Particulate composition containing graphene and

By mixing the particle composition of graphene nanosheets and binder in a turbine mixer, the instability and grinding difficulties of particulate materials in water or organic solvents in traditional processes are solved, and dust-free and controllable Particulate compositions, suitable for a variety of industrial applications, improve performance and safety.

CN118974180APending Publication Date: 2024-11-15DIRAC TAPRAS AG
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202380029043.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-05-03
Filing Date
2023-05-02
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The prior art is difficult to provide a general-purpose granular material suitable for water or organic solvents, and traditional processes have problems of adhesion, instability and grinding difficulties, and lack simple, safe and environmentally friendly manufacturing processes.

Method used

Using a particle composition containing graphene nanosheets and binder, a dust-free, controllable particle composition is formed by mixing particulate materials, graphene and binder in a turbine mixer, suitable for dispersion in water or organic solvents. , avoiding grinding steps and simplifying the process.

Benefits of technology

It realizes stable dispersion in water or organic solvents, improves the performance and processing convenience of the particulate composition, reduces process costs and environmental impact, and is suitable for a variety of industrial applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118974180A_ABST
    Figure CN118974180A_ABST
Patent Text Reader

Abstract

A particulate composition comprising a particulate material selected from the group consisting of pigments and fillers, graphene nanoplatelets, and a binder, and methods of making coatings, varnishes, and inks using the composition.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a particle composition containing graphene, a particle material and one or more binders, and a method for producing the particle composition. The present invention also relates to a dispersion of the particle composition in a liquid medium, and the use of the dispersion in various industrial applications. Background Art

[0002] Many compounds or substances exist in the form of solid particulate materials and must be processed into liquid dispersions or pastes in granular or powder form, depending on the concentration of the active substance (such as pigments, fillers, etc.). The dispersion or paste is used in large quantities or is further processed to obtain the desired final product or object. For example, if the substance is a pigment, it can be used as a pigment or dispersed in a liquid to color paints, varnishes, inks, etc.

[0003] Solid particulate materials usually do not have a controlled particle size and / or shape because of safety and environmental considerations (dust-free). And better product quality.

[0004] In addition, solid particulate materials are often used in combination with additives that have the desired functionality, such as binders or wetting agents and dispersants, which help to improve the stability of the dispersion. Other additives interact with the particulate material to improve the performance of the solid particles in the desired application. For example, additives that improve the mechanical resistance or fire or light resistance of the material are often used.

[0005] However, certain known particulate compositions containing materials of interest, such as pigments for the production of coatings, do not offer optimal performance in terms of corrosion resistance, fire resistance in wood coating applications, mechanical resistance, impermeability and more generally barrier properties.

[0006] According to the invention, a pigment is a colored substance or material, either white or black, which, by dispersion in a solvent, can permanently impart its own color or hue, making reflected or transmitted light appear in a specific color due to the selective absorption of specific wavelengths.

[0007] Pigments generally have a higher tinting strength relative to the solvent or material with which they are mixed.

[0008] Pigments and fillers are particulate materials with a very irregular surface that varies from compound to compound and are often combined with other, quite different substances such as carrier systems.

[0009] In addition, many materials, including pigments, often have small particle sizes in addition to their irregular shapes, which may occur naturally or as a result of grinding. The smaller the particles, the greater their surface energy, and the more likely they are to agglomerate during production or processing, resulting in uncontrollable agglomerate size and shape. Both the irregular shape and small size of the particles can cause difficulties during processing, may be harmful to human health, and may adversely affect the quality of the final product.

[0010] Pigments and fillers are notoriously difficult to meter, handle and integrate into carrier systems. For example, in liquid coating formulations, pigments and fillers are often incorporated by mixing them with dissolved resins in solvent-based or water-based systems.

[0011] The presence of solvents tends to destabilize the contact between the resin and the pigment or filler due to their flocculating properties. This instability can lead to reaggregation of the primary pigment particles. This phenomenon is often referred to as "flocculation". To reduce instability and avoid flocculation, wetting agents and dispersing additives such as binders can be added.

[0012] The binder has a dual function: to reduce the surface tension between the primary pigment particles, to disperse them and to stabilize them, thus avoiding reagglomeration phenomena.

[0013] The conventional production process for spray systems involves a grinding technique in which a single pigment paste is subjected to multiple passes in a grinder lasting several hours, where the pigment is incorporated into a suitable resin.

[0014] However, one of the major limitations of using conventional pigment compositions in solid form (pigment particles that have been coated with an amorphous resin with a relatively low glass transition temperature (Tg), such as aldehydes, ketones or acrylic resins) is the sticking phenomenon that occurs at temperatures above 40°C.

[0015] It must also be noted that the prior art embodiments do not provide satisfactory solutions for preparing liquid dispersions of particulate materials in water or organic solvents, because the materials generally need to be designed or adjusted for a specific dispersion, that is, the prior art particulate materials are not suitable for so-called "general purpose" uses, which is what people want.

[0016] Furthermore, the prior art embodiments do not provide a relatively simple, safe and environmentally friendly optimal solution for the manufacturing process of granular materials. Summary of the invention

[0017] It is therefore an object of the present invention to provide a universal composition of granular type (both aqueous and solvent-based) comprising a granular material and one or more additives which improve the properties of the composition, wherein the granular composition has a substantially regular and controllable form, can be dispersed in water or in an organic solvent without prior adaptation to a specific type of dispersion, i.e. is suitable for such use in both aqueous and solvent-based dispersions.

[0018] Another object of the present invention is to provide a method for preparing a granular composition comprising a granular material and one or more additives, which method is simple, effective, and "grinding-free", that is, one or more grinding steps in a grinder are not required, thereby greatly shortening the processing time.

[0019] Another object of the present invention is to provide a dispersion of a particulate composition comprising a particulate material and one or more additives in water or an organic solvent.

[0020] Therefore, one aspect of the present invention relates to a granular composition comprising: 20 to 95 weight percent of particulate material, the particulate material being a filler; 0.02 to 50 wt % graphene nanoplatelets; 0.5 to 60 wt % of a binder; At least 90% of the graphene nanosheets have a lateral dimension (x, y) of 50 to 20,000 nanometers, a thickness (z) of 1 to 50 nanometers, and a C / O ratio of ≥40:1. Preferably, the particulate material also includes a pigment.

