / g or less. When the intrinsic viscosity is 0.50 dl / g or more, a large amount of breakage will not occur during the stretching process, so it is preferred. On the contrary, when it is 0.70 dl / g or less, the cutting property when cutting into a prescribed product width is good, and dimensional defects will not occur, so it is preferred. In addition, the raw material pellets are preferably fully vacuum dried.
[0129] In addition, when it is simply referred to as "polyester film" in this specification, it means a polyester film which has a surface layer A and a surface layer B (laminated).
[0130] The method for producing the polyester film of the present invention is not particularly limited, and a conventionally commonly used method can be used. For example, the polyester can be melted and extruded into a film in an extruder, and cooled in a rotating cooling drum to obtain an unstretched film, and the unstretched film can be biaxially stretched to obtain the film. The biaxially stretched film can be obtained by a method in which a uniaxially stretched film in the longitudinal or transverse direction is biaxially stretched successively in the transverse direction or longitudinal direction, or by a method in which an unstretched film is biaxially stretched simultaneously in the longitudinal and transverse directions.
[0131] In the present invention, the stretching temperature during stretching of the polyester film is preferably set to be equal to or higher than the secondary phase transition point (Tg) of the polyester. The film is preferably stretched 1 to 8 times in each of the longitudinal and transverse directions, and particularly preferably stretched 2 to 6 times.
[0132] The thickness of the polyester film is preferably 12 μm or more and 50 μm or less, more preferably 15 μm or more and 38 μm or less, and even more preferably 19 μm or more and 33 μm or less. If the thickness of the film is 12 μm or more, there is no need to worry about deformation due to heat during film production, processing, and molding, so it is preferred. On the other hand, if the thickness of the film is 50 μm or less, the amount of film discarded after use will not become extremely large, reducing the environmental burden, so it is preferred.
[0133] The polyester film substrate may be a single layer or a multilayer of two or more layers. For example, the substrate film may be a polyester film having a surface layer A substantially free of particles having a particle size of 1.0 μm or more and a surface layer B containing particles. The surface layer A preferably substantially does not contain inorganic particles having a particle size of 1.0 μm or more.
[0134] In this embodiment, particles having a particle size of less than 1.0 μm and 1 nm or more may be present in the surface layer A. By making the surface layer A substantially free of particles having a particle size of 1.0 μm or more, such as inorganic particles, the phenomenon of the particle shape in the substrate being transferred to the resin sheet and causing problems can be reduced.
[0135] In one embodiment, by making the surface layer A also contain no particles having a particle diameter of less than 1.0 μm, it is possible to more effectively suppress the phenomenon in which the particle shape in the substrate is transferred to the resin sheet and causes a problem.
[0136] In one embodiment, the polyester film substrate is preferably a laminated film having a surface layer A substantially free of inorganic particles on at least one side. Thus, it is possible to further effectively suppress the phenomenon that the particle shape in the substrate is transferred to the resin sheet and causes adverse conditions. For example, it is preferred that the surface layer A substantially free of particles having a particle size of less than 1.0 μm also substantially free of particles having a particle size of 1.0 μm or more.
[0137] Here, in the present invention, "substantially free of particles" means that, for example, in the case of inorganic particles smaller than 1.0 μm, when the inorganic elements are quantified by fluorescent X-ray analysis, the content is 50 ppm or less, preferably 10 ppm or less, and most preferably below the detection limit. This is because, even if particles are not actively added to the film, sometimes contamination components from foreign matter, dirt attached to the production line or equipment in the raw resin or film manufacturing process will peel off and mix into the film. In addition, "substantially free of particles with a particle size of 1.0 μm or more" means that particles with a particle size of 1.0 μm or more are not actively included.
[0138] In the case of a laminated polyester film having a multilayer structure of two or more layers, it is preferred that a surface layer B containing inorganic particles and the like is provided on the opposite side of a surface layer A containing substantially no inorganic particles.
[0139] As a stacked structure, if the layer on one side of the coating release layer is set to the A layer, the layer on its opposite side is set to the B layer, and the core layer other than them is set to the C layer, the layer structure in the thickness direction can list the stacked structures such as release layer / A / B or release layer / A / C / B. Of course, the C layer can also be a plurality of layers. In addition, the surface layer B also can not contain inorganic particles. In this case, in order to give the slipperiness for winding the film into a roll, it is preferred that a coating layer at least comprising inorganic particles and a binder is provided on the surface layer B.
[0140] In the polyester film substrate of the present invention, from the viewpoint of the slipperiness of the film and the ease of air removal, the surface layer B forming the surface opposite to the surface on which the release layer is applied preferably contains inorganic particles, and silicon dioxide particles and / or calcium carbonate particles are particularly preferably used. The content of the inorganic particles contained in the surface layer B is preferably 5000 ppm or more and 15000 ppm or less based on the total amount of the inorganic particles.
[0141] At this time, the regional surface average roughness (Sa) of the film of surface layer B is preferably in the range of more than 1nm and less than 40nm. More preferably, it is in the range of more than 5nm and less than 35nm. When the total of silicon dioxide particles and / or calcium carbonate particles is more than 5000ppm and Sa is more than 1nm, when the film is rolled into a roll, air can be uniformly dispersed, and the roll has good appearance and good planarity, so it is suitable for manufacturing ultra-thin layer ceramic green sheets. In addition, when the total of silicon dioxide particles and / or calcium carbonate particles is less than 15000ppm and Sa is less than 40nm, it is not easy to gather lubricants, and coarse protrusions will not be formed. Therefore, when manufacturing ultra-thin layer ceramic green sheets, the quality is stable, so it is preferred.
[0142] As the particles contained in the above-mentioned B layer, in addition to using silicon dioxide and / or calcium carbonate, inactive inorganic particles and / or heat-resistant organic particles, etc. can also be used. From the viewpoint of transparency and cost, silicon dioxide particles and / or calcium carbonate particles are more preferably used. In addition, as other inorganic particles that can be used, aluminum oxide-silicon dioxide composite oxide particles, hydroxyapatite particles, etc. can be listed. In addition, as heat-resistant organic particles, cross-linked polyacrylic acid particles, cross-linked polystyrene particles, benzoguanamine particles, etc. can be listed. In addition, when using silicon dioxide particles, porous colloidal silica is preferred, and when using calcium carbonate particles, from the viewpoint of preventing the lubricant from falling off, it is preferred to utilize polyacrylic acid polymer compounds to implement surface-treated light calcium carbonate.
[0143] The average particle size of the inorganic particles added to the surface layer B is preferably 0.1 μm or more and 2.0 μm or less, and particularly preferably 0.5 μm or more and 1.0 μm or less. If the average particle size of the inorganic particles is 0.1 μm or more, the slip property of the release film is good, so it is preferred. In addition, if the average particle size is 2.0 μm or less, there is no concern about adverse effects on the smoothness of the release layer surface, and therefore, there is no concern about pinholes in the ceramic green sheet, so it is preferred.
[0144] From the viewpoint of reducing pinholes, it is preferred that no recycled raw materials be used for the layer on the side where the release layer is provided, that is, the surface layer A, in order to prevent the incorporation of inorganic particles such as lubricants.
[0145] The thickness ratio of the layer on the side of the release layer, i.e., the surface layer A, is preferably 20% or more and 50% or less of the thickness of all layers of the base film. If it is 20% or more, it is not easy to be affected by particles contained in the surface layer B etc. from the inside of the film, and the regional surface average roughness Sa is easy to meet the above range, so it is preferred. If it is 50% or less of the thickness of all layers of the base film, the use ratio of recycled raw materials in the surface layer B can be increased, and the environmental burden is small, so it is preferred.
[0146] In addition, from the viewpoint of economic efficiency, the layer other than the surface layer A (surface layer B or the intermediate layer C) may use 50% by mass or more and 90% by mass or less of recycled raw materials of film scraps or plastic bottles. In this case, the type, amount, particle size and regional surface average roughness (Sa) of the lubricant contained in the B layer preferably also meet the above ranges.
