Sealing device
By using a vulcanized sealing material with modified rubber composition and filler, the problem of oxidation and decomposition of natural rubber at high temperature is solved, high mechanical strength and compression resistance at high pressure and high temperature are achieved, and the stability of sealing performance is improved .
Patent Information
- Application Number
- CN202380031439.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-31
- Filing Date
- 2023-03-30
- Publication Date
- 2024-11-15
AI Technical Summary
Existing natural rubber sealing materials are prone to oxidation and decomposition in high-temperature air, resulting in decreased mechanical strength and permanent deformation, making it difficult to maintain sealing performance under high pressure and high temperature conditions.
Using a rubber composition, including natural rubber, epoxidized modified natural rubber, carbon black or silica filler, organic peroxide crosslinking agent and silane coupling agent, the sealing main part is manufactured by vulcanized molding products to ensure that Maintain high mechanical strength at high pressure and reduce compression permanent deformation at high temperatures.
The high mechanical strength, low temperature cold resistance and high temperature compression resistance of sealing materials under high pressure and high temperature conditions are achieved, which significantly improves the stability of sealing performance.
Smart Images

Figure CN118974450A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a sealing device. Background Art
[0002] In October 2020, the Japanese government announced that it would achieve carbon neutrality with zero greenhouse gas emissions by 2050. In terms of raw materials, switching from petroleum resources to plant resources that absorb carbon dioxide can contribute to carbon neutrality. As a plant resource, natural rubber made from tree sap has excellent mechanical strength and cold resistance, so it is advantageous for the application of materials requiring high sealing properties. As an example of the use of such natural rubber, hydrogen sealing materials can be cited.
[0003] In a hydrogen society, which is expected to be a means of decarbonization, carbon dioxide is not emitted when energy is used. In order to realize a hydrogen society, hydrogen stations and fuel cell vehicles have been put into practical use, but sealing technology that can safely manage hydrogen without leakage under high pressure and in a wide temperature range is required. Therefore, the combination of hydrogen application and natural rubber brings a synergistic decarbonization effect, and further, it can be expected that cracks in sealing products under high pressure will be suppressed and elasticity reduction (cold resistance) at low temperatures will be improved.
[0004] However, in general, diene rubbers such as natural rubber have the property of being easily thermally degraded. If natural rubber is exposed to high-temperature air for a long time in a compressed state, stress relaxation due to oxidative decomposition will occur, and permanent deformation will remain after compression is released. Such a phenomenon is fatal to sealing products that use the restoring force of rubber to seal fluids. Therefore, in order to use natural rubber as a hydrogen sealing material, it is necessary to improve the resistance to compression permanent deformation in high-temperature air.
[0005] Patent Document 1 describes a sealing material for a high-pressure hydrogen container for a fuel cell vehicle that can withstand changes in pressure or temperature, and cites natural rubber as one type of rubber that can be applied. However, Patent Document 1 does not mention the improvement of the compression set resistance of natural rubber in high-temperature air because the sealing performance in a high-temperature hydrogen atmosphere is the object rather than in a high-temperature air atmosphere. In addition, the exposure time to high-temperature hydrogen is also relatively short, at 1 hour, and there is no record of the matching information of the rubber material that can achieve the desired performance.
[0006] Therefore, there is a need to review natural rubber sealing materials that have high mechanical strength under high pressure, show excellent cold resistance, and further can exhibit excellent resistance to compression set in high-temperature air for a long period of time.
[0007] Prior art literature
[0008] Patent Literature
[0009] Patent Document 1: Japanese Patent Application Publication No. 2008-57711 Summary of the invention
[0010] Technical problem to be solved by the invention
[0011] The present invention provides a sealing device which exhibits high mechanical strength under high pressure and is excellent in cold resistance in a low temperature range and in resistance to compression set in a high temperature range.
[0012] Solutions for solving technical problems
[0013] A sealing device according to an embodiment of the present invention is a sealing device that is arranged between two members facing each other and seals a space between the two members, wherein the sealing device includes a sealing body portion that contacts the space, wherein the sealing body portion has a tensile strength of 10 MPa or more measured in accordance with the provisions of JIS K 6251:2017, an elongation at break measured in accordance with the provisions of JIS K 6251:2017 of 200% or more, a TR10 temperature in a low-temperature elastic recovery test measured in accordance with the provisions of JIS K 6261-4:2017 of -40°C or less, and a compression set of 40% or less after 70 hours at 100°C measured in accordance with the provisions of JIS K 6262:2013 according to the shape of a G25 O-ring described in the provisions of JIS B 2401-1:2012.
[0014] In one embodiment of the present invention, the sealing body is annular.
[0015] In one embodiment of the present invention, the sealing body portion is held by a support ring.
[0016] In one embodiment of the present invention, the cross-sectional shape of the sealing body portion is a protrusion shape.
[0017] In one embodiment of the present invention, the sealing body portion is provided on a plate-shaped substrate, and the substrate is a plate made of metal or carbon.
[0018] In one embodiment of the present invention, the substrate and the sealing body portion are bonded to each other by an adhesive contained in the sealing body portion.
[0019] In one embodiment of the present invention, the sealing body portion is in contact with hydrogen gas.
[0020] In one embodiment of the present invention, the sealing body portion is in contact with liquid hydrogen.
[0021] In one embodiment of the present invention, the sealing device is a sealing device used in a hydrogen energy system.