[0021] On the other hand, the present invention relates to a method for preparing the above-mentioned particulate composition, wherein the particulate material, the graphene nanosheets and the binder are mixed in a turbine mixer device having an impeller, the blades of the impeller rotate at a peripheral speed of 4 to 50 m / s, and the method is carried out at a temperature of 20 to 150°C.

[0022] In another aspect, the present invention relates to a dispersion of the above-mentioned granular composition in a liquid selected from water and an organic solvent. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] The present invention will be described below with reference to the accompanying drawings, in which:

[0024] Figure 1A , 1B and 1C are schematic diagrams of the interior of an apparatus for performing the method for preparing a particle composition of the present invention under different operating conditions; DETAILED DESCRIPTION

[0025] According to the present specification, the term "particulate material" refers to pigments, fillers or combinations thereof in the form of solid particles or powders used in the production of water-based or solvent-based coatings.

[0026] According to the invention, pigments and fillers are substances or compounds that absorb part or all of the spectrum and reflect its complementary part, thus forming a visible color.

[0027] In this specification, whenever an element or a group of elements is preceded by the transitional phrase "comprising", it also refers to the same composition or group of elements preceded by the transitional phrase "essentially consisting of...", "consisting of..." or "selected from..."

[0028] According to the present invention, the particulate material defined above is combined with graphene nanoplatelets, one or more binders and optionally other additives to form a particulate composition suitable for further processing to obtain the desired end product, such as a liquid dispersion.

[0029] Therefore, when the particulate material is combined with graphene and in particulate form under the action of a binder, it has better performance than the individual particulate materials, or is easier to process or use. In the application of surface coatings and paints, the combination of pigments and / or fillers with graphene represents the active ingredient of the particulate composition.

[0030] According to the present invention, the binder is a wetting and dispersing agent that can reduce the interfacial tension between the particulate material and the graphene nanosheets.

[0031] The granular composition of the present invention comprises particles with a particle size of 50 to 4000 microns, which are screened by a digital electromagnetic sieving instrument. Vibrationmod.FTL0200 digital electromagnetic vibrating screen measurement.

[0032] In the present specification, the term "particle size" refers to a numerical value indicating an average particle size, that is, a volume-based particle size of particles (defined herein as "particles") existing in the form of aggregates or agglomerates.

[0033] Volume-based particle size is equal to the diameter of an ideal sphere that would completely contain a given particle. The diameter of an ideal sphere is equivalent to the mesh size of a sieve. Volume-based particle size using a digital electromagnetic sieving instrument Vibrationmod.FTL0200 digital electromagnetic vibrating screen measurement.

[0034] According to one aspect of the present invention, the granular composition comprises particles having a particle size of 100 to 3000 microns, which are sieved by a digital electromagnetic sieving instrument. Vibrationmod.FTL0200 digital electromagnetic vibrating screen measurement.

[0035] According to one aspect of the present invention, the granular composition comprises particles with a particle size of 500 to 2000 μm, which are sieved by a digital electromagnetic sieving instrument. Vibrationmod.FTL0200 digital electromagnetic vibrating screen measurement.

[0036] According to one aspect of the invention, the granular composition is dust-free and substantially free of nano-sized solid particulate material. In particular, it does not contain solid particulate materials with a size of less than 10 microns, which will generate dust and cause environmental problems, wherein the term "free" means that it does not contain solid particulate materials with a size of less than 10 microns, or its content is at most 5% by weight. exist.

[0037] In a more general aspect, the present invention relates to a particle composition comprising graphene, one or more pigments and / or fillers, one or more binders, and possibly further additives, which can improve the application performance of anti-corrosion coatings and fire retardant coatings.

[0038] The pigment constituting the granular material of the present invention may be an inorganic metal-based pigment, such as a chromium pigment, an iron oxide pigment or a copper pigment. These pigments are either colored pigments or, like titanium pigments, they may be colored pigments or white pigments.

[0039] The pigments may also be organic pigments, either completely natural pigments or pigments of natural origin, i.e. semi-synthetic or synthetic organic pigments.

[0040] Preferably, the solid particulate material is an inorganic pigment.

[0041] Regarding colors, the following pigments can be used (according to the color index): -Yellow pigments, such as PY 184; PY 138; PY 139; PY 42; PY 216; PY 74; PY 109; PY 119; PY83; PY 65; PY 151; PY 53; PY 110; PY 3; PY 154; PY 150; PY 17; PY 13; PY 14; PY 216;PY199;PY 128;PY 109;PY 168; -Orange pigments, such as PO 73; PO 34; PO 36; PO 13; PO 61; PO 71; PO 64; PO 16; PO 83; PO62; PO 180; - red pigments, such as P.Red 101; P.Red 254; P.Red 122; P.Red 177; P.Red 179; P.Red 170; P.Red 23; P.Red 202; P.Red 146; P.Red 168; P.Red 166; P.Red 112; P.Red 207; P.Red 185; P.Red 60; P.Red 38; P.Red 214; P.Red 144; P.Red 255; - violet pigments such as PV 19, PV 23 and PV 37; - blue pigments, such as PB 15:0; PB 15:1; PB 15:2; PB 15:3; PB 15:4; PB 60; PB 28; - Green pigments, such as PG 7; PG 17; PG 36; - Brown pigments, such as P.Brown 24; - Black pigments, such as P.Black 6; P.Black 7; P.Black 11.

[0042] Preferably, the pigment is selected from the group consisting of: yellow iron oxide - P.Yellow 42, bismuth vanadate - P.Yellow 184, Mixed Metal Oxide-P.Yellow.216; Red Iron Oxide-P.Red 101, Dichromatic Pirro (DPP)-P.Red 254; Chinacridone-P.Red 122; Diossazina-P.Violet 23; Chinacridone-P.Violet19; Phthalocyanine Blue Alfa-P.Blu 15:1; Phthalocyanine Blue Beta-P.Blu 15:3; Phthalocyanine Blue-P.Blu 15:2; Phthalocyanine Blue-P.Blu 15:4; Idanthrone P.Blu 60; Phthalocyanine green-P.Green.7. Chromium titanate-P.Brown.24; Carbon black-P.Black.7; Carbon black-P.Black.6.

[0043] According to another aspect of the present invention, the solid particulate material is a filler.