[0147] In addition, in order to improve the adhesion of the release layer applied later or prevent static electricity, a coating layer may be provided on the surface of the surface layer A and / or the surface layer B before stretching in the film forming process or after uniaxial stretching, or a surface treatment may be performed.
[0148] In one embodiment, in order to improve the adhesion with the release layer, the release layer forming surface coated with the aqueous coating composition can be surface treated or an easy-adhesion layer can be provided. As surface treatment, plasma treatment, corona discharge treatment, ultraviolet treatment, flame treatment and electron beam / radiation treatment can be listed, and as an easy-adhesion layer, a layer containing the same resin as the substrate film, and then containing an antistatic agent, a pigment, a surfactant, a lubricant, an anti-blocking agent, etc. can be listed. When the aqueous coating composition is added with an adhesion improver such as a coupling agent, even if an easy-adhesion layer is not provided, the release layer can also have sufficient adhesion to the substrate film.
[0149] [Formation of Release Layer]
[0150] In one embodiment, the release layer is formed by applying an aqueous coating composition comprising an aqueous emulsion of an alkenyl-containing silicone and an aqueous emulsion of an Si-H-containing silicone. In this case, the release layer is formed on at least one surface of the substrate film. The release layer is formed by applying the aqueous coating liquid on the substrate film, heating / drying the aqueous coating liquid, and reacting and curing the components of the aqueous coating liquid to form the release layer. The release layer is preferably formed in the film forming step.
[0151] The thickness of the release layer is preferably 5 nm or more and 100 nm or less in terms of thickness after drying. If the thickness of the release layer is above the lower limit, it is easy to obtain sufficient peelability. If it is below the upper limit, there is a tendency that the peel strength is not easy to increase, and there is also a tendency that it is easy to apply without making the release layer component of the water-based coating liquid present a high concentration or increasing the coating amount. Therefore, the thickness of the release layer is more preferably 5 nm or more and 70 nm or less, and further preferably 5 nm or more and 50 nm or less.
[0152] When the water-based coating liquid is applied to the substrate film, the solid content concentration is preferably 20% by mass or less, more preferably 1% by mass or more and 10% by mass or less, based on the release layer component in the water-based coating liquid. If the solid content concentration of the release layer component in the water-based coating liquid is above the lower limit, there is a tendency that the film-forming property becomes good. In addition, if the solid content concentration is below the upper limit, the stability of the water-based coating liquid and the appearance of the release layer tend to become good. As an aqueous solvent for adjusting the solid content concentration, water is preferably used.
[0153] The aqueous coating liquid applied to the substrate film to form the release layer can be applied at any stage, but is preferably applied during the production process of the polyester film, and more preferably applied to the polyester film before the orientation crystallization is completed. Thereafter, after stretching in at least one direction, heat treatment can be performed to complete the crystal orientation.
[0154] Here, the polyester film before the completion of crystal orientation includes: an unstretched film; a uniaxially oriented film obtained by orienting the unstretched film along either the longitudinal direction (hereinafter sometimes referred to as the film continuous film forming direction, the length direction, or the MD direction) or the transverse direction (hereinafter sometimes referred to as the direction orthogonal to the longitudinal direction, the width direction, or the TD direction); a film obtained by further stretching and orienting the unstretched film at a low ratio along both the longitudinal and transverse directions (a biaxially stretched film before the orientation crystallization is finally completed by re-stretching along the longitudinal or transverse direction), etc.
[0155] Among them, it is preferred that a water-based coating liquid is applied to an unstretched film or a uniaxially stretched film obtained by orientation in one direction, and the so-called online coating is directly performed by longitudinal stretching and / or transverse stretching and heat fixing. The release layer can be dried by a stretching process or a heat fixing treatment after coating, and a drying process can be added as needed. In addition, when a catalyst is used to cure the composition to obtain a cured film, it can be cured by a stretching process or a heat fixing treatment, and a curing process can be further added as needed.
[0156] When applying the water-based coating liquid to the polyester film, it is preferred that: as a pretreatment for improving the coating properties, the film surface is subjected to a physical treatment such as corona surface treatment, flame treatment, plasma treatment, etc.; or, the aforementioned emulsifier is combined with the composition and used as a wetting agent; a surfactant is additionally added as a wetting agent.
[0157] As the coating method, any known coating method can be applied, and for example, roll coating, gravure coating, roll brush coating, spray coating, air knife coating, impregnation, curtain coating, etc. can be used alone or in combination.
[0158] [Properties of release film]
[0159] In the present invention, the surface free energy of the release layer in the test method described later is preferably in the range of 10mN / m or more and 40mN / m or less, more preferably in the range of 12mN / m or more and 38mN / m or less, further preferably in the range of 14mN / m or more and 36mN / m or less, and particularly preferably in the range of 15mN / m or more and 35mN / m or more. If the surface free energy of the release layer is below the upper limit, the adhesion is reduced and it is not easy to be re-stripped. In addition, if it is above the lower limit, it is not easy to produce defects caused by the repulsion of the processing layer such as the ceramic sheet and the resin sheet coated on the surface of the release layer, and it is not easy to produce pinhole defects.
[0160] [use]
[0161] The release film of the present invention can be used as a process film used in manufacturing a laminated ceramic capacitor, casting a resin sheet, etc. In particular, even if a thin film resin sheet having a thickness of 1 μm or less after drying is produced, the wettability is good, so that pinholes in the processing layer are reduced. For example, when used as a release film for green sheet production, the defect rate of thin-walled laminated ceramic capacitors can be reduced.
[0162] Example
[0163] The present invention will be described in more detail below with reference to Examples and Comparative Examples, but the present invention is not limited to the following Examples. The evaluation methods of physical properties and the like in the following Examples are as follows.
[0164] (1) Coating uniformity of release layer
[0165] The release film was cut into A4 sheets, and the release layer was visually observed using a fluorescent lamp or a halogen lamp. The number of aggregated coating defects (number per A4 sheet) was compared and evaluated based on the following criteria.
[0166] ◎: No coating defects
[0167] ○: 1 to 2 coating defects
[0168] △: 3 to 5 coating defects
[0169] ×: There are 6 or more coating defects
[0170] (2) Surface free energy of release layer
[0171] For the sample humidified at 23°C and 50% RH for 24 hours, a contact angle meter (DMo-501 manufactured by Kyowa Interface Science Co., Ltd.) was used to measure the static contact angle when water was dropped and allowed to stand for 30 seconds. The static contact angles of ethylene glycol and diiodomethane were measured in the same manner, and the surface tension components of the following liquids were used to establish the following simultaneous equations related to the surface tension components of the release layer (the respective measurement liquids of water, ethylene glycol, and diiodomethane were set as 1, 2, and 3, γLD represents the dispersion force component of the liquid, γLP represents the polar force component of the liquid, γLH represents the hydrogen bonding component of the liquid, γL represents the total value of the surface tension components in the liquid, and γSD represents the dispersion force component of the release layer, γSP represents the polar force component of the release layer, and γSH represents the hydrogen bonding component of the release layer. In addition, θ represents the contact angle.).
[0172] (γSD·γLD1) 1 / 2 +(γSP·γLP1) 1 / 2 +(γSH·γLH1) 1 / 2 =γL1(1+cosθ1) / 2
[0173] (γSD·γLD2) 1 / 2 +(γSP·γLP2) 1 / 2 +(γSH·γLH2) 1 / 2 =γL2(1+cosθ2) / 2
[0174] (γSD·γLD3) 1 / 2 +(γSP·γLP3) 1 / 2 +(γSH·γLH3) 1 / 2 =γL3(1+cosθ3) / 2
[0175] It should be noted that γLD, γLP, γLH, and γL of water, ethylene glycol, and diiodomethane are as shown in Table 1.