[0022] A sealing device according to another embodiment of the present invention is a sealing device which is arranged between two components facing each other and seals the space between the two components, wherein the sealing device includes a sealing main body portion which contacts the space, and the sealing main body portion is a vulcanized molded product of a rubber composition, wherein the rubber composition contains: (A) a natural rubber component selected from natural rubber and epoxy-modified natural rubber having an epoxidation degree of greater than 1% and less than 50%; (B) a filler selected from carbon black and silica; (C) an organic peroxide-based crosslinking agent; and any (D) a silane coupling agent (wherein, when the filler is carbon black, the rubber composition contains epoxy-modified natural rubber having an epoxidation degree of greater than 1% and less than 50%, and when the filler is silica, the rubber composition also contains a silane coupling agent).
[0023] In one embodiment of the present invention, the rubber composition further contains (E) at least one additive selected from the group consisting of a cross-linking accelerator, an auxiliary agent, and an antioxidant.
[0024] Effects of the Invention
[0025] According to the present invention, it is possible to provide a sealing device which exhibits high mechanical strength under high pressure and is excellent in cold resistance in a low temperature range and in resistance to compression set in a high temperature range. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 It is a cross-sectional view of a main part of a sealing device according to an embodiment of the present invention.
[0027] Figure 2 About Figure 1 The sealing device shown is a cross-sectional view of a sealing device according to another embodiment.
[0028] Figure 3 It is a schematic diagram of a sealing device according to another embodiment of the present invention.
[0029] Figure 4 yes Figure 3 A schematic cross-sectional view of a sealing arrangement is shown.
[0030] Figure 5 This is a schematic diagram showing the shape of a test piece produced when measuring the mechanical strength of the test piece A obtained in the example and the comparative example.
[0031] Figure 6 This is a schematic diagram showing the cross-section of the shape of a test piece produced when measuring compression set using the test piece B obtained in the example and the comparative example. DETAILED DESCRIPTION
[0032] Hereinafter, the sealing device according to the embodiment of the present invention will be described in detail with reference to the drawings. It should be noted that the room temperature described below is within the range of 23°C ± 2°C.
[0033] <Sealing device>
[0034] The sealing device of this embodiment is disposed between two components facing each other and seals the space between the two components, and includes a sealing body in contact with the space. The sealing device of this embodiment is preferably used in a hydrogen energy system, in which case the sealing body is in contact with hydrogen or liquid hydrogen, and the sealing device is used as a hydrogen gas seal or a liquid hydrogen seal.
[0035] <First embodiment>
[0036] Figure 1 This is an example of an embodiment of a sealing device including such a sealing body portion. Figure 1 The sealing device 1 shown is mounted in the mounting groove (mounting portion) 4 of one member 2 of two members 2 and 3 facing each other and in close contact with the other member 3, thereby sealing between the two members 2 and 3. The sealing device 1 includes a sealing ring (rubber annular seal ring) 11 made of a rubber elastic body, a first support ring (support ring) 21 arranged on the low pressure side L of the sealing ring 11, and a second support ring 31 arranged between the sealing ring 11 and the first support ring 21. The two members 2 and 3 are, for example, high pressure hydrogen pipes for fuel cells connected to each other, and the sealing housing portion of the other pipe member 3 is arranged on the outer peripheral side of the sealing housing portion of the one pipe member 2, and the sealing device 1 is mounted in the annular mounting groove 4 provided on the outer peripheral surface of the sealing housing portion of the one pipe member 2, and in close contact with the inner peripheral surface of the sealing housing portion of the other pipe member 3. The sealing fluid is high pressure hydrogen gas to flow from the high pressure side H to the low pressure side L.
[0037] As the first support ring 21, a support ring made of nylon (trade name) is used. Nylon is one of the resin materials that is difficult for gas to pass through. In addition, as the second support ring 31, a support ring made of a material softer than the first support ring 21, such as PTFE resin, is used. For ease of assembly, both support rings 21 and 31 are mostly used as joint rings with a portion of the circumference cut off. In the case of considering gas leakage, it is preferable to use a jointless type without cutting.
[0038] The seal ring 11 corresponds to the seal main body of the sealing device of the present invention. The seal ring 11 is formed in an annular shape and is held by the first and second support rings 21 and 31. The material of the seal ring 11 is the same as the material forming the seal main body described later, or the seal ring 11 shows the characteristics of the seal main body described later.
[0039] The mounting groove 4 is basically formed as a space with a rectangular cross section, but the high-pressure side mounting portion 4a in the bottom of the groove for mounting the seal ring 11 is formed in a flat cylindrical surface. In addition, the low-pressure side mounting portion 4b for mounting the first and second support rings 21 and 31, which is continuous with the low-pressure side L of the high-pressure side mounting portion 4a, is formed in an inclined surface shape of a conical surface in such a manner that the interval (radial interval) between the two members 2 and 3 gradually narrows from the high-pressure side H toward the low-pressure side L, that is, in such a manner that the groove depth of the mounting groove 4 gradually becomes shallower, thereby forming an inclined bottom surface 4c.
[0040] In addition, the first and second support rings 21 and 31 mounted on the low-pressure side mounting portion 4b are basically formed into a rectangular cross-section, but the inner circumferential surfaces of the first and second support rings 21 and 31 are formed into a conical inclined surface in a manner corresponding to the inclined bottom surface 4c so that their inner diameter dimensions gradually increase from the high-pressure side H toward the low-pressure side L, thereby forming inclined surfaces 21a and 31a.
[0041] In the sealing device 1 of such a structure, when Figure 1 When pressure P acts on the right side of the seal ring 11, the seal ring 11 is pressed against the second support ring 31 on the low-pressure side, but the second support ring 31 is molded of PTFE resin, which is softer than the first support ring 21 made of nylon. Therefore, it is possible to prevent the seal ring 11 from being repeatedly pressed against a hard material and being damaged when alternating pressure is generated. In addition, since the second support ring 31 is molded of PTFE resin, which is a soft material, overflow is likely to occur, but overflow is prevented by the first support ring 21, which is molded of nylon, which is a hard material.