[0044] Preferably, the filler is selected from the group consisting of calcium carbonate, kaolin, mica, talc, silicon dioxide (preferably fumed silica), barium sulfate, zinc phosphate, calcium phosphate, organic stearates and metal stearates (such as stearates of aluminum, barium, calcium, magnesium, tin and zinc), aluminum silicate and any combination thereof. According to one aspect of the present invention, the filler is calcium carbonate.

[0045] According to one aspect of the present invention, a granular or powdered free-flowing composition comprises: a) 20 to 95% by weight of a particulate material comprising a filler; b) 0.02 to 50 wt. % of graphene nanoplatelets; c) 0.5% to 60% by weight of a binder;

[0046] At least 90% of the graphene nanosheets have a lateral dimension (x, y) of 50 to 20,000 nanometers and a thickness (z) of 1 Up to 50 nm, C / O ratio ≥40:1.

[0047] Preferably, the granular composition comprises: a) 30 to 90% by weight of a particulate material comprising a filler; b) 0.05 to 40 wt % of graphene nanoplatelets; c) 1.0 to 58% by weight of a binder.

[0048] Preferably, the particulate material also includes a pigment.

[0049] According to one aspect of the present invention, at least 90% of the graphene nanosheets have a lateral dimension (x, y) of 80 to 15000. nanometer.

[0050] According to one aspect of the present invention, at least 90% of the graphene nanosheets have a thickness (z) of 3 to 20 nanometers.

[0051] According to one aspect of the present invention, at least 90% of the graphene nanosheets have a C / O ratio ≥ 45:1.

[0052] According to one aspect of the present invention, at least 90% of the graphene nanosheets have a lateral dimension (x, y) of 100 to 10,000. nanometer.

[0053] According to one aspect of the present invention, at least 90% of the graphene nanosheets have a thickness (z) of 5 to 15 nanometers.

[0054] According to one aspect of the present invention, at least 90% of the graphene nanosheets have a C / O ratio ≥ 50:1.

[0055] In this specification, the size of the graphene nanoplatelets is defined with reference to the Cartesian axis x, y, z system, it being understood that these particles are essentially flat plates, but may also have irregular shapes. In any case, the lateral dimensions and thickness provided with reference to the x, y and z axis directions must be the maximum dimension in each of the above directions.

[0056] The structural characterization of graphene can be carried out using ISO / TS21356-1 and 202103 test methods.

[0057] The structural characterization of graphene in the composition of the present invention can be carried out by methods known to the skilled person, wherein the graphene is separated from the particulate material (i.e., pigment or filler), the binder, and any other components in the composition. A suitable method comprises: a first step, repeatedly washing with water to remove the binder, and then separating the particulate material and the graphene by centrifugation.

[0058] According to the present invention, graphene in the form of nanoplatelets (GNPs) can be used as an additive for coatings and polymers (thermoplastics and elastomers). The addition of graphene gives the particulate material unique properties, such as: improved corrosion resistance, improved flame resistance (wood coatings), greater mechanical resistance, enhanced barrier properties, greater impermeability, improved thermal and electrical conductivity, antibacterial and antifouling properties.

[0059] The present invention ensures that graphene has higher dispersibility in different types of resins, while also making it easier to incorporate graphene into particles. In addition, the use of a formulation into which a dispersant has been incorporated improves the dispersion quality compared to using graphene itself and using a dispersant alone.

[0060] Graphene is a material composed of a single atomic layer of hybridized carbon atoms in the form of sp 2 . As a result, they are arranged into a tightly packed, highly crystalline and regular hexagonal honeycomb structure.

[0061] According to the invention, phosphates of various metals (e.g. zinc phosphates or calcium phosphates) are widely used corrosion inhibitor materials in the coating field; in fact, they act as passivators: when the coating is exposed to oxygen and water, the phosphate forms a thin layer on the substrate, passivating the substrate and preventing rust. There are many types of phosphates, the most common being zinc phosphate, but calcium phosphate is also used, especially to replace zinc.

[0062] Graphene works in tandem with phosphates to help form an insulating layer that prevents rust.

[0063] Therefore, it is necessary to add phosphate (zinc, calcium or other phosphate) to the formulation of the particle composition containing graphene.

[0064] Graphene can be used as an additive or a partial replacement for zinc salts; some examples of particle compositions are reported below.

[0065] In a particular embodiment of the invention, the granular composition does not contain zinc phosphate or calcium phosphate.

[0066] Several methods for preparing graphene are known from scientific and patent literature, such as chemical vapor deposition, epitaxial growth, chemical exfoliation, and chemical reduction of graphene oxide (GO).

[0067] The applicant DirectaPlus S.pA is the owner of patents and patent applications related to methods for producing structures comprising graphene layers, such as EP 2 038 209 B1, EP 3 157 864 B1 and 3 157 865 B1. The latter two patents describe methods for producing high-purity graphene dispersions from which graphene nanosheets of the size required for the implementation of the present invention can be obtained.

[0068] DirectaPlus S.pA produces and sells high-purity graphene, i.e. C / O ratio ≥ 40, with the above-mentioned size characteristics. Brand Name

[0069] The C / O ratio of the graphene used in the composition of the present invention can be determined by elemental analysis using an elemental analyzer (CHNS O), which provides the weight percentages of various elements. The obtained values ​​are normalized with the atomic weights of the two elements C and O, and their ratio is obtained to obtain the C / O ratio.

[0070] If a more precise determination is required, the C / O ratio can be determined using a transmission electron microscope (TEM) combined with an energy dispersive X-ray spectrometer (TEM-EDX, also known as TEM-EDS). This is a combination of two effective techniques, because the microscopic surface structure of the sample can be observed more accurately and in more detail using a TEM than with a conventional optical microscope. The resolution of a scanning electron microscope is less than 1 nanometer, which is much higher than that of an optical microscope. Therefore, a higher quality and more precise image of the sample surface morphology can be obtained. Alternatively, the SEM can also be replaced by a TEM, or transmission electron microscope.

[0071] When the elemental composition of a sample needs to be determined, an EDX detector can be installed on the TEM instrument. The EDX detector identifies the elements in the sample and determines their concentration and distribution. This allows accurate determination of C and O.

[0072] As mentioned above, it is necessary to initially separate the graphene from the other components of the composition in order to determine the structural characteristics of the graphene.