[0176] [Table 1]
[0177]
[0178] Next, the surface free energy γS of the release layer surface is calculated using the following formula from the numerical values of γSD, γSP, and γSH obtained as described above.
[0179] γS=γSD+γSP+γSH
[0180] (3) Dirt test of release layer (friction resistance)
[0181] The release surface of the release film was scratched once with an index finger at a load of about 500 gf, and the whitening state of the release layer surface was visually observed and evaluated according to the following criteria.
[0182] ○: No change
[0183] △: Slightly whitened
[0184] ×: Whitening
[0185] (4) Scratch test of release layer (adhesion)
[0186] The release surface of the release film was scratched 10 times with the thumb at a load of about 500 gf. In order to confirm the fall-off of the silicone in this part, an adhesive tape (manufactured by Nitto Denko Corporation, trade name "31BTAPE") was attached, the peeling state of the adhesive tape was confirmed, and evaluation was performed according to the following criteria.
[0187] ○: No peeling change when the adhesive tape is peeled off
[0188] △: When the adhesive tape is peeled off, there is a slight change in peeling
[0189] ×: When the adhesive tape is peeled off, there is a peeling change
[0190] (5) Ceramic sheet peelability
[0191] 100 parts by mass of barium titanate (BaTiO3, manufactured by KCM Corporation), 7 parts by mass of polyvinyl butyral (manufactured by Sekisui Chemical Co., Ltd.), 3 parts by mass of dioctyl phthalate, and 3 parts by mass of a dispersant (DISPERBYK-103, manufactured by BYK-Chemie) were added to a mixed solvent of toluene:ethanol=1:1 (volume ratio), and dispersed in a ball mill to prepare a slurry. The slurry was uniformly applied to the release layer of the release film in a manner to have a thickness of 2 μm after drying, and then dried to form a ceramic sheet. The release film formed with the ceramic sheet was cut into 25 mm×150 mm, and an adhesive tape (manufactured by Nitto Denko Corporation, trade name "31B TAPE") was attached to the ceramic sheet side to prepare a test piece. The test piece was humidified at 23°C and 50% humidity for 24 hours, and then the ceramic piece was peeled off using a tensile tester at a peeling angle of 180° and a peeling speed of 300 mm / min to measure the peel strength. The peel strength of the ceramic piece was judged based on the following indicators.
[0192] ◎: Peel strength less than 1g / 25mm
[0193] ○: Peel strength is 1 g / 25 mm or more and less than 3 g / 25 mm
[0194] △: Peel strength is 3 g / 25 mm or more and 12 g / 25 mm or less
[0195] ×: The peel strength exceeds 12 g / 25 mm or the ceramic sheet is broken.
[0196] (6) Recyclability evaluation
[0197] Regarding the recyclability, the size and number of foreign matter contained in the film were magnified 20 times by transmission illumination using a universal projector, and the number of foreign matter with a maximum diameter of 50 μm or more was counted. The measurement area was set to 0.05 m 2 .
[0198] ◎: The number of foreign objects is less than 10 / 0.05m 2 , there is no problem in using.
[0199] ○: Number of foreign objects is 10 / 0.05m 2 More than but less than 30 / 0.05m 2 , which slightly affects the flatness, but there is no problem in use.
[0200] △: The number of foreign objects is 30 / 0.05m 2 More than but less than 100 / 0.05m 2 , can be used for limited purposes.
[0201] ×: The number of foreign objects is 100 / 0.05m 2 As mentioned above, the deformation of the casting surface is very obvious and cannot be used.
[0202] (7) Number average molecular weight
[0203] The content was measured by gel permeation chromatography (GPC) and calculated as a polystyrene-equivalent value.
[0204] (8) Thickness of release layer
[0205] After cutting the release film into small triangular pieces, a Pt (platinum) layer with a thickness of 2nm is formed on the surface of the release layer by coating. The obtained sample is fixed in a multi-axis embedding capsule, embedded with epoxy resin, and sliced in a direction perpendicular to the surface direction of the film using a slicer ULTRACUT-S to obtain an ultra-thin sample with a thickness of 50nm. Next, the obtained ultra-thin sample is placed on a grid and steam-stained with 2% osmic acid at 60°C for 2 hours. Using the ultra-thin sample after steam staining, a transmission electron microscope LEM-2000 is used to observe the cross section of the film at an acceleration voltage of 100kV to measure the thickness of the release layer. The measurement is performed at any 10 points, and their average value is taken as the thickness of the release layer (unit: nm).
[0206] [Example 1-1]
[0207] The polyethylene terephthalate ([η]=0.64dl / g, Tg=78°C) containing 0.1% by mass of calcium carbonate particles with an average particle size of 0.6μm was melted by an extruder, passed through a filter with a filtration accuracy of 10μm, extruded from a mold, and cooled by a cooling drum by a conventional method to form an unstretched film. Then, after being stretched to 3.3 times at 80°C in the longitudinal direction, the water-based coating liquid (aqueous coating composition) obtained in Manufacturing Example 1-1 was uniformly applied by a roller coater in such a manner that the product thickness became the release layer thickness shown in Table 2. It should be noted that the water-based coating liquid used was a coating liquid used within 24 hours after preparation.
[0208] Next, the coated film was dried at 110°C, stretched to 4.5 times in the transverse direction at 140°C, and then heat-set at 235°C for about 10 seconds to obtain a release film (thickness 25 μm) having a release layer formed by reacting and curing the water-based coating liquid, and the evaluation was performed. The evaluation results are shown in Table 2.
[0209] It should be noted that 40% by mass of the following raw materials are used: when taking the product roll, for each embodiment and comparative example, the part of the release film that does not become the product, and the release film that does not become the product due to defects, etc. are crushed until the major diameter of the film piece becomes less than about 5 mm, and the raw materials are obtained by melting and regenerating.
[0210] <Production Example 1-1>
[0211] (Sample 1-1A)
[0212] Using an emulsifier capable of stirring the entire container (NP Labo Co., Ltd., device name "Super Planetary Stirrer"), a raw material containing 96% by mass of a1 of formula (1), 100% by mole, b1, 0% by mole, and a number average molecular weight of 9000 silicone oil, and 4% by mass of polyoxyethylene tridecyl ether (LION SPECIALTY CHEMICALS CO., LTD., trade name "LEOCOL TD-90") as a surfactant was mechanically emulsified in an aqueous medium to obtain a water-based emulsion of sample 1-1A having a solid content of 50% by mass. In addition, the emulsion particle size was adjusted to an average particle size of 210 nm by adjusting the stirring speed and stirring time during emulsification.
[0213]
[0214] (Sample 1-2A)
[0215] Using an emulsifier capable of stirring the entire container (NPLabo Co., Ltd., device name "Super Planetary Stirrer"), a raw material containing 96% by mass of a2 of formula (2), 50% by mole, 50% by mole of b2, and a number average molecular weight of 3000 silicone oil, and 4% by mass of polyoxyethylene tridecyl ether (LION SPECIALTYCHEMICALS CO., LTD., trade name "LEOCOL TD-90") as a surfactant was mechanically emulsified in an aqueous medium to obtain a water dispersion of sample 1-2A having a solid content of 50% by mass. In addition, the emulsion particle size was adjusted to an average particle size of 170 nm by adjusting the stirring speed and stirring time during emulsification.
[0216]
[0217] (Water-based coating liquid)
[0218] As a water-based coating liquid, the solid content mass of the silicone of Sample 1-1A and Sample 1-2A was prepared to be the compounding amount shown in Table 2, and other components were set as follows. The following coupling agent was mixed at 3 mass% relative to the total mass of the silicone, the following platinum catalyst was mixed at 60 ppm relative to the total mass of the solid content of Sample 1-1 and Sample 1-2, and the following cross-linking reaction inhibitor was mixed at 120 ppm relative to the mass of the water-based coating liquid, and the solid content concentration of the water-based coating liquid was diluted with water to obtain the target release layer thickness, thereby preparing a water-based coating liquid.