[0042] In addition, the assembly groove 4 is provided with an inclined bottom surface 4c that gradually narrows the interval between the two components 2 and 3 from the high-pressure side H to the low-pressure side L, and the two support rings 21 and 31 are provided with inclined surfaces 21a and 31a corresponding to the inclined bottom surface 4c on the inner circumferential surface. As a result, when the sealing fluid pressure acts on the two support rings 21 and 31 through the sealing ring 11, the two support rings 21 and 31 are compressed in a form (shape) pressed into a narrow part and strongly and closely contact with each other. Therefore, since the compression phenomenon caused by the above-mentioned inclined surfaces 21a and 31a occurs in the two support rings 21 and 31, not only is it more difficult for the sealing ring 11 to overflow, but also in the case where the high-pressure hydrogen gas as the sealing fluid cannot be sealed by the sealing ring 11 alone, it can be expected that the support rings 21 and 31 can be used for sealing.
[0043] In addition, the support ring 21 is formed of nylon, which is difficult to pass gas. Therefore, from this aspect, the leakage caused by the high-pressure hydrogen gas as the sealing fluid passing through the support ring 21 can be effectively reduced. Furthermore, since the radial width dimension of the support ring 21 is smaller than the radial width dimension of the second support ring 31, the permeation area is set small. Therefore, from this aspect, the high-pressure hydrogen gas as the sealing fluid can be effectively sealed.
[0044] Furthermore, the sealing device 1 of the present embodiment can be used not only in a cylindrical gap between two members but also in a planar gap, that is, a gap between end faces. Figure 2 This is an example of an embodiment of such a sealing device. Figure 2 In the sealing device 1A at the bottom, in order to seal the cylindrical gap between the one piping member 2 and the other piping member 3, the first to second support rings 21, 31 are arranged in the axial direction, and Figure 2 In the upper sealing device 1B, the first and second support rings 21 and 31 are arranged in the radial direction to seal the planar gap between the one piping member 2 and the other piping member 3. And, by such a double arrangement, leakage to the outside can be further reduced.
[0045] <Second embodiment>
[0046] Figure 3 This is an example of a sealing device according to another embodiment of the present invention. Figure 3 The sealing device 100 shown is a sealing component for a separator stacked on both sides of an electrolyte membrane / electrode assembly (hereinafter referred to as MEA) in a general fuel cell, that is, a single cell seal for a fuel cell. Such a single cell seal for a fuel cell is arranged between the separator and the MEA, which are two components facing each other, to seal the space between the separator and the MEA (not shown). In the separator of the fuel cell, in order to prevent leakage to the outside, it is necessary to supply the fluid for the fuel cell (hydrogen-containing fuel gas, oxygen-containing oxidant gas, etc.) to the MEA, and the sealing gasket with a jointless shape plays the role of sealing (sealing) this fuel cell fluid in the space surrounded by the sealing gasket.
[0047] Figure 3 The sealing device 100 shown in the figure has a plate-like substrate 101 on its surface, and a sealing gasket 102 of a seamless shape made of elastic material and extending along the surface of the substrate 101 is formed around a vent hole 101a. Figure 4 It is shown along Figure 3 The schematic cross section of the sealing device 100 taken along the line AA' of FIG. 1 shows a sealing gasket 102 formed as four protrusions protruding from the surface of the substrate 101. Figure 4As shown in FIG. 1 , the sealing gasket 102 includes a base 102a bonded to the surface of the substrate 101 and a sealing lip 102b protruding from the base 102a in a mountain shape. Figure 3 On the AA′ line, there is a portion (not shown) where the molding material of the gasket 102 flows in and out during molding of the gasket 102 .
[0048] As the substrate 101, for example, a metal plate such as stainless steel, a thin plate such as a carbon plate, etc. is used. The substrate 101 and the sealing gasket 102 are bonded via an adhesive layer or by an adhesive contained in the sealing gasket 102. In addition, the sealing device 100 can also be an integrally molded single cell seal in which a sealing gasket 102 of a jointless shape made of an elastic material and extending along the surface of the substrate 101 is integrally molded on the surface of the plate-like substrate 101. The substrate 101 as such an integrally molded single cell seal is a component included in the single cell structure of the fuel cell that is integrally molded with the sealing gasket 102, and examples thereof include a separator, MEA, a gas diffusion layer (GDL), and the like.
[0049] The sealing gasket 102 corresponds to the sealing body of the sealing device of the present invention. Figure 4 As shown, the cross-sectional shape of the gasket 102 is a protrusion shape. The material of the gasket 102 is the same as the material forming the sealing body part described later, and the gasket 102 shows the characteristics possessed by the sealing body part described later.
[0050] <Seal body>
[0051] The sealing body of the sealing device of the present embodiment is a vulcanized molded product of a rubber composition, which contains: (A) a natural rubber component selected from natural rubber and epoxy-modified natural rubber having an epoxidation degree of 1% or more and less than 50%; (B) a filler selected from carbon black and silica; (C) an organic peroxide-based crosslinking agent; and any (D) a silane coupling agent. Wherein, when the filler is carbon black, the rubber composition contains epoxy-modified natural rubber having an epoxidation degree of 1% or more and less than 50%, and when the filler is silica, the rubber composition also contains a silane coupling agent. Natural rubber is believed to cause an oxidative decomposition reaction starting from a diene structure (C=C bond) in a high-temperature air atmosphere. Therefore, in a rubber composition containing a natural rubber component filled with carbon black, by using an appropriately epoxidized natural rubber, compression set can be suppressed and resistance to compression set in high-temperature air can be improved. Furthermore, by further adding a silane coupling agent to the rubber composition containing the silica-filled natural rubber component, even if the natural rubber is not epoxidized, the compression set resistance in high temperature air can be improved while maintaining excellent cold resistance.