[0073] According to the embodiments described in the above patent documents, the process for producing graphene is carried out continuously by continuously feeding graphite flakes into a high-temperature expansion step, continuously discharging the obtained expanded graphite into an aqueous medium, and continuously exfoliating and reducing the size of the expanded graphite dispersed in the aqueous medium using an ultrasonic and / or high-pressure homogenization method.

[0074] As described in these patent documents, the final dispersion of graphene nanosheets obtained can be concentrated or dried, depending on the final morphological requirements of the graphene.

[0075] The goal of drying the dispersion is to obtain a dry powder that is easily redispersible in a variety of matrices, including solvents and polymers, where liquids are undesirable or manageable at the process level, or where water cannot be used due to chemical incompatibility.

[0076] A significant advantage of the production process described in the above patent document is that it can be operated without the use of surfactants. In fact, the graphene nanosheets thus obtained are of high purity, both due to the high C / O ratio and due to the absence of foreign substances (such as surfactants) that could contaminate them. In fact, the conductivity of graphene without surfactant is significantly higher than that of graphene produced using a surfactant process. This improves the performance of graphene in many applications.

[0077] Graphene nanosheets with the above lateral dimensions, thickness (z), and C / O ratio have high electrical conductivity.

[0078] The binder of the granular composition of the present invention is a wetting and dispersing agent selected from the following groups: Polyurethane oligomers and polyurethane polymers, wherein the modified polyurethane content is 100%; nonionic surfactants including fatty acid ethoxylates, alcohol ethoxylates and ethoxylated sorbitan esters, preferably free of alkylphenol ethoxylates (APEO) and volatile organic compounds (VOCs), including sorbitan monooleate; Anionic surfactants, preferably free of alkylphenol polyoxyethylene ethers (APEO) and volatile organic compounds (VOC); including sodium polynaphthyl methane sulfonate, polymers containing ethylene oxide, sodium polyphosphate, sodium polyacrylate; Phosphate esters and their salts, including 6-ethoxy and 9-ethoxytridecyl phosphate; Aldehyde and ketone resins; Epoxidized soybean oil; Polyethers modified with phosphate groups and their salts; Fatty acid modified polyester Polymers and copolymers having pigment-affinity groups, including modified polyethers having high pigment-affinity groups; 2,5-furandione, telomer with 1,1'(1,1-dimethyl-3-methylene-1,3-propanediyl)bis(benzene) and ethynylbenzene, 3(dimethylamino)propyl imide, imide with polyethylene polypropylene glycol 2-aminopropyl methyl ether, quaternized benzoic acid salt of 2[(C1016 alkoxy)methyl]ethylene oxide; Sodium polycarboxylate; A mixture of 5-chloro-2-methyl-2-hydrogen-isothiazol-3-one and 2-methyl-2-hydrogen-isothiazol-3-one (CASN° 55965-84-9).

[0079] As regards the nonionic, APEO- and VOC-free surfactants, these preferably have a pH of 5 to 7 and a viscosity of at most 100 s, the latter being measured in accordance with DIN EN ISO 2431, flow cup 6 mm, 23° C.

[0080] Regarding aldehyde resins and ketone resins, product examples are sold by BASF The products have an average molecular weight between 800 and 2000 Da and a melting point between 70 and 130 °C.

[0081] As regards copolymers having pigment-affinic groups, an example is the product sold under the trademark Byk 2055 by BYK-Chemie.

[0082] As for non-ionic wetting agents and emulsifiers that do not contain alkylphenols, Elementis’ Nuosperse FN265 Products sold under the trademark.

[0083] In particular, according to the invention, the wetting and dispersing additive is selected from the following commercial products: -Disperbyk 2055 is an acrylate copolymer or acrylic acid copolymer. It has pigment-affinic groups. DISPERBYK-2055 is a high molecular weight wetting and dispersing additive with a solids content of 100%. -Disperbyk 2013 is a structural copolymer with a comb-like structure, the CPT group being specifically a styrene-maleic anhydride copolymer with quaternized groups. -Disperbyk-180, an alkyl ammonium salt of a phosphate ester; -Disperbyk2012, modified styrene maleic acid copolymer solution -Atmer 110-116, an ethoxylated sorbitan ester. Physical form: liquid; Source: vegetable / synthetic; -Tegodispers 650, a nonionic wetting and dispersing agent suitable for water-based and solvent-based products; - Gen0451, a solvent-free polyurethane oligomer; high molecular weight wetting and dispersing additive for waterborne and solventborne coating systems. VOC-free, APEO-free, 100% active. - Cliqsperse LP2004-1, an amine-functionalized styrene-maleic anhydride imine copolymer;

[0084] The above-mentioned various types of binders have a high affinity for the pigment, filler and graphene constituting the particle composition of the present invention. They ensure the stabilization of the pigments, fillers and nanographene particles constituting the composition, thereby stabilizing the particles of the composition. Additionally, the binder stabilizes the dispersion of the particles in the composition.

[0085] The granular composition of the present invention may be prepared by mixing the components in a turbine mixer apparatus.

[0086] The turbine mixer device is a high shear granulator comprising a cylindrical container with at least one feed opening and one discharge opening, and optionally equipped with a heating and / or cooling jacket to achieve and / or maintain the temperature in the container at a predetermined temperature. In the chamber inside the container, a rotating shaft is mounted, on which at least one impeller with blades is mounted. The container is closed by a top cover. Figure 1A , 1B and 1C show a partial schematic diagram of the device, in which the top cover is not shown.

[0087] like Figure 1A As shown, the particulate material, graphene nanosheets and binder are fed into a turbine mixer device. The impeller rotates so that the blades reach a peripheral speed of 4 to 50 m / s. The mixing is carried out at a temperature of 20 to 150°C.

[0088] like Figure 1B As shown, the device removes the mixture of graphene, binder, pigment and / or filler from a static stage, and pushes it to form a tornado-like vortex that is enclosed in a cylindrical cavity and begins to rotate from the bottom to the top of the cavity. The mixture then collapses and moves under the influence of gravity towards the middle of the cavity, as Figure 1C As shown, Due to the obstruction of the top cover, the mixture falls to the lower part of the container, where it is pushed upward and outward again, forming a spiral rise. The vortex created by this effect ensures mixing and agglomeration of the particles, resulting in dust-free, free-flowing particles.