[0219] · Coupling agent: 3-glycidoxypropyltriethoxysilane (manufactured by JNC Corporation, trade name "Sila-Ace S510")
[0220] · Platinum-based catalyst: platinum-based catalyst emulsion (manufactured by Wacker, trade name “CATALYST EM440”)
[0221] Cross-linking reaction inhibitor: 1-ethynylcyclohexanol (manufactured by Alfa Lancaster)
[0222] [Examples 1-2 to 1-3]
[0223] In Example 1-1, except that the contents of Sample 1-1A and Sample 1-2A were changed as shown in Table 2 when preparing the water-based coating liquid, release films were prepared under the same conditions as in Example 1-1 and the above evaluations were performed.
[0224] [Examples 1-4]
[0225] In Example 1-1, except that the water-based coating liquid was prepared using the sample 1-1B prepared in Preparation Example 1-2 instead of the sample 1-1A, a release film was produced under the same conditions as in Example 1-1 and the above evaluation was performed.
[0226] <Production Example 1-2> (Sample 1-1B)
[0227] Using an emulsifier capable of stirring the entire container (NP Labo Co., Ltd., device name "Super Planetary Stirrer"), a raw material containing 96% by mass of a1 of formula (1), 100 mol%, b1, 0 mol%, and a number average molecular weight of 5000 silicone oil, and 4% by mass of polyoxyethylene tridecyl ether as a surfactant (LION SPECIALTY CHEMICALS CO., LTD., trade name "LEOCOL TD-90") was mechanically emulsified in an aqueous medium to obtain a water-based emulsion of sample 1-1B having a solid content of 50% by mass. In addition, the emulsion particle size was adjusted to an average particle size of 190 nm by adjusting the stirring speed and stirring time during emulsification.
[0228] [Examples 1-5]
[0229] In Example 1-1, except that the water-based coating liquid was prepared using the sample 1-1C prepared in Preparation Example 1-3 instead of the sample 1-1A, a release film was prepared under the same conditions as in Example 1-1 and the above evaluation was performed.
[0230] <Production Example 1-3> (Sample 1-1C)
[0231] Using an emulsifier capable of stirring the entire container (NP Labo Co., Ltd., device name "Super Planetary Stirrer"), a raw material containing 96% by mass of a1 of formula (1), 100 mol%, b1, 0 mol%, and a number average molecular weight of 3000 silicone oil, and 4% by mass of polyoxyethylene tridecyl ether as a surfactant (LION SPECIALTY CHEMICALS CO., LTD., trade name "LEOCOL TD-90") was mechanically emulsified in an aqueous medium to obtain a water-based emulsion of sample 1-1C having a solid content of 50% by mass. In addition, the emulsion particle size was adjusted to an average particle size of 170 nm by adjusting the stirring speed and stirring time during emulsification.
[0232] [Examples 1-6]
[0233] In Example 1-1, except that the water-based coating liquid was prepared using the sample 1-1D prepared in Preparation Example 1-4 instead of the sample 1-1A, a release film was prepared under the same conditions as in Example 1-1 and the above evaluation was performed.
[0234] <Production Example 1-4> (Sample 1-1D)
[0235] Using an emulsifier capable of stirring the entire container (NPLabo Co., Ltd., device name "Super Planetary Stirrer"), a raw material containing 96% by mass of a1 of formula (1) is 96 mol%, b1 is 4 mol%, and the number average molecular weight of the silicone oil is 7000, and 4% by mass of polyoxyethylene tridecyl ether (LION SPECIALTYCHEMICALS CO., LTD., trade name "LEOCOL TD-90") as a surfactant is mechanically emulsified in an aqueous medium to obtain a water-based emulsion of sample 1-1D having a solid content of 50% by mass. In addition, the emulsion particle size was adjusted to an average particle size of 200 nm by adjusting the stirring speed and stirring time during emulsification.
[0236] [Comparative Examples 1-1 to 1-3]
[0237] In Examples 1-1 to 1-3, except that the water-based coating liquid obtained in Preparation Example 1-5 was used instead of the water-based coating liquid obtained in Preparation Example 1-1, release films were prepared under the same conditions as in Examples 1-1 to 1-3 and the above evaluations were performed.
[0238] <Production Example 1-5>
[0239] (Sample 1-1E)
[0240] Using an emulsifier capable of stirring the entire container (NP Labo Co., Ltd., device name "Super Planetary Stirrer"), a raw material containing 96% by mass of a1 of formula (1), 97% by mole, 3% by mole of b1, and a number average molecular weight of 30,000 silicone oil, and 4% by mass of polyoxyethylene tridecyl ether (LION SPECIALTY CHEMICALS CO., LTD., trade name "LEOCOL TD-90") as a surfactant was mechanically emulsified in an aqueous medium to obtain a water-based emulsion of sample 1-1E having a solid content of 50% by mass. In addition, the emulsion particle size was adjusted to an average particle size of 200 nm by adjusting the stirring speed and stirring time during emulsification.
[0241] (Sample 1-2B)
[0242] Using an emulsifier capable of stirring the entire container (NPLabo Co., Ltd., device name "Super Planetary Stirrer"), a raw material containing 96% by mass of a2 of formula (2), 55% by mole, b2, 45% by mole, and a number average molecular weight of 7000 silicone oil, and 4% by mass of polyoxyethylene tridecyl ether (LION SPECIALTYCHEMICALS CO., LTD., trade name "LEOCOL TD-90") as a surfactant was mechanically emulsified in an aqueous medium to obtain a water dispersion of sample 1-2B having a solid content of 50% by mass. In addition, the emulsion particle size was adjusted to an average particle size of 190 nm by adjusting the stirring speed and stirring time during emulsification.
[0243] (Water-based coating liquid)
[0244] As aqueous coating liquids, aqueous coating liquids were prepared under the same conditions as in Production Example 1-1 except that the solid content mass of silicone in Sample 1-1E and Sample 1-2B was adjusted to the blending amount shown in Table 2.
[0245] [Comparative Examples 1-4]
[0246] In Example 1-1, no release layer was applied. Except for this, a film was formed in the same manner as in Example 1-1 to prepare a substrate film. In addition, 88% by mass of a1 of formula (1) was 96 mol%, b1 was 4 mol%, and the number average molecular weight of the silicone was 150,000, 9% by mass of a2 of formula (2) was 80 mol%, b2 was 20 mol%, and the number average molecular weight of the silicone was 20,000, and 3% by mass of the catalyst: CM670 (produced by Momentive) were mixed, and the necessary amount of platinum catalyst was added. The solid content concentration of the coating liquid was diluted with an organic solvent of methyl ethyl ketone and toluene at 70% by mass / 30% by mass in a manner to obtain the target release layer thickness, and a coating liquid was prepared. Using a coating machine, the coating liquid was applied to the substrate film to form a release layer, and dried at a temperature of 130° C. and a time of 30 seconds to prepare a release film, and the above-mentioned evaluation was performed. The results are shown in Table 2. It should be noted that since the release layer is formed using an organic solvent, special explosion-proof equipment is required, and exhaust treatment of the dried organic solvent is also required separately compared to the examples.
[0247] [Comparative Examples 1-5]
[0248] The film was prepared in the same manner as in Example 1-1 except that the release layer was not applied, and a substrate film was prepared. In addition, 88% by mass of a1 of formula (1) was 99 mol%, b1 was 1 mol%, and the number average molecular weight of the silicone was 8000, 9% by mass of a2 of formula (2) was 60 mol%, b2 was 40 mol%, and the number average molecular weight of the silicone was 4000, and 3% by mass of the catalyst: CM670 (produced by Momentive) was mixed in accordance with the solid content ratio, and the solid content concentration of the coating liquid was diluted with an organic solvent of 70% by mass / 30% by mass of methyl ethyl ketone and toluene in a manner to obtain the target release layer thickness, and a coating liquid was prepared. Using a coating machine, the coating liquid was applied to the substrate film to form a release layer, and dried at a temperature of 130°C and a time of 30 seconds to prepare a release film, and the above-mentioned evaluation was performed. The results are shown in Table 2. It should be noted that since the release layer is formed using an organic solvent, special explosion-proof equipment is required, and exhaust treatment of the dried organic solvent is also required separately compared to the examples.