[0052] In this way, when manufacturing the sealing body, by using the above-mentioned specific rubber composition, even if natural rubber is used as the main raw material, it is possible to obtain a sealing body that is not easy to break even under high pressure, has high elastic recovery even in a low temperature range, and has a small compression permanent deformation in a high temperature range, which are the required characteristics of a hydrogen sealing material. As a result, a sealing body exhibits high mechanical strength under high pressure, and can further achieve a sealing device that is excellent in cold resistance in a low temperature range and resistance to compression permanent deformation in a high temperature range.
[0053] The shape of the sealing body is not particularly limited and can be any shape according to the application. For example, the cross-sectional shape can be a sheet-shaped sealing member such as a square, rectangular, or disc-shaped, an annular sealing member such as an O-ring or an angle ring, or these annular portions can be formed on a part of the sealing body.
[0054] (A) Natural rubber ingredients
[0055] As for the natural rubber component, natural rubber that has not been chemically modified or natural rubber that has been epoxidized to a degree of epoxidation of the diene portion of 1% or more and less than 50% is used. Natural rubber is a rubber refined from the sap (latex) of a natural tree, and is a diene rubber different from synthetic rubber produced by chemical synthesis using petroleum, naphtha, etc. as raw materials. The diene portion of the natural rubber can be epoxidized by the reaction of formic acid and hydrogen peroxide. The epoxy-modified natural rubber has a degree of epoxidation of 1% or more and less than 50%, preferably a degree of epoxidation of 10% or more and 40% or less, and more preferably a degree of epoxidation of 20% or more and 30% or less.
[0056] Natural rubber and epoxy-modified natural rubber may be used alone or in combination of two or more. By using such natural rubber, the mechanical properties of the sealing body can be improved. In addition, natural rubber and epoxy-modified natural rubber may also be commercial products. Examples of commercial products of natural rubber and epoxy-modified natural rubber include natural rubber "RSS No. 1" (imported by Toyota Chemiplas), natural rubber "ENR25" with an epoxidation degree of 25% (imported by Sanyo Trading), and the like.
[0057] (B) Filler
[0058] A filler is added to the rubber composition. By including a filler in the rubber composition, the mechanical strength and compression set of the obtained vulcanized product can be improved. As the filler, general carbon black and carbon dioxide are used as reinforcing materials. The filler can be used alone or in combination of two or more.
[0059] Carbon black can be appropriately selected from known materials, for example, hard carbon blacks such as super abrasion resistant (SAF: Super Abrasion Furnace) carbon black, quasi-super abrasion resistant (ISAF: Intermediate Super Abrasion Furnace) carbon black, high abrasion resistant (HAF: High Abrasion Furnace) carbon black and easy processing channel (EPC: Easy Processing Channel) carbon black, and soft carbon blacks such as conductive (XCF: eXtra Conductive Furnace) carbon black, good extrudability (FEF: Fast Extruding Furnace) carbon black, general purpose (GPF: General Purpose Furnace) carbon black, high stress (HFM: High Modulus Furnace) carbon black, medium reinforcement (SRF: Semi-ReinForcing Furnace) carbon black, fine particle thermal decomposition (FT: Fine Thermal) carbon black and medium particle thermal decomposition (MT: Medium Thermal) carbon black. Commercially available products of carbon black include, for example, "Vulcan (registered trademark) 3L" (HAF carbon) manufactured by Cabot Corporation. The content of carbon black is not particularly limited, but is preferably 1 part by mass or more and 100 parts by mass or less, and more preferably 25 parts by mass or more and 75 parts by mass or less, relative to 100 parts by mass of the natural rubber component. Carbon black may be used alone or in combination of two or more.
[0060] Silica can be appropriately selected from known materials, but preferably has good mixing operability. Regarding the silica generally used, dry silica manufactured by a method such as a thermal decomposition method of halogenated silicic acid or an organosilicon compound, or a method of heating and reducing silica sand and air oxidation of gasified SiO, wet silica manufactured by a thermal decomposition method of sodium silicate, etc. can be cited. As a commercially available product of silica, for example, "Ultrasil (registered trademark) 360" manufactured by Evonik Japan Co., Ltd. can be cited. The content of silica is not particularly limited, but relative to 100 parts by mass of the natural rubber component, it is preferably more than 1 part by mass and less than 100 parts by mass, and more preferably more than 25 parts by mass and less than 75 parts by mass. Silica can be used alone or in combination of two or more.
[0061] (C) Organic peroxide crosslinking agent
[0062] The organic peroxide crosslinking agent is used as a crosslinking agent for forming peroxide crosslinks of the natural rubber component. By using the organic peroxide crosslinking agent as a crosslinking agent, excellent compression set resistance is imparted to the seal body portion. Examples of the organic peroxide crosslinking agent include diisopropylbenzene peroxide, cumene peroxide, p-methane hydroperoxide, 2,5-dimethylhexane-2,5-dihydroperoxide, di-tert-butyl peroxide, benzoyl peroxide, m-tolyl peroxide, 2,5-dimethyl-2,5-bis(tert-butylperoxy)hexane, 2,5-dimethyl-2,5-bis(tert-butylperoxy)-3-hexyloxy, 1,3-di(tert-butylperoxy)hexane, 2,5-dimethyl-2,5-bis-dimethyl-2,5-di(benzoylperoxy)hexane, 1,3,3-tetramethylbutylperoxy-2-ethylhexanoate, tert-butyl peroxybenzoate, tert-butyl peroxylaurate, di(tert-butylperoxy)adipate, di(2-ethoxyethylperoxy)dicarboxylate, and bis(4-tert-butylcyclohexyl)peroxydicarboxylate. Among these, dicumyl peroxide is preferably used.