[0089] The presence of the impeller cuts off the vortex and counteracts the advancement of the particles, thus ensuring the dispersion of any tiny agglomerates, providing the best dispersion of graphene and making it evenly distributed within the particles. Under the rotation and cutting action of the vortex, the mechanical energy of mixing / agglomeration is converted into heat energy.

[0090] Preferably, the rotating shaft comprises 1 to 7 impellers, more preferably 4 impellers, which are mounted in series on the rotating shaft.

[0091] Preferably, the turbine mixer apparatus comprises a heating and / or cooling jacket for controlling the temperature of the chamber in which the components are mixed.

[0092] Preferably, the temperature is between 30°C and 150°C, more preferably between 60 and 120°C.

[0093] Preferably, the total time for carrying out the process is between 5 and 60 minutes.

[0094] According to one aspect of the invention, the binder is introduced into the turbine mixer gradually, ie is fed in a continuous manner over time.

[0095] According to one aspect of the present invention, the preparation of the composition of the present invention is carried out in a discontinuous manner, for example, in a batch mode rather than a continuous mode.

[0096] According to one aspect of the present invention, the preparation method of the composition of the present invention is carried out without using any solvent, that is, it is basically a dry process. The so-called "dry process" means that the amount of liquid in the preparation process is not higher than 5% by weight of the entire composition.

[0097] Specifically, the term "solvent" refers to a substance or mixture of substances that can dissolve or disperse other substances and is liquid at room temperature, i.e. between 20 and 40°C, such as a non-polar solvent, a polar deactivating solvent, a polar protic solvent or any mixture thereof, including a diluent that does not dissolve any component in the mixture.

[0098] According to one aspect, the present invention relates to a dispersion of the above defined particulate composition in a liquid selected from water and an organic solvent, wherein the term "solvent" has the same meaning as above.

[0099] The above compositions can be used to produce water-based and solvent-based dispersions. These dispersions (if the amount of liquid is relatively small, they can also be defined as "pastes") that can be further processed in a variety of applications, especially in surface coating applications, such as the production of paints, etc.

[0100] Due to the presence of graphene, the use of this dispersion on substrates (especially on the surface of non-conductive substrates) can form thermally and electrically dispersive coatings, thereby improving the performance and quality of the coating. The use of this dispersion on these substrates can indeed obtain a coating that is essentially conductive and heat-dissipating.

[0101] The following examples illustrate some embodiments of the invention and are provided by way of non-limiting illustration. Example

[0102] The apparatus used for preparing the granular composition of the present invention is a turbine mixer having a container with a capacity of 20 liters and equipped with 4 impellers.

[0103] Graphene nanosheets were produced by DirectaPlus S.pA. and the particle sizes are stated in each example below. Example 1

[0104] Preparation of CP701 composition

[0105] Add 4450 g of barium sulfate and 6.5 g of DirectaPlus S.pA's graphene PureG+ into the turbine mixer. and 543.5 g of the wetting agent Disperbyk 2013 (Byk-Chemie), which is a styrene-maleic anhydride copolymer with quaternary ammonium groups.

[0106] Graphene PureG+ consists of graphene nanosheets, at least 90% (D90) of which have a lateral dimension less than 9905 nm and a thickness of 8 nm. The C / O ratio is 40 / 1.

[0107] The mixture was mixed at a temperature of 75°C for 20 minutes at a peripheral speed of 23 m / s, and then a granular composition was discharged, the particle size of which was less than 1500 microns and the weight content was as follows: Barium sulfate (filler): 89% Graphene nanosheets: 0.13% Binder: 10.87% Example 2

[0108] Preparation of CP702 composition

[0109] Add 4450 g of barium sulfate and 31.5 g of DirectaPlus S.pA's graphene PureG+ into the turbine mixer. and 518.5 g of the wetting agent Disperbyk 2013 (Byk-Chemie), a styrene-maleic anhydride copolymer with quaternary ammonium groups.

[0110] Graphene PureG+ consists of graphene nanosheets, at least 90% (D90) of which have a lateral dimension less than 9305 nm and a thickness of 14 nm. The C / O ratio is 47 / 1.

[0111] The mixture was mixed at a temperature of 80°C for 20 minutes at a peripheral speed of 36 m / s, and then a granular composition was discharged, the particle size of which was less than 1000 microns and the weight content was as follows: Barium sulfate (filler): 89% Graphene nanosheets: 0.63% Adhesive: 10.37% Example 3

[0112] Preparation of CP703 composition

[0113] Add 4450 g of barium sulfate and 6.5 g of DirectaPlus S.pA's graphene PureG+ into the turbine mixer. and 543.5 g of the wetting agent Disperbyk 2013 (Byk-Chemie), a styrene-maleic anhydride copolymer with quaternary ammonium groups.

[0114] Graphene PureG+ consists of graphene nanosheets, at least 90% (D90) of which have a lateral dimension less than 8570 nm and a thickness of 13 nm. The C / O ratio is 50 / 1.

[0115] The mixture was mixed at a temperature of 75°C for 20 minutes at a peripheral speed of 36 m / s, and then a granular composition was discharged, the particle size of which was less than 1000 microns and the weight content was as follows: Barium sulfate (filler): 89% Graphene nanosheets: 0.13% Binder: 10.87% Example 4

[0116] Preparation of CP704 composition

[0117] Add 4450 g of barium sulfate and 31.5 g of DirectaPlus S.pA's graphene PureG+ into the turbine mixer. And 518.5 grams of wetting agent Cliqsperse LP2004-1 (CLIQ Swiss Tech.

[0118] Graphene PureG+ consists of graphene nanosheets, at least 90% (D90) of which have a lateral dimension of less than 7980 nm and a thickness of 14 nm. The C / O ratio is 60 / 1.

[0119] The mixture was mixed at a temperature of 80°C for 20 minutes at a peripheral speed of 36 m / s, and then a granular composition was discharged, the particle size of which was less than 1500 μm and the weight content was as follows: Barium sulfate (filler): 89% Graphene nanosheets: 0.63% Binder: 10.37% Example 5

[0120] Preparation of CP705 composition

[0121] Add 4300 g of barium sulfate and 150 g of DirectaPlus S.pA graphene into the turbine mixer. Pure G+, and 550 grams of wetting agent Cliqsperse LP2004-1 (CLIQ Swiss Tech).