[0249] [Table 2]
[0250]
[0251] As shown in Table 2, in Examples 1-1 to 1-6, it is possible to obtain a release film that easily takes into account both the release property and wettability of the release layer, and has good coating uniformity and recyclability of the release layer. In contrast, in Comparative Examples 1-1 to 1-3, in which the molecular weight of the silicone is large, there is a tendency for the coating uniformity to deteriorate, the ceramic sheet to undergo heavy peeling, and the recyclability is also deteriorated. In Comparative Examples 1-4 to 1-5, in which a solvent-based coating liquid is used to form the release layer in an offline manner, the coating uniformity of the release layer and the adhesion of the release layer are reduced, and in particular, in Comparative Example 1-4, in which the molecular weight of the silicone is large, the recyclability is also deteriorated.
[0252] [Example 2-1]
[0253] Polyethylene terephthalate ([η] = 0.65dl / g, Tg = 78°C) containing 0.15% by mass of calcium carbonate particles with an average particle size of 0.6μm was melted by an extruder, passed through a filter with a filtration accuracy of 10μm, extruded from a mold, and cooled by a cooling drum by a conventional method to form an unstretched film. Then, after being stretched to 3.2 times at 80°C in the longitudinal direction, the water-based coating liquid (aqueous coating composition) obtained in Manufacturing Example 2-1 was uniformly applied by a roller coater in such a manner that the product thickness became the release layer thickness shown in Table 3. It should be noted that the water-based coating liquid used was a coating liquid used within 24 hours after preparation.
[0254] Next, the coated film was dried at 105°C, stretched to 4.6 times in the transverse direction at 145°C, and then heat-set at 230°C for about 10 seconds to obtain a release film (thickness 25 μm) having a release layer formed by reacting and curing the water-based coating liquid, and the evaluation was performed. The evaluation results are shown in Table 3.
[0255] It should be noted that 45% by mass of the following raw materials are used: when taking the product roll, for each embodiment and comparative example, the part of the release film that does not become the product, the release film that does not become the product due to defects, etc., is crushed until the major diameter of the film piece becomes less than about 5 mm, and the raw material is obtained by melting and regenerating it.
[0256] <Production Example 2-1>
[0257] (Sample 2-1A)
[0258] Using an emulsifier capable of stirring the entire container (NPLabo Co., Ltd., device name "Super Planetary Stirrer"), a raw material containing 95% by mass of silicone oil having a number average molecular weight of 8000, 2 mol% of formula (A), 4 mol% of formula (B), 90 mol% of formula (C), 2 mol% of formula (D), and 2 mol% of formula (E), and 5% by mass of polyoxyethylene tridecyl ether (ADEKA CORPORATION, trade name "ADEKA TOL TN-100") as a surfactant was mechanically emulsified in an aqueous medium to obtain an aqueous emulsion of sample 2-1A having a solid content of 45% by mass. In addition, the emulsion particle size was adjusted to an average particle size of 200 nm by adjusting the stirring speed and stirring time during emulsification.
[0259]
[0260] (Sample 2-2A)
[0261] Using an emulsifying device (NPLabo Co., Ltd., device name "Super Planetary Stirrer") capable of stirring the entire container, a3 of formula (F) containing 95% by mass, 60 mol%, b3 of 40 mol%, a silicone oil with a number average molecular weight of 4000, and 5% by mass of polyoxyethylene tridecyl ether (ADEKA CORPORATION, trade name "ADEKA TOL TN-100") as a surfactant was mechanically emulsified in an aqueous medium to obtain a water dispersion of sample 2-2 having a solid content of 40% by mass. In addition, the emulsion particle size was adjusted to an average particle size of 180 nm by adjusting the stirring speed and stirring time during emulsification.
[0262]
[0263] (Water-based coating liquid)
[0264] As a water-based coating liquid, the solid content mass of the silicone of Sample 2-1A and Sample 2-2A was prepared in the blending amount shown in Table 3, and other components were set as follows. The following coupling agent was mixed at 5 mass% relative to the total mass of the silicone, the following platinum catalyst was mixed at 50 ppm relative to the total mass of the solid content of Sample 2-1 and Sample 2-2, and the following cross-linking reaction inhibitor was mixed at 100 ppm relative to the mass of the water-based coating liquid, and the solid content concentration of the water-based coating liquid was diluted with water so as to obtain the target release layer thickness, thereby preparing a water-based coating liquid.
[0265] · Coupling agent: 3-glycidoxypropyltriethoxysilane (manufactured by Shin-Etsu Chemical Co., Ltd., trade name "KBE-403")
[0266] · Platinum-based catalyst: platinum-based catalyst emulsion (manufactured by Wacker, trade name “CATALYST EM440”)
[0267] Cross-linking reaction inhibitor: 1-ethynylcyclohexanol (manufactured by Alfa Lancaster)
[0268] [Examples 2-2 to 3]
[0269] In Example 2-1, except that the contents of Sample 2-1A and Sample 2-2A were changed as shown in Table 3 when preparing the water-based coating liquid, release films were prepared under the same conditions as in Example 2-1 and the above evaluations were performed.
[0270] [Examples 2-4]
[0271] In Example 2-2, except that the water-based coating liquid was prepared using the sample 2-1B prepared in Preparation Example 2-2 instead of the sample 2-1A, a release film was prepared under the same conditions as in Example 2-2 and the above evaluation was performed.
[0272] <Production Example 2-2> (Sample 2-1B)
[0273] Using an emulsifier capable of stirring the entire container (NPLabo Co., Ltd., device name "Super Planetary Stirrer"), a raw material containing 95% by mass of a silicone oil having a number average molecular weight of 4000, which is 3 mol% of formula (A), 7 mol% of formula (B), 85 mol% of formula (C), 2 mol% of formula (D), and 3 mol% of formula (E), and 5% by mass of polyoxyethylene tridecyl ether as a surfactant (ADEKA CORPORATION, trade name "ADEKA TOL TN-100") was mechanically emulsified in an aqueous medium to obtain a water-based emulsion of sample 2-1B having a solid content of 50% by mass. In addition, the emulsion particle size was adjusted to an average particle size of 180 nm by adjusting the stirring speed and stirring time during emulsification.
[0274] [Example 2-5]
[0275] In Example 2-2, except that the water-based coating liquid was prepared using the sample 2-1C prepared in Preparation Example 2-3 instead of the sample 2-1A, a release film was prepared under the same conditions as in Example 2-2 and the above evaluation was performed.
[0276] <Production Example 2-3> (Sample 2-1C)
[0277] Using an emulsifier capable of stirring the entire container (NPLabo Co., Ltd., device name "Super Planetary Stirrer"), a raw material containing 95% by mass of silicone oil having a number average molecular weight of 6000, 10% by mole of formula (A), 5% by mole of formula (B), 84% by mole of formula (C), 1% by mole of formula (D), and 10% by mole of formula (E), and 5% by mass of polyoxyethylene tridecyl ether as a surfactant (ADEKA CORPORATION, trade name "ADEKA TOL TN-100") was mechanically emulsified in an aqueous medium to obtain a water-based emulsion of sample 2-1C having a solid content of 40% by mass. In addition, the emulsion particle size was adjusted to an average particle size of 210 nm by adjusting the stirring speed and stirring time during emulsification.
[0278] [Comparative Examples 2-1 to 3]
[0279] In Examples 2-1 to 3, except that the water-based coating liquid obtained in Preparation Example 2-4 was used instead of the water-based coating liquid obtained in Preparation Example 2-1, release films were prepared under the same conditions as in Examples 2-1 to 2-3 and the above evaluations were performed.