[0063] As commercially available products of organic peroxide crosslinking agents, for example, "PERCUMYL (registered trademark) D" manufactured by NOF Corporation can be used. The content of the organic peroxide crosslinking agent is preferably 0.1 parts by mass or more and 10 parts by mass or less, and more preferably 1 part by mass or more and 5 parts by mass or less, relative to 100 parts by mass of the natural rubber component. The organic peroxide crosslinking agent can be used alone or in combination of two or more.
[0064] (D) Silane coupling
[0065] When the rubber composition contains silica as a filler, a silane coupling agent is further added to the rubber composition. As the silane coupling agent, a silane coupling agent having a mercapto group is preferred, for example, 3-mercaptopropyltrimethoxysilane, 3-mercaptopropyltriethoxysilane, 3-mercaptopropyldiethoxysilane, 3-mercaptopropyltripropoxysilane, 3-mercaptopropyldipropoxysilane, 3-mercaptopropyldipropoxymethoxysilane, 3-mercaptopropyltributoxysilane, 3-mercaptopropyldibutoxymethoxysilane, 3-mercaptopropylmethyldimethoxysilane, 3-mercaptopropyldimethoxymethoxysilane, 3-mercaptopropyltri ... Mercaptopropyldiethoxysilane, 3-mercaptopropyldiethoxymethoxysilane, 3-mercaptopropylmethyldipropoxysilane, 3-mercaptopropylpropoxydimethylsilane, 3-mercaptopropylmethyldiisopropoxysilane, 3-mercaptopropylisopropoxydimethylsilane, 3-mercaptopropylmethyldibutoxysilane, 3-mercaptopropyldimethylbutoxysilane, 2-mercaptoethyltrimethoxysilane, 2-mercaptoethyltriethoxysilane, mercaptomethyltrimethoxysilane, mercaptomethyltriethoxysilane, etc.
[0066] As a commercially available product of the silane coupling agent, for example, "KBM-803" manufactured by Shin-Etsu Silicone Co., Ltd. can be used. The content of the silane coupling agent is preferably 0.1 parts by mass or more and 10 parts by mass or less, and more preferably 1 part by mass or more and 5 parts by mass or less, relative to 100 parts by mass of the natural rubber component. The silane coupling agent may be used alone or in combination of two or more.
[0067] (E) Other additives
[0068] The rubber composition may also include other ingredients in addition to the above-mentioned ingredients as required. As other ingredients, various additives such as crosslinking accelerators, plasticizers, anti-aging agents, auxiliary agents, lubricants, adhesives, lubricants, flame retardants, mildew inhibitors, and antistatic agents may be cited. These additives may be used alone or in combination of two or more. In addition, their amounts are not particularly limited as long as they do not hinder the purpose and effect of the present invention, and may be appropriately added according to the purpose of the combination.
[0069] <Method for manufacturing seal body>
[0070] The method for manufacturing the sealing body is not particularly limited. For example, the natural rubber component, filler, and organic peroxide crosslinking agent described above, as well as a silane coupling agent and any various additives as required, are appropriately mixed in a predetermined ratio, and then kneaded using a mixer such as a single-screw extruder, a twin-screw extruder, a roll, a Banbury mixer, a kneader, or a high-shear mixer to manufacture the rubber composition. It should be noted that before kneading, mastication, preliminary kneading, etc. may be performed as required.
[0071] Furthermore, the rubber composition obtained by vulcanization molding can manufacture a vulcanized molded product having the shape of a sealing main body. The vulcanization molding of the rubber composition is carried out by using an injection molding machine, a compression molding machine, etc., and is generally carried out by pressurization vulcanization at about 150 to 230° C. for about 0.5 to 30 minutes. In addition, after the primary vulcanization (pressurization vulcanization) such as the embodiment, in order to reliably implement the vulcanization to the inside of the vulcanized molded product, a secondary vulcanization can also be carried out as needed. The secondary vulcanization can be carried out by oven heating, steam heating, hot air heating, etc., generally at about 150 to 250° C. for about 0.5 to 24 hours.
[0072] (Mechanical Strength)
[0073] In the sealing body of the sealing device of the present embodiment, the tensile strength (test piece shape: dumbbell-shaped No. 6, speed: 500 mm / min, distance between markings: 20±0.5 mm, atmosphere: air, test temperature: tensile strength measured at room temperature) measured in accordance with the provisions of JIS K6251:2017 (Japanese Industrial Standards made by changing the technical content based on ISO37 (2011 5th edition)) is 10 MPa or more, preferably 15 MPa or more. In addition, in the sealing body, the elongation at cutting measured in accordance with the provisions of JIS K 6251:2017 (test piece shape: dumbbell-shaped No. 6, speed: 500 mm / min, distance between markings: 20±0.5 mm, atmosphere: air, test temperature: elongation at cutting measured at room temperature) is 200% or more, preferably 300% or more. Since the seal body portion has a tensile strength of 10 MPa or more and an elongation at break of 200% or more, it is possible to provide a sealing device including the seal body portion that exhibits high mechanical strength even under high pressure.
[0074] (cold resistance)
[0075] In the sealing body of the sealing device of the present embodiment, the temperature of TR10 in the low temperature elastic recovery test (TR test) measured in accordance with the provisions of JIS K6261-4:2017 (Japanese Industrial Standards prepared by changing the technical content based on ISO2921 (2011 5th edition)) (test piece shape: I-shaped as described in the provisions of JIS K6261-4:2017, heat medium: ethanol, test temperature: the temperature of TR10 in the low temperature elastic recovery test (TR test) measured under the conditions of -70°C to 23°C) is -40°C or less, preferably -60°C or less. Since the temperature in TR10 is -40°C or less, it is possible to provide a sealing device including a sealing body having excellent cold resistance in a low temperature region.