[0122] Graphene PureG+ consists of graphene nanosheets, at least 90% (D90) of which have a lateral dimension of less than 7000 nm and a thickness of 20 nm. The C / O ratio is 58 / 1.

[0123] The mixture was mixed at a temperature of 75°C for 20 minutes at a peripheral speed of 36 m / s, and then a granular composition was discharged, the particle size of which was less than 1500 microns and the weight content was as follows: Barium sulfate (filler): 86% Graphene nanosheets: 3% Binder: 11% Example 6

[0124] Preparation of CP706 composition

[0125] Add 2200 grams of silica (Syloid 622 from Grace) and 65 grams of graphene Pure G+ from Directa Plus S.pA, as well as 2735 grams of wetting agent Cliqsperse LP2004-1 into the turbine mixer. (CLIQSwissTech.

[0126] Graphene PureG+ consists of graphene nanosheets, at least 90% (D90) of which have a lateral dimension of less than 10,000 nanometers, thickness is 9 nanometers, C / O ratio is 76 / 1.

[0127] The mixture was mixed at a temperature of 75°C for 20 minutes at a peripheral speed of 36 m / s, and then a granular composition was discharged, the particle size of which was less than 1000 microns and the weight content was as follows: Silica (filler): 44% Graphene nanosheets: 1.3% Binder: 54.7% Example 7

[0128] Preparation of CP707 composition

[0129] In the above turbine mixer, add 2450 grams of silicon dioxide (Perkasil from Grace) and 140 grams of DirectaPlus S.pA's graphene PureG+ and 2410 grams of wetting agent Cliqsperse LP2004-1 (CLIQ SwissTech).

[0130] Graphene PureG+ consists of graphene nanosheets, at least 90% (D90) of which have a lateral dimension of less than 5000 nm and a thickness of 6 nm. The C / O ratio is 150 / 1.

[0131] The mixture was mixed at a temperature of 75°C for 20 minutes at a peripheral speed of 36 m / s, and then a granular composition was discharged, the particle size of which was less than 1000 microns and the weight content was as follows: Silica (filler): 49% Graphene nanosheets: 2.8% Binder: 48.2% Example 8

[0132] Preparation ingredient CP708

[0133] In the turbine mixer, add 4600 g of barium sulfate and 250 g of DirectaPlus S.pA's graphene PureG+. and 150 g of the wetting agent Disperbyk 2013 (Byk-Chemie), a styrene-maleic anhydride copolymer with quaternary ammonium groups.

[0134] Graphene PureG+ consists of graphene nanosheets, at least 90% (D90) of which have a lateral dimension of less than 8500 nm and a thickness of 11 nm. The C / O ratio is 93 / 1.

[0135] The mixture was mixed at a temperature of 97°C for 20 minutes at a peripheral speed of 36 m / s, and then a granular composition was discharged, the particle size of which was less than 150 μm and the weight content was as follows: Barium sulfate (filler): 92% Graphene nanosheets: 5% Binder: 3% Example 9

[0136] Preparation ingredient CP709

[0137] In the turbine mixer, add 4400 g of barium sulfate and 250 g of DirectaPlus S.pA graphene PureG+. and 350 g of the wetting agent Disperbyk 2013 (Byk-Chemie), a styrene-maleic anhydride copolymer with quaternary ammonium groups.

[0138] Graphene PureG+ consists of graphene nanosheets, at least 90% (D90) of which have a lateral dimension of less than 8500 nm and a thickness of 11 nm. The C / O ratio is 93 / 1.

[0139] The mixture was mixed at a temperature of 97°C for 20 minutes at a peripheral speed of 36 m / s, and then a granular composition was discharged, the particle size of which was less than 150 μm and the weight content was as follows: Barium sulfate (filler): 88% Graphene nanosheets: 5% Binder: 7% Example 10

[0140] Preparation of CP710 composition

[0141] In the turbine mixer, add 4200 g of barium sulfate and 500 g of DirectaPlus S.pA graphene PureG+. and 300 g of the wetting agent Disperbyk 2013 (Byk-Chemie), a styrene-maleic anhydride copolymer with quaternary ammonium groups.

[0142] Graphene PureG+ consists of graphene nanosheets, at least 90% (D90) of which have a lateral dimension of less than 7500 nm and a thickness of 2.5 nm. The C / O ratio is 85 / 1.

[0143] The mixture was mixed at a temperature of 97°C for 20 minutes at a peripheral speed of 36 m / s, and then a granular composition was discharged, the particle size of which was less than 150 μm and the weight content was as follows: Barium sulfate (filler): 84% Graphene nanosheets: 10% Binder: 6% Example 11

[0144] Preparation of UP301 composition

[0145] In the above turbine mixer, add 4250 g of iron oxide red pigment (Bayferrox 130 from Lanxess) and 6.5 g of graphene Pure G+ from Directa Plus S.pA, and 743.5 g of wetting agent Disperbyk 180 (Byk-Chemie), which is an alkyl alcohol ammonium salt of a copolymer with acidic groups.

[0146] Graphene Pure G+ consists of graphene nanosheets, at least 90% (D90) of which have a lateral dimension of less than 8670 nanometers, thickness is 14 nanometers. C / O ratio is 90 / 1.

[0147] The mixture was mixed at a temperature of 120°C for 20 minutes at a peripheral speed of 36 m / s, and then a granular composition was discharged, the particle size of which was less than 2000 microns and the weight content was as follows: Iron oxide (pigment): 85% Graphene nanosheets: 0.13% Binders: 14.87% Example 12

[0148] Preparation of composition UP302

[0149] In the above turbine mixer, add 4250 g of iron oxide red pigment (Bayferrox 130 from Lanxess) and 31.5 g of graphene Pure G+ from Directa Plus S.pA, and 718.5 g of wetting agent Disperbyk 180 (Byk-Chemie), which is an alkyl alcohol ammonium salt of a copolymer with acidic groups.

[0150] Graphene PureG+ consists of graphene nanosheets, at least 90% (D90) of which have a lateral dimension of less than 7980 nm and a thickness of 13 nm. The C / O ratio is 130 / 1.