[0280] <Production Example 2-4>
[0281] (Sample 2-1D)
[0282] Using an emulsifier capable of stirring the entire container (NPLabo Co., Ltd., device name "Super Planetary Stirrer"), a raw material containing 95% by mass of formula (A), 30% by mole, formula (B), 5% by mole, formula (C), 30% by mole, formula (D), 1% by mole, formula (E), 34% by mole, and a number average molecular weight of 250,000 silicone oil, and 5% by mass of polyoxyethylene tridecyl ether as a surfactant (ADEKA CORPORATION, trade name "ADEKA TOL TN-100") was mechanically emulsified in an aqueous medium to obtain a water-based emulsion of sample 2-1D having a solid content of 40% by mass. In addition, the emulsion particle size was adjusted to an average particle size of 300 nm by adjusting the stirring speed and stirring time during emulsification.
[0283] (Sample 2-2B)
[0284] Using an emulsifying device (NPLabo Co., Ltd., device name "Super Planetary Stirrer") capable of stirring the entire container, a raw material containing 95% by mass of a3 of formula (F) is 50 mol%, b3 is 50 mol%, and a number average molecular weight of 8000 silicone oil, and 5% by mass of polyoxyethylene tridecyl ether (ADEKA CORPORATION, trade name "ADEKA TOL TN-100") as a surfactant is mechanically emulsified in an aqueous medium to obtain a water dispersion of sample 2-2 having a solid content of 50% by mass. In addition, the emulsion particle size is adjusted to an average particle size of 210 nm by adjusting the stirring speed and stirring time during emulsification.
[0285] (Water-based coating liquid)
[0286] As aqueous coating liquids, aqueous coating liquids were prepared under the same conditions as in Production Example 2-1, except that the solid content mass of silicone in Sample 2-1D and Sample 2-2B was adjusted to the blending amount shown in Table 3.
[0287] [Comparative Examples 2-4]
[0288] Except that the release layer is not applied, the film is formed in the same manner as in Example 2-1 to prepare a substrate film. Silicone: SD-7335 (manufactured by Dow Toray Co., Ltd., addition reaction type, number average molecular weight of 900000) 80 mass%, silicone: SD-7236 (manufactured by DOW TORAY CO., LTD., addition reaction type containing silicone resin, number average molecular weight of 580000) 20 mass%, catalyst: SRX-212 (manufactured by DOW TORAY CO., LTD.) 0.02 mass% are mixed in accordance with the solid content ratio, and the solid content concentration of the coating liquid is diluted with toluene in a manner to obtain the target release layer thickness to prepare a coating liquid. Using a coating machine, the coating liquid is applied to the substrate film to form a release layer, and drying is carried out under the conditions of a temperature of 150°C and a time of 30 seconds to prepare a release film, and the above-mentioned evaluation is performed. The results are shown in Table 3. It should be noted that since the release layer is formed using an organic solvent, special explosion-proof equipment is required, and exhaust treatment of the dried organic solvent is also required separately compared to the examples.
[0289] [Comparative Example 2-5]
[0290] The film was prepared in the same manner as in Example 2-1 except that the release layer was not applied, and a substrate film was prepared. In addition, a1 of formula (1) was 96 mol%, b1 was 4 mol%, and 88 mass% of an organosilicon with a number average molecular weight of 150,000, a2 of formula (2) was 80 mol%, b2 was 20 mol%, and 9 mass% of an organosilicon with a number average molecular weight of 20,000, and a catalyst: CM670 (produced by Momentive) was 3 mass% was mixed, and a necessary amount of a platinum catalyst was added. The solid content concentration of the coating liquid was diluted with an organic solvent of methyl ethyl ketone and toluene at 70 mass% / 30 mass% in a manner to obtain the target release layer thickness, and a coating liquid was prepared. Using a coating machine, the coating liquid was applied to the substrate film to form a release layer, and dried at a temperature of 130°C and a time of 30 seconds to prepare a release film, and the above-mentioned evaluation was performed. The results are shown in Table 3. It should be noted that since the release layer is formed using an organic solvent, special explosion-proof equipment is required, and exhaust treatment of the dried organic solvent is also required separately compared to the examples.
[0291]
[0292] [Table 3]
[0293]
[0294] As shown in Table 3, in Examples 2-1 to 2-5, release films that easily achieve both the release layer's releasability and wettability, and have good coating uniformity and recyclability of the release layer can be obtained. In contrast, in Comparative Examples 2-1 to 2-3, in which the molecular weight of the silicone is large, there is a tendency for deterioration in coating uniformity, heavy peeling of the ceramic sheet, and deterioration in recyclability. In Comparative Examples 2-4 to 2-5, which use a solvent-based coating liquid and form a release layer in an offline manner, and use silicone with a large molecular weight, the recyclability is deteriorated. In particular, in Comparative Example 2-5, the adhesion of the release layer is reduced, making it difficult to achieve both the release layer's releasability and wettability.
[0295] [Example 3-1]
[0296] Polyethylene terephthalate ([η] = 0.63dl / g, Tg = 78°C) containing 0.25% by mass of calcium carbonate particles with an average particle size of 0.6μm was melted by an extruder, passed through a filter with a filtration accuracy of 10μm, extruded from a mold, and cooled by a cooling drum by a conventional method to form an unstretched film. Then, after being stretched to 3.2 times at 80°C in the longitudinal direction, the water-based coating liquid (aqueous coating composition) obtained in Manufacturing Example 3-1 was uniformly applied by a roller coater in such a manner that the product thickness became the release layer thickness shown in Table 4. It should be noted that the water-based coating liquid used was a coating liquid used within 24 hours after preparation.
[0297] Next, the coated film was dried at 105°C, stretched to 4.6 times in the transverse direction at 145°C, and then heat-set at 230°C for about 10 seconds to obtain a release film (thickness 25 μm) having a release layer formed by reacting and curing the water-based coating liquid, and the evaluation was performed. The evaluation results are shown in Table 4.
[0298] It should be noted that 40% by mass of the following raw materials are used: when taking the product roll, for each embodiment and comparative example, the part of the release film that does not become the product, the release film that does not become the product due to defects, etc., is crushed until the major diameter of the film piece becomes less than about 5 mm, and the raw material is obtained by melting and regenerating it.
[0299] <Production Example 3-1>
[0300] (Sample 3-1A)
[0301] Using an emulsifier capable of stirring the entire container (manufactured by NPLabo Co., Ltd., device name "Super Planetary Stirrer"), a raw material containing 97% by mass of a1 of formula (1), 100% by mole, b1, 0% by mole, and a number average molecular weight of 8000 silicone oil, and 3% by mass of polyoxyethylene tridecyl ether (manufactured by Kao Corporation, trade name "EMULGEN 1108") as a surfactant was mechanically emulsified in an aqueous medium to obtain an aqueous emulsion of sample 3-1A having a solid content of 40% by mass. In addition, the emulsion particle size was adjusted to an average particle size of 200 nm by adjusting the stirring speed and stirring time during emulsification.
[0302]
[0303] (Sample 3-2A)
[0304] Using an emulsifier capable of stirring the entire container (NPLabo Co., Ltd., device name "Super Planetary Stirrer"), a raw material containing 96% by mass of a2 of formula (2), 50% by mole, 50% by mole of b2, and a number average molecular weight of 3500 silicone oil, and 4% by mass of polyoxyethylene tridecyl ether (Kao Corporation, trade name "EMULGEN 1108") as a surfactant was mechanically emulsified in an aqueous medium to obtain a water dispersion of sample 3-2 having a solid content of 40% by mass. In addition, the emulsion particle size was adjusted to an average particle size of 180 nm by adjusting the stirring speed and stirring time during emulsification.