[0076] (Compression set resistance)
[0077] In the sealing body portion of the sealing device of the present embodiment, the shape of the G25 O-ring described in JIS B 2401-1:2012 (a Japanese industrial standard prepared by changing the technical content based on ISO3601-1 (2008 4th edition)), the compression set after 70 hours at 100° C. measured in accordance with JIS K 6262:2013 (a Japanese industrial standard prepared by changing the technical content based on ISO815-1 and ISO815-2 (both 2008 1st editions)) (compression plate: smooth stainless steel plate, test piece shape: G25 O-ring described in JIS B 2401-1:2012, spacer thickness: 2.30 mm, compression rate: 25%, atmosphere: air, test temperature: 100° C., exposure time: 70 hours, storage conditions after opening: compression set measured under the conditions of 30 minutes at room temperature) is 40% or less, preferably 35% or less. Since the compression set under such conditions is 40% or less, it is possible to provide a sealing device including a sealing body portion having excellent compression set resistance in a high temperature region.
[0078] Based on the above embodiments, the present invention relates to the following [1] to [7].
[0079] A sealing device is arranged between two components facing each other and seals the space between the two components. The sealing device is characterized in that:
[0080] comprising a sealing body portion in contact with the space,
[0081] In the sealing body, the tensile strength measured in accordance with the provisions of JIS K 6251:2017 is 10 MPa or more, the elongation at break measured in accordance with the provisions of JIS K 6251:2017 is 200% or more, the temperature of TR10 in the low-temperature elastic recovery test measured in accordance with the provisions of JIS K 6261-4:2017 is -40°C or less, and the shape of the G25 O-ring described in the provisions of JIS B 2401-1:2012 is measured in accordance with the provisions of JIS K 6262:2013. The compression set after 70 hours at 100°C is 40% or less in the electrolysis device.
[0082] The sealing device according to the above-mentioned [1], wherein the sealing body portion is annular.
[0083] The sealing device according to the above-mentioned [1] or [2], wherein the sealing body portion is held by a support ring.
[0084] The sealing device according to the above-mentioned [1], wherein the cross-sectional shape of the sealing body portion is a protrusion shape.
[0085] The sealing device according to the above [4], wherein the sealing body portion is provided on a plate-shaped substrate, and the substrate is a plate made of metal or carbon.
[0086] The sealing device according to the above [5], wherein the base material and the sealing body are bonded to each other by an adhesive contained in the sealing body.
[0087] The sealing device according to any one of [1] to [6] above, wherein the sealing body is in contact with hydrogen gas.
[0088] The sealing device according to any one of [1] to [6] above, wherein the sealing body is in contact with liquid hydrogen.
[0089] The sealing device according to any one of [1] to [8] above, wherein the sealing device is used in a hydrogen energy system.
[0090] A sealing device is arranged between two components facing each other and seals the space between the two components. The sealing device is characterized in that:
[0091] comprising a sealing body portion in contact with the space,
[0092] The sealing body is a vulcanized product of a rubber composition, wherein the rubber composition comprises: (A) a natural rubber component selected from natural rubber and epoxy-modified natural rubber having an epoxidation degree of 1% or more and less than 50%; (B) a filler selected from carbon black and silica; (C) an organic peroxide-based crosslinking agent; and optionally (D) a silane coupling agent (wherein, when the filler is carbon black, the rubber composition contains epoxy-modified natural rubber having an epoxidation degree of 1% or more and less than 50%, and when the filler is silica, the rubber composition also contains a silane coupling agent).
[0093] The sealing device according to the above
[10] , wherein the rubber composition further contains (E) at least one additive selected from the group consisting of a cross-linking accelerator, an auxiliary agent, and an antioxidant.
[0094] Although the embodiments of the present invention have been described above, the present invention is not limited to the above embodiments, but includes all aspects included in the concept of the present invention and the claims, and various modifications can be made within the scope of the present invention.
[0095] Example
[0096] Next, examples of the present invention will be described, but the present invention is not limited to these examples.
[0097] (Example 1)
[0098] 100 parts by mass of natural rubber having an epoxidation degree of 25% ("ENR25", imported from Sanyo Trading) was placed in a kneading extruder ("Labo The rubber was mixed with a mixture of 1% tantalum ("Plastomill 30C150", manufactured by Toyo Seiki Co., Ltd.), and masticated at 50°C for 15 minutes. Then, 50 parts by mass of filler A (carbon black: trade name "Vulcan (registered trademark) 3L", manufactured by Cabot Japan Co., Ltd.), 2.5 parts by mass of crosslinking agent A (dicumyl peroxide: trade name "PERCUMYL (registered trademark) D", manufactured by NOF Corporation), 5 parts by mass of auxiliary agent A (zinc white: trade name "zinc oxide", manufactured by Shodo Chemical Industry Co., Ltd.), 1 part by mass of auxiliary agent B (stearic acid: trade name "DTST", manufactured by Miyoshi Oil & Fats Co., Ltd.), and 2 parts by mass of antioxidant (2,2,4-trimethyl-1,2-dihydroquinoline polymer: trade name "NOCRAC224", manufactured by Ouchi Shinko Chemical Industry Co., Ltd.) were added, and kneaded at 50°C for 15 minutes to prepare a rubber stock. Next, the obtained rubber stock was put into a roll kneading mill ("LABORTORY MILL", manufactured by Kansai Roll Co., Ltd.), and the rubber stock was passed five times at a roll gap of 1.5 to 2.5 mm, and then passed ten times at a roll gap of 1 mm to prepare a rubber composition.