[0151] The mixture was mixed at a temperature of 120°C for 20 minutes at a peripheral speed of 36 m / s, and then a granular composition was discharged, the particle size of which was less than 2000 microns and the weight content was as follows: Iron oxide (pigment): 85% Graphene nanosheets: 0.63% Binders: 14.37% Example 13

[0152] Preparation of UP201 composition

[0153] In the turbine mixer, 3900 g of iron oxide yellow transparent pigment (BASF's Sicotan Yellow L1916) and 12.5 g of Directa Plus S.pA's graphene Pure G+ and 1087.5 g of wetting agent Disperbyk 180 were added. (Byk-Chemie), which is an alkyl alcohol ammonium salt of a copolymer with acidic groups.

[0154] Graphene PureG+ consists of graphene nanosheets, at least 90% (D90) of which have a lateral dimension of less than 10100 nanometers, thickness is 15 nanometers, C / O ratio is 130 / 1.

[0155] The mixture was mixed at a temperature of 110°C for 25 minutes at a peripheral speed of 36 m / s, and then a granular composition was discharged, the particle size of which was less than 2000 microns and the weight content was as follows: Iron oxide (pigment) 78% Graphene nanosheets 0.25% Binder: 21.75% Example 14

[0156] Preparation of composition UP202

[0157] In the above composition, 3800 g of iron oxide yellow transparent pigment (Sicotan Yellow L1916 from BASF), 62.5 g of graphene Pure G+ from Directa Plus S.pA, and 1137.5 g of wetting agent Disperbyk 180 were added. (Byk-Chemie), which is an alkyl alcohol ammonium salt of a copolymer with acidic groups.

[0158] Graphene Pure+ consists of graphene nanosheets, at least 90% (D90) of which have a lateral dimension of less than 9170 nanometers. The thickness is 19 nm. The C / O ratio is 100 / 1.

[0159] The mixture was mixed at a temperature of 120°C for 25 minutes at a peripheral speed of 36 m / s, and then a granular composition was discharged, the particle size of which was less than 2000 microns and the weight content was as follows: Iron oxide (pigment): 76% Graphene nanosheets: 1.25% Binder: 22.75% Example 15

[0160] Preparation of dispersions in water

[0161] The compositions of Examples 2, 4, 5, 6, 8 and 9 were used to prepare dispersions in deionized water containing 75 wt% of the composition and 0.5 wt% of the wetting and dispersing agent Edaplan 490 (nonionic surfactant free of APEO and VOC). The disperser used was a BYK Dispermat CV equipped with 20-40 mm unshielded blades, rotating at a speed of 4000 revolutions per minute for 4 minutes. The wettability of the composition was very good and no solid lumps were formed. The dispersion was After storage at 40°C for 7 days, no precipitation and no gel formation occurred.

[0162] These dispersions are pastes suitable for preparing anticorrosion coatings. Example 16

[0163] Preparation of water-based anti-corrosion coatings.

[0164] A dispersion of the composition CP708 of Example 8 prepared in water as described in Example 14 was used to prepare a water-based anticorrosive coating having the composition described in Table 1 below. The coating was prepared by mixing the various ingredients in a container. One ingredient was added to the container at a time. For ingredients that were unstable in water, such as organic molecules, organic solvents, or anticorrosive additives, these ingredients were first pre-dispersed in water and then gradually added to the final matrix to prevent coagulation.

[0165] Table 1 Example 17

[0166] Preparation of water-based anti-corrosion coatings.

[0167] The dispersion of the composition CP709 of Example 9 prepared in water according to the method described in Example 14 was used to prepare a water-based anticorrosive coating having the composition described in the following Table 2. The components were mixed according to the method described in Example 15 to prepare the coating.

[0168] Table 2 Example 18 (Comparative Example)

[0169] Preparation of water-based anti-corrosion coatings.

[0170] For comparison purposes, a dispersion of barium sulfate alone in water prepared as described in Example 14, which was not formulated into the granular composition of the present invention, was used to prepare a waterborne anticorrosive coating having the composition described in Table 3 below. The coating was prepared by mixing the ingredients as described in Example 15.

[0171] Table 3 Example 19

[0172] Testing of water-based anti-corrosion coatings.

[0173] The coatings were used to prepare the test specimens according to DIN EN ISO 1513. A 5.5x15 cm circular steel plate with a single hole was coated with two layers of paint, each with a thickness of 200 microns. The panel was then dried at 20°C and 55% humidity for 72 hours.

[0174] Testing samples after first coat of paint

[0175] According to the requirements of the DIN EN ISO 17872 standard corrosion test method, a 2 mm wide score is made on the paint layer. Then use the tape Tesa 4124 Ultra Strong to cover the edge and back of the steel plate. Then according to DIN EN ISO 9227 (Salt spray test) The corrosion test was carried out under the conditions of 40±2°C and 80±5% humidity.

[0176] After 500 hours of exposure to salt spray, the steel panels were scratched at the markings before testing. The degree of penetration and diffusion of the salt spray was then evaluated by measuring how much of the coating fell off the sample surface. To determine whether the shedding was due to the penetration of salt spray, the samples were rubbed after a cut was made on the panel to evaluate the proper adhesion of the coating. None of the three samples in this example showed signs of shedding due to low adhesion of the coating to the bracket.

[0177] The data in Table 4 show that after replacing barium sulfate with the components of compositions CP708 and 709, the permeability resistance was improved by 48% and 46%.

[0178] Table 4

[0179] Testing samples after second coat of paint

[0180] The second series of samples used a double coating and were subjected to the same salt spray test after 500 hours. The results are shown in Table 5:

[0181] Table 5

[0182] The samples made with the double coating showed no signs of peeling due to poor adhesion between the coating and the substrate. The data in Table 5 show that replacing barium sulfate with CP708 and 709 improves the permeation resistance by 17% and 12%, respectively.

[0183] The incorporation tests with predispersions made with compositions 708 and 709 were successful. The complete replacement of barium sulfate with the composition of the invention significantly reduced the penetration of salt spray, thereby improving corrosion resistance. This effect was more pronounced on samples coated with a single layer of coating, but was still visible on the double layer samples. Example 20

[0184] Preparation of solvent-based anti-corrosion coatings. The composition CP708 of Example 8 was used to prepare a solvent-based anti-corrosion coating, and its composition is described in Table 6 below. The coating was prepared by mixing the ingredients as described in Example 15. The ingredients were added individually to the coating mixing vessel, but no pre-dispersion was required as the ingredients were stable in the solvent.