[0305]
[0306] (Water-based coating liquid)
[0307] As a water-based coating liquid, the solid content mass of the silicone of Sample 3-1A and Sample 3-2A was prepared in the blending amount shown in Table 4, and other components were set as follows. 5 mass % of the following polyvinyl alcohol and 3 mass % of the following coupling agent were mixed with respect to the total mass of the silicone, 50 ppm of the following platinum catalyst was mixed with respect to the total mass of the solid content of Samples 3-1 and 3-2, and 100 ppm of the following cross-linking reaction inhibitor was mixed with respect to the mass of the water-based coating liquid, and the solid content concentration of the water-based coating liquid was diluted with water so as to obtain the target release layer thickness, thereby preparing a water-based coating liquid.
[0308] Polyvinyl alcohol: polyvinyl alcohol having a viscosity of 27 mPa·s (4 mass % aqueous solution, temperature of 20° C.) and a saponification degree of 96 mol % (manufactured by Kuraray Co., Ltd., trade name “KURARAY POVAL27-96”)
[0309] · Coupling agent: 3-glycidoxypropyltriethoxysilane (manufactured by Shin-Etsu Chemical Co., Ltd., trade name "KBE-403")
[0310] · Platinum-based catalyst: platinum-based catalyst emulsion (manufactured by Wacker, trade name “CATALYST EM440”)
[0311] Cross-linking reaction inhibitor: 1-ethynylcyclohexanol (manufactured by Alfa Lancaster)
[0312] [Example 3-2]
[0313] In Example 3-1, except that the water-based coating liquid was prepared using the sample 3-1B prepared in Preparation Example 3-2 instead of the sample 3-1A, a release film was prepared under the same conditions as in Example 3-1 and the above evaluation was performed.
[0314] <Production Example 3-2> (Sample 3-1B)
[0315] Using an emulsifier capable of stirring the entire container (manufactured by NPLabo Co., Ltd., device name "Super Planetary Stirrer"), a raw material containing 97% by mass of a1 of formula (1) with 100 mol%, b1 with 0 mol%, and a number average molecular weight of 4000 silicone oil, and 3% by mass of polyoxyethylene tridecyl ether (manufactured by Kao Corporation, trade name "EMULGEN 1108") as a surfactant was mechanically emulsified in an aqueous medium to obtain an aqueous emulsion of sample 3-1B having a solid content of 40% by mass. In addition, the emulsion particle size was adjusted to an average particle size of 180 nm by adjusting the stirring speed and stirring time during emulsification.
[0316] [Example 3-3]
[0317] In Example 3-1, except that the water-based coating liquid was prepared using the sample 3-1C prepared in Preparation Example 3-3 instead of the sample 3-1A, a release film was prepared under the same conditions as in Example 3-1 and the above evaluation was performed.
[0318] <Production Example 3-3> (Sample 3-1C)
[0319] Using an emulsifier capable of stirring the entire container (manufactured by NPLabo Co., Ltd., device name "Super Planetary Stirrer"), a raw material containing 97% by mass of a1 of formula (1), 98% by mole, 2% by mole of b1, and a number average molecular weight of 8000 silicone oil, and 3% by mass of polyoxyethylene tridecyl ether (manufactured by Kao Corporation, trade name "EMULGEN 1108") as a surfactant was mechanically emulsified in an aqueous medium to obtain a water-based emulsion of sample 3-1C having a solid content of 40% by mass. In addition, the emulsion particle size was adjusted to an average particle size of 200 nm by adjusting the stirring speed and stirring time during emulsification.
[0320] [Examples 3-4]
[0321] In Example 3-1, except that the water-based coating liquid was prepared using the sample 3-1D prepared in Preparation Example 3-4 instead of the sample 3-1A, a release film was prepared under the same conditions as in Example 3-1 and the above evaluation was performed.
[0322] <Production Example 3-4> (Sample 3-1D)
[0323] Using an emulsifier capable of stirring the entire container (NPLabo Co., Ltd., device name "Super Planetary Stirrer"), a raw material containing 97% by mass of a silicone oil having a number average molecular weight of 7000, 1 mol% of formula (A), 3 mol% of formula (B), 93 mol% of formula (C), 2 mol% of formula (D), 1 mol% of formula (E), and 3% by mass of polyoxyethylene tridecyl ether as a surfactant (Kao Corporation, trade name "EMULGEN 1108") was mechanically emulsified in an aqueous medium to obtain a water-based emulsion of sample 3-1D having a solid content of 40% by mass. In addition, the emulsion particle size was adjusted to an average particle size of 180 nm by adjusting the stirring speed and stirring time during emulsification.
[0324]
[0325] [Examples 3-5]
[0326] In Example 3-4, when preparing the water-based coating liquid, the contents of Sample 3-1D and Sample 3-2A were changed as shown in Table 4. The same conditions as in Example 3-4 were used to prepare release films and perform the above evaluations. The results are shown in Table 4.
[0327] [Examples 3-6]
[0328] In Example 3-1, except that the water-based coating liquid was prepared using the sample 3-1E prepared in Preparation Example 3-5 instead of the sample 3-1A, a release film was prepared under the same conditions as in Example 3-1 and the above evaluation was performed.
[0329] <Production Example 3-5> (Sample 3-1E)
[0330] Using an emulsifier capable of stirring the entire container (manufactured by NPLabo Co., Ltd., device name "Super Planetary Stirrer"), a raw material containing 97% by mass of silicone oil having a number average molecular weight of 3000 of formula (A), 2% by mole of formula (B), 91% by mole of formula (C), 1% by mole of formula (D), and 2% by mole of formula (E), and 3% by mass of polyoxyethylene tridecyl ether (manufactured by Kao Corporation, trade name "EMULGEN 1108") as a surfactant was mechanically emulsified in an aqueous medium to obtain a water-based emulsion of sample 3-1E having a solid content of 40% by mass. In addition, the emulsion particle size was adjusted to an average particle size of 170 nm by adjusting the stirring speed and stirring time during emulsification.
[0331] [Examples 3-7]
[0332] In Example 3-1, a release film was produced and evaluated under the same conditions as in Example 3-1 except that the following polyvinyl alcohol (Kuraray Co., Ltd., trade name "Kuraray POVAL 27-96") was used instead of polyvinyl alcohol to prepare the water-based coating liquid. The results are shown in Table 4.
[0333] Polyvinyl alcohol: polyvinyl alcohol having a viscosity of 23 mPa·s (4 mass % aqueous solution, temperature of 20° C.) and a saponification degree of 88 mol % (manufactured by Mitsubishi Chemical Corporation, trade name “GOHSENOL GM-14R”)
[0334] [Comparative Examples 3-1 to 3-2]
[0335] In Examples 3-4 to 3-5, except that the water-based coating liquid obtained in Preparation Example 3-6 was used instead of the water-based coating liquid obtained in Preparation Example 3-4, release films were prepared under the same conditions as in Examples 3-4 to 3-5 and the above evaluations were performed.
[0336] <Production Example 3-6>
[0337] (Sample 3-1F)
[0338] Using an emulsifier capable of stirring the entire container (manufactured by NPLabo Co., Ltd., device name "Super Planetary Stirrer"), a raw material containing 96% by mass of silicone oil having a number average molecular weight of 270,000 of formula (A), 35% by mole of formula (B), 5% by mole of formula (C), 25% by mole of formula (D), 33% by mole of formula (E), and 4% by mass of polyoxyethylene tridecyl ether (manufactured by Kao Corporation, trade name "EMULGEN 1108") as a surfactant was mechanically emulsified in an aqueous medium to obtain a water-based emulsion of sample 3-1F having a solid content of 40% by mass. In addition, the emulsion particle size was adjusted to an average particle size of 260 nm by adjusting the stirring speed and stirring time during emulsification.