[0099] <Preparation of test pieces for measuring mechanical strength and cold resistance>
[0100] The obtained rubber composition was cross-linked under hot pressing at 170° C. using a press (“80TON Press”, manufactured by Kitan Machinery Industry Co., Ltd.), and cross-linked for a time 1.5 times that of t90 (90% cross-linking time), thereby press vulcanization (primary vulcanization) was performed to prepare a test piece A.
[0101] <Preparation of test pieces for compression set measurement>
[0102] The obtained rubber composition was cross-linked under hot pressing at 170° C. using a press (“50 ton KV press”, manufactured by Kodai Shoji Co., Ltd.), and press vulcanization (primary vulcanization) was performed by cross-linking for a time 1.5 times t90 (90% cross-linking time) to prepare a test piece B.
[0103] <Tensile strength and elongation at break>
[0104] The tensile strength and elongation at break of the test piece A were measured under the following test conditions using a tensile tester ("Strograph (registered trademark) AE", manufactured by Toyo Seiki Co., Ltd.) in accordance with JIS K 6251:2017. The results are shown in Table 1.
[0105] [Test conditions]
[0106] ·Test piece shape: dumbbell shape No. 6
[0107] (The test piece is Figure 5 In the dumbbell shape shown, S represents the marking line, D represents the initial marking line spacing, and T represents the parallel portion. In the dumbbell shape No. 6, D = 20 ± 0.5 mm, and T thickness = 2.0 ± 0.2 mm. )
[0108] Speed: 500mm / min
[0109] Atmosphere: Air
[0110] Test temperature: room temperature
[0111] <Cold resistance>
[0112] For the test piece A, a low temperature elastic recovery test (TR test) was performed under the following test conditions in accordance with JIS K6261-4:2017 using a TR tester ("No. 145-L", manufactured by Yasuda Seiki Co., Ltd.), and the temperature at TR10 was measured. The results are shown in Table 1.
[0113] [Test conditions]
[0114] ·Test piece shape: I-shaped as specified in JIS K6261-4:2017
[0115] Heat medium: ethanol
[0116] Test temperature: -70℃~23℃
[0117] <Compression set resistance>
[0118] The compression set of the test piece B was measured under the following test conditions in accordance with JIS K 6262: 2013. The results are shown in Table 1.
[0119] [Test conditions]
[0120] Compression plate: smooth stainless steel plate
[0121] ·Test piece shape: G25 O-ring as specified in JIS B 2401-1:2012
[0122] ( Figure 6 This is a schematic diagram showing the cross section of the O-ring used for the test piece. d1 represents the inner diameter and d2 represents the thickness. In the G25 O-ring, d1 = 24.4 ± 0.25 mm and d2 = 3.1 ± 0.10 mm.
[0123] Spacer thickness: 2.30mm
[0124] Compression rate: 25%
[0125] Atmosphere: Air
[0126] Test temperature: 100℃
[0127] Exposure time: 70 hours
[0128] Storage conditions after opening: 30 minutes at room temperature
[0129] (Example 2)
[0130] The rubber composition and the test pieces A and B were prepared in the same manner as in Example 1, except that natural rubber ("RSS No. 1", imported from Toyota Tsutsu Chemiplas) was used instead of natural rubber having an epoxidation degree of 25%, filler B (silicon dioxide: trade name "Ultrasil (registered trademark) 360", manufactured by Evonik Japan) was used instead of filler A, and 1 part by mass of a silane coupling agent (mercapto-containing silane coupling agent: trade name "KBM-803", manufactured by Shin-Etsu Silicone Co., Ltd.) was further configured. The above-mentioned measurements were performed. The results are shown in Table 1.
[0131] (Comparative Example 1)
[0132] A rubber composition and each test piece A and B were prepared in the same manner as in Example 1, except that a natural rubber ("RSS No. 1", a product imported from Toyota Tsutsu Chemiplas) was used instead of a natural rubber having an epoxidation degree of 25%, 0.5 parts by mass of a crosslinking agent B (sulfur: trade name "colloidal sulfur A", manufactured by Tsurumi Chemical Industry Co., Ltd.) was used instead of a crosslinking agent A, 1.5 parts by mass of a crosslinking accelerator A (N-cyclohexyl-2-benzothiazole sulfonamide: trade name "NOCCELER (registered trademark) CZ-G", manufactured by Ouchi Shinko Chemical Co., Ltd.) and 1 part by mass of a crosslinking accelerator B (tetramethylthiuram disulfide: trade name "NOCCELER (registered trademark) TT-P", manufactured by Ouchi Shinko Chemical Co., Ltd.) were further added, and when preparing each test piece A and B, the crosslinking temperature was changed from 170° C. to 150° C., and the above-mentioned measurement was performed. The results are shown in Table 1.
[0133] (Comparative Example 2)
[0134] A rubber composition and test pieces A and B were prepared in the same manner as in Example 1, except that natural rubber ("RSS No. 1", a product imported from Toyota Tsutsu Chemiplas) was used instead of natural rubber having an epoxidation degree of 25%, and the above-mentioned measurements were performed. The results are shown in Table 1.
[0135] (Comparative Example 3)
[0136] A rubber composition and test pieces A and B were prepared in the same manner as in Example 1, except that natural rubber having an epoxidation degree of 50% ("ENR50", imported from Sanyo Trading) was used instead of natural rubber having an epoxidation degree of 25%, and the above-mentioned measurements were performed. The results are shown in Table 1.
[0137] (Comparative Example 4)
[0138] A rubber composition and test pieces A and B were prepared in the same manner as in Example 2 except that the silane coupling agent was not blended, and the above-mentioned measurements were performed. The results are shown in Table 1.
[0139]
Table 1
[0140]
[0141] The components shown in Table 1 are as follows. In addition, the values of the components in Table 1 represent "parts by mass".