[0185] Table 6

[0186] Table 7

[0187] Table 8

[0188] Table 9

[0189] Table 10 (Comparison) Reference coating

[0190] The reference coating in Table 10 is a standard solvent-based anticorrosive formulation. One of the two inorganic fillers was substituted for this standard composition. One comparison was made with CP708 (Table 7) or CP709 (Table 9) Replacement of part of the inorganic filler BaSO4. Another comparison is to replace part of the inorganic corrosion inhibitor with CP708 (Table 6) and CP709 (Table 8).

[0191] The corrosion resistance was evaluated according to DIN EN ISO 9227 and the test time of these samples was 900 hours as described in Example 18. The data in Table 9 show that replacing 5 percent of zinc phosphate with compositions CP708 and CP709 increases the permeation resistance by 42% and 58%, respectively.

[0192] Tests in which compositions CP708 and CP709 were added directly to the final coating were successful. After replacing barium sulfate with the composition of the invention, salt spray penetration was significantly reduced while corrosion resistance was enhanced. This effect was more pronounced in the samples using CP708, but was still visible in the samples using CP709.

[0193] Table 9

Claims

1. A granular composition comprising: a) 20 to 95% by weight of particulate material, the particulate material being a filler; b) 0.02 to 50 wt. % of graphene nanoplatelets; c) 0.5 to 60% by weight of a binder; in, At least 90% of the graphene nanosheets have a lateral dimension (x, y) of 50 to 20,000 nanometers, a thickness (z) of 1 to 50 nanometers, and a C / O ratio of ≥40:

1.

2. The granular composition according to claim 1 or 2, wherein The particulate material also includes pigments.

3. The granular composition according to claim 1 or 2, characterized in that The particle size of the particles of the granular composition is between 50 and 4000 microns, and the particles are screened by a digital electromagnetic vibration screen. Vibrationmod.FTL0200 measurement.

4. The granular composition according to claim 1 or 2, characterized in that The filler is selected from the group consisting of calcium carbonate; kaolin; mica; talc; silica; barium sulfate; zinc phosphate; calcium phosphate; organic stearates and metal stearates such as aluminum, barium, calcium, magnesium, tin and zinc stearates; aluminum silicate; and any combination thereof.

5. The granular composition according to claim 1 or 2, characterized in that The binder is a wetting and dispersing agent.

6. The granular composition according to claim 1 or 2, characterized in that The binder is a wetting and dispersing agent selected from the group consisting of: Polyurethane oligomers and polyurethane polymers, with a modified polyurethane content of 100%; nonionic surfactants including fatty acid ethoxylates, alcohol ethoxylates and ethoxylated sorbitan esters, preferably free of alkylphenol ethoxylates (APEO) and volatile organic compounds (VOCs), including sorbitan monooleate; Anionic surfactants, preferably free of alkylphenol ethoxylates (APEO) and volatile organic compounds (VOC); Including sodium polynaphthyl methane sulfonate, polymers containing ethylene oxide, sodium polyphosphate, sodium polyacrylate; Phosphates and their salts, including 6-ethoxy and 9-ethoxy tridecyl phosphate; Aldehyde and ketone resins; Epoxidized soybean oil; Polyethers modified with phosphate groups and their salts; Fatty acid modified polyester Polymers and copolymers having pigment-affinity groups, including modified polyethers having high pigment-affinity groups; 2,5-furandione, telomer with 1,1'(1,1-dimethyl-3-methylene-1,3-propanediyl)bis(benzene) and ethynylbenzene, 3(dimethylamino)propyl imide, imide with polyethylene polypropylene glycol 2-aminopropyl methyl ether, quaternized benzoic acid salt of 2[(C1016 alkoxy)methyl]ethylene oxide; Sodium polycarboxylate; A mixture of 5-chloro-2-methyl-2-hydrogen-isothiazol-3-one and 2-methyl-2-hydrogen-isothiazol-3-one (CASN° 55965-84-9).

7. The granular composition according to claim 2, characterized in that The pigment is selected from the group consisting of: P.Yellow 42; P.Yellow 184; P.Yellow.216; P.Red 101;P.Red 254;P.Red 122; P.Violet23; P.Violet 19;P.Blu 15:1;P.Blu 15:3;P.Blu 15:2;P.Blu 15:4;P.Blu 60;P.Green.7;P.Brown.24;P.Black.7; P.Black.

6.

8. The granular composition according to claim 1 or 2, characterized in that The granular composition does not contain zinc phosphate or calcium phosphate.

9. A method for preparing a granular composition, comprising: a) 20 to 95% by weight of particulate material, said particulate material being a filler; b) 0.02 to 50 wt % of graphene nanoplatelets, wherein the graphene nanoplatelets have a lateral dimension (x, y) of 50 to 20,000 nm, a thickness (z) of 1 to 50 nm, and a C / O ratio of ≥40:1; c) 0.5 to 60% by weight of a binder; in, The particulate material, the graphene nanoplatelets and the binder are mixed in a turbo-mixer device equipped with at least one impeller whose blades rotate at a peripheral speed of 4 to 50 m / s, and the method is carried out at a temperature of 20 to 150°C. The method according to claim 6, characterized in that the turbine mixer device comprises a rotating shaft and a heating and / or cooling jacket for controlling the temperature, and the rotating shaft is equipped with 1 to 7 impellers installed in series.

10. The method according to claim 9, wherein: The particulate material also includes pigments.

11. The method according to claim 9 or 10, characterized in that: The total operation time of the method is from 5 to 60 minutes.

12. A dispersion of the granular composition of claim 1 or 2 in a liquid selected from water and an organic solvent.

13. Use of the particle composition according to claim 1 or 2, or the dispersion according to claim 8, for preparing a coating, a varnish or an ink.

14. A coating comprising the particle composition of claim 1 or 2.

Citation Information

Patent Citations

  • Ternary polymerized graphene nanometer anti-corrosion coating and preparation technique

    CN107325686A

  • Graphene modified epoxide anticorrosive coating and preparation method thereof

    CN109777253A

  • Thin-layer graphene dispersion slurry and preparation method and application thereof

    CN109943127A

  • Thin-layer graphene aqueous slurry and preparation method and application thereof

    CN109943128A

  • Graphene modified inorganic anticorrosive coating, preparation method thereof and graphene modified inorganic anticorrosive coating layer

    CN111471333A