[0339] (Sample 3-2B)
[0340] Using an emulsifier capable of stirring the entire container (NPLabo Co., Ltd., device name "Super Planetary Stirrer"), a raw material containing 96% by mass of a2 of formula (2), 50% by mole, 50% by mole of b2, and a number average molecular weight of 9000 silicone oil, and 4% by mass of polyoxyethylene tridecyl ether (Kao Corporation, trade name "EMULGEN 1108") as a surfactant was mechanically emulsified in an aqueous medium to obtain a water dispersion of sample 3-2B having a solid content of 50% by mass. In addition, the emulsion particle size was adjusted to an average particle size of 230 nm by adjusting the stirring speed and stirring time during emulsification.
[0341] (Water-based coating liquid)
[0342] As aqueous coating liquids, aqueous coating liquids were prepared under the same conditions as in Production Example 3-1 except that the solid content mass of silicone in Sample 3-1F and Sample 3-2B was adjusted to the blending amount shown in Table 4.
[0343] [Reference Example 3-3]
[0344] In Example 3-4, except that polyvinyl alcohol was not added as another component of the release layer, a release film was produced under the same conditions as in Example 3-4 and the above evaluation was performed.
[0345] [Comparative Examples 3-4]
[0346] Except that the release layer is not applied, the film is formed in the same manner as in Example 3-1 to prepare a substrate film. Silicone: KS-774 (manufactured by Shin-Etsu Astech, addition reaction type, number average molecular weight of 750,000) 86.9 mass%, silicone: KS-3800 (manufactured by Shin-Etsu Astech Co., Ltd., resin type) 13 mass%, catalyst: CAT-PL-50T (manufactured by Shin-Etsu Chemical Co., Ltd.) 0.1 mass% are mixed in accordance with the solid content ratio, and the solid content concentration of the coating liquid is diluted with toluene in a manner to obtain the target release layer thickness to prepare a coating liquid. Using a coating machine, the coating liquid is applied to the substrate film to form a release layer, and drying is carried out under the conditions of a temperature of 150°C and a time of 30 seconds to prepare a release film, and the above-mentioned evaluation is performed. The results are shown in Table 4. It should be noted that since the release layer is formed using an organic solvent, it is necessary to carry out coating in a special explosion-proof facility, and exhaust treatment of the dried organic solvent is also required separately compared to the examples.
[0347] [Comparative Examples 3-5]
[0348] Instead of the release layer, the coating liquid described below was applied to form a primer layer, and a film was formed in the same manner as in Example 3-1 to prepare a substrate film. As a coating liquid instead of the release layer, polyvinyl alcohol: GOHSENOL GL-03 (manufactured by Mitsubishi Chemical Corporation) 70 mass%, polyester resin: PLAS COAT Z-561 (manufactured by GOO CHEMICAL CO., LTD.) 25 mass%, surfactant: EMULGEN 420 (manufactured by Kao Corporation) 5 mass% were mixed in terms of solid content ratio, and the solid content concentration of the coating liquid was adjusted with water so that the coating thickness after film formation was 30 nm and used.
[0349] On the surface of the primer layer of the substrate film on which the coating film was formed, a release layer was applied in the same manner as in Comparative Example 3-4. The results are shown in Table 4. It should be noted that since an organic solvent was used to form the release layer in the same manner as in Comparative Example 3-4, the coating was required to be performed in a special explosion-proof device, and exhaust treatment of the dried organic solvent was also required separately compared to the examples.
[0350] [Table 4]
[0351]
[0352] As shown in Table 4, in Examples 3-1 to 3-7, it is possible to obtain a release film that easily takes into account both the release property and wettability of the release layer, and has good coating uniformity and recyclability of the release layer. In contrast, in Comparative Examples 3-1 to 3-2, where the molecular weight of the silicone is large, there is a tendency for the coating uniformity to deteriorate, the ceramic sheet to be releasable, and the recyclability is also deteriorated. In Reference Example 3-3, in which a water-based coating liquid containing no polyvinyl alcohol is used to form a release layer, the adhesion of the release layer is slightly reduced.
[0353] In Comparative Examples 3-4 to 3-5, which used a solvent-based coating liquid and formed a release layer in an off-line manner and used a silicone with a large molecular weight, wettability was reduced and recyclability was deteriorated. In particular, in Comparative Example 3-4, the adhesion of the release layer was also reduced.
[0354] Industrial Applicability
[0355] The release film of the present invention has high coating uniformity and releasability of the release layer, relatively good wettability, is easily used as a film for various processes, is recyclable, and can reduce the burden on the environment, and has extremely high industrial utilization value.
Claims
1. A release film comprising a substrate film and a release layer, wherein the release layer is formed by reacting and curing an aqueous coating composition, The aqueous coating composition comprises an alkenyl-containing organosilicon and an Si—H-containing organosilicon, wherein the alkenyl-containing organosilicon has two or more alkenyl groups in the molecule and optionally has SiO 4 / 2 The Q unit shown in FIG. 1 has a number average molecular weight of 1,000 or more and less than 10,000, and the Si-H group-containing silicone has two or more Si-H groups in the molecule and has a number average molecular weight of 1,000 or more and 5,000 or less.
2. The release film according to claim 1, wherein The aqueous coating composition includes a polyvinyl alcohol-based resin.
3. The release film according to claim 2, wherein The polyvinyl alcohol-based resin has a viscosity of 5 mPa·s to 50 mPa·s when a 4 mass % aqueous solution is measured at 20° C., and a saponification degree of 85 mol % to 99 mol %.
4. The release film according to claim 1, wherein The alkenyl-containing organosilicon has SiO 4 / 2 The Q unit shown.
5. The release film according to claim 1, wherein The alkenyl-containing organosilicon is represented by the following general formula (I): In the general formula (I), R 1 are optionally the same or different, and are alkenyl groups having 2 to 8 carbon atoms, or monovalent hydrocarbon groups having 1 to 16 carbon atoms including alkyl groups or aryl groups, and [SiO] b1 The silicon atom bonded to R 1 At least one of them is an alkenyl group having 2 to 8 carbon atoms; R 2 are optionally the same or different, and are monovalent hydrocarbon groups having 1 to 16 carbon atoms, including alkyl groups or aryl groups; 1 are optionally the same or different, and are represented by the general formula (Ia), In the general formula (Ia), R 1 With R of general formula (I) 1 The same, and R 1 Optional same or different, Including Y 1 In the general formula (I) as a whole, when all silicon atoms including the terminal are set to 100 mol%, a1 is 50 mol% or more and 98 mol% or less, b1 is 0 mol% or more and 10 mol% or less, c1 is 0 mol% or more and 30 mol% or less, d1 is 0 mol% or more and 50 mol% or less, and in the case of Y 1 In the general formula (I), R 1 Two or more of them are alkenyl groups having 2 to 8 carbon atoms.
6. The release film according to claim 1, wherein The Si-H group-containing organic silicon is represented by the following general formula (II): In the general formula (II), R 3 They are optionally the same or different and are monovalent hydrocarbon groups having 1 to 16 carbon atoms, including alkyl or aryl groups; when a2+b2 is 100 mol %, a2 is 30 mol % to 90 mol %, and b2 is 10 mol % to 70 mol %.
7. The release film according to claim 1, wherein The aqueous coating composition contains 1 part by mass or more and 50 parts by mass or less of the Si—H group-containing silicone relative to 100 parts by mass of the alkenyl group-containing silicone.
8. The release film according to claim 1, wherein The release layer is formed by coating the aqueous coating composition on a substrate film before the crystal orientation is completed, stretching the substrate film in at least one direction, and then performing a heat treatment to complete the crystal orientation.
9. The release film according to claim 1, wherein The substrate film is a polyester film.
10. The release film according to any one of claims 1 to 9, wherein The release film is a release film for a laminated ceramic capacitor or a release film for a resin sheet.
Citation Information
Patent Citations
Polyester film
JP2000289168A
Polysiloxane coating material and releasing film
JP2003292894A
Polysiloxane composition and releasing film
JP2003292895A
Silicone release polyester film
JP2021011081A
Mold release film
WO2017200056A1