[0142] ·Natural rubber: Trade name "RSS No. 1", imported from Toyota Chemiplas
[0143] · Natural rubber with 25% epoxidation degree ("ENR25", imported from Sanyo Trading)
[0144] · Natural rubber with 50% epoxidation degree ("ENR50", imported from Sanyo Trading)
[0145] Filler A: Carbon black (trade name "Vulcan (registered trademark) 3L", manufactured by Cabot Japan Co., Ltd.)
[0146] Filler B: silicon dioxide (trade name "Ultrasil (registered trademark) 360", manufactured by Evonik Japan Co., Ltd.)
[0147] Cross-linking agent A: dicumyl peroxide (trade name "PERCUMYL (registered trademark) D", manufactured by NOF Corporation)
[0148] Cross-linking agent B: Sulfur (trade name "colloidal sulfur A", manufactured by Tsurumi Chemical Industries, Ltd.)
[0149] Silane coupling agent: mercapto group-containing silane coupling agent (trade name "KBM-803", manufactured by Shin-Etsu Silicone Co., Ltd.)
[0150] · Additive A: Zinc white (trade name "zinc oxide", manufactured by Shodo Chemical Industry Co., Ltd.)
[0151] · Additive B: stearic acid (trade name "DTST", manufactured by Miyoshi Oil & Fats Co., Ltd.)
[0152] Antiaging agent: 2,2,4-trimethyl-1,2-dihydroquinoline polymer (trade name "NOCRAC224", manufactured by Ouchi Shinko Chemical Industry Co., Ltd.)
[0153] As can be seen from Table 1, in Examples 1 and 2, the tensile strength is 10 MPa or more and the elongation at break is 200% or more, showing high mechanical strength even under high pressure. In addition, in Examples 1 and 2, the temperature of TR10 in the low-temperature elastic recovery test is -40°C or less, and the compression set after 70 hours at 100°C is 40% or less, so the cold resistance in the low temperature region and the compression set resistance in the high temperature region are excellent.
[0154] On the other hand, in Comparative Example 1 using a sulfur crosslinking agent as a crosslinking agent, the compression set is higher than 40% and the compression set resistance is poor. In addition, in Comparative Example 2 using carbon black as a filler and unmodified natural rubber as a natural rubber component, the compression set is higher than 40% and the compression set resistance is poor. On the other hand, in Comparative Example 3 using carbon black as a filler and using a natural rubber with an epoxidation degree of 50% as a natural rubber component, the compression set is less than 40%, but the temperature of TR10 in the low-temperature elastic recovery test is higher than -40°C and the cold resistance is poor. Furthermore, in Comparative Example 4 using silica as a filler but not using a silane coupling agent, the compression set is higher than 40% and the compression set resistance is poor.
[0155] Description of Reference Numerals
[0156] 1, 1A, 1B sealing device, 2 a member (piping member), 3 another member (piping member), 4 mounting groove, 4a high-pressure side mounting position, 4b low-pressure side mounting position, 4c inclined bottom surface, 11 sealing ring, 21 first support ring (support ring), 21a, 31a inclined surface, 31 second support ring, 100 sealing device, 101 substrate, 101a vent hole, 102 sealing pad, 102a base, 102b sealing lip
Claims
1. A sealing device, arranged between two components facing each other, and sealing the space between the two components, wherein the sealing device is characterized in that: comprising a sealing body portion in contact with the space, In the sealing body, the tensile strength measured in accordance with the provisions of JIS K 6251:2017 is 10 MPa or more, the elongation at break measured in accordance with the provisions of JIS K 6251:2017 is 200% or more, the temperature of TR10 in the low-temperature elastic recovery test measured in accordance with the provisions of JIS K 6261-4:2017 is -40°C or less, and the shape of the G25 O-ring described in the provisions of JIS B 2401-1:2012, the compression set after 70 hours at 100°C measured in accordance with the provisions of JIS K 6262:2013 is 40% or less.
2. The sealing device according to claim 1, wherein: The sealing body is annular.
3. The sealing device according to claim 1 or 2, wherein: The sealing body portion is held by a support ring.
4. The sealing device according to claim 1, wherein: The cross-sectional shape of the sealing body is a protrusion shape.
5. The sealing device according to claim 4, wherein: The sealing body is provided on a plate-shaped substrate, and the substrate is a plate made of metal or carbon.
6. The sealing device according to claim 5, wherein: The base material and the sealing body portion are bonded to each other by an adhesive contained in the sealing body portion.
7. The sealing device according to claim 1 or 2, wherein: The sealing body portion is in contact with hydrogen gas.
8. The sealing device according to any one of claims 1 or 2, wherein: The sealing body portion is in contact with liquid hydrogen.
9. The sealing device according to claim 1 or 2, wherein: The sealing device is used in a hydrogen energy system.
10. A sealing device, arranged between two components facing each other, and sealing the space between the two components, wherein the sealing device is characterized in that: comprising a sealing body portion in contact with the space, The sealing body is a vulcanized product of a rubber composition, wherein the rubber composition comprises: (A) a natural rubber component selected from natural rubber and epoxy-modified natural rubber having an epoxidation degree of 1% or more and less than 50%; (B) a filler selected from carbon black and silica; (C) an organic peroxide crosslinking agent; and (D) a silane coupling agent, wherein: When the filler is carbon black, the rubber composition contains epoxy-modified natural rubber having an epoxidation degree of 1% or more and less than 50%, and when the filler is silica, the rubber composition further contains a silane coupling agent.
11. The sealing device according to claim 10, wherein: The rubber composition further contains (E) at least one additive selected from the group consisting of a cross-linking accelerator, an auxiliary agent and an antioxidant.