Method for evaluating liquid material and device for evaluating liquid material
By adding non-reactive fluorescent labeling compounds to the liquid, using fluorescence spectral observation and spectral analysis, the changes in water content and impurities in the liquid are detected in real time, and the performance deterioration and detection caused by reactive fluorescent labeling agents in the prior art are solved. Difficulty issues achieve efficient quality monitoring.
Patent Information
- Application Number
- CN202380031446.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-29
- Filing Date
- 2023-03-08
- Publication Date
- 2024-11-15
AI Technical Summary
In the prior art, when detecting changes in water content and impurities in liquids, reactive fluorescent labeling agents are required, resulting in deterioration of performance and difficulty in real-time monitoring, affecting the quality of the optical film.
The non-reactive fluorescent labeled compound was added to the liquid, and the peak intensity shift was measured through fluorescence spectral observation and spectral analysis, and the water content and impurity changes were detected in real time, avoiding the use of reactive fluorescent labeling agents.
High-precision real-time detection of changes in water content and impurities in the liquid substance is achieved, which reduces feedback time, improves manufacturing efficiency, and avoids performance degradation problems.
Smart Images

Figure CN118974544A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a method and device for evaluating a liquid substance, and more particularly to a method for evaluating a liquid substance capable of detecting minute changes in the amount of water, impurities, etc. in the liquid substance at any time without using a reactive fluorescent labeling agent. Background Art
[0002] In recent years, as the uses of optical films such as polarizer protective films and phase difference films for liquid crystal display devices and organic electroluminescent display devices belonging to display devices, substrate films for touch panels and gas barrier substrate films, as well as substrate films for nanoimprinting and substrate films for flexible electronic circuits, etc., a stable supply of high-quality optical films with high transparency and high functionality has been required.
[0003] Here, when producing a resin molded product, there is known a process of dissolving a resin in a solvent and adding a functional additive to obtain a desired product in order to improve processability.
[0004] The intermediate products in the process are composed of resins, additives, and solvents, but their quality may be affected by batch variations due to different suppliers. In addition, in the factory, very small impurities may be mixed in during storage or piping, which may affect product quality.
[0005] As an evaluation system for monitoring changes such as the above-mentioned quality variations, Patent Documents 1 and 2 disclose methods of quantifying trace impurities in a sample by adding a fluorescent substance as a medium and causing the fluorescent substance to react.
[0006] Patent Document 3 discloses a water content detection method using a fluorescent substance that generates hydrogen peroxide by directly reacting with water and thereby emits fluorescence indirectly.
[0007] However, in the technologies disclosed in Patent Documents 1 to 3, reactive fluorescent labeling agents are used to detect changes in the object in order to detect fluorescent information of impurities. That is, the added fluorescent labeling compound itself becomes an impurity after the reaction, which reduces the performance of resin molded products such as films and is not conducive to the quality of current optical films.
[0008] Prior art literature
[0009] Patent Literature
[0010] Patent Document 1: Japanese Patent Application Publication No. 2001-56327
[0011] Patent Document 2: Japanese Patent Application Publication No. 2011-95111
[0012] Patent Document 3: International Publication No. 2029 / 039963 Summary of the invention
[0013] The present invention has been made in view of the above problems and circumstances, and aims to provide a method and apparatus for evaluating a liquid material that can detect minute changes in the amount of water, impurities, etc. in the liquid material at any time without using a reactive fluorescent labeling agent.
[0014] In order to solve the above-mentioned problems, the inventors have studied the causes of the above-mentioned problems and found that by adding a fluorescent labeling compound as a non-reactive additive to a liquid and measuring the change in the peak intensity of the fluorescence spectrum of the liquid, it is possible to detect slight changes in the amount of water, impurities, etc. in the liquid at any time without using a reactive fluorescent labeling agent, thereby completing the present invention.
[0015] That is, the above-mentioned problems according to the present invention are solved by the following means.
[0016] 1. A method for evaluating a liquid substance, comprising at least a solvent, a resin and a non-reactive additive.
[0017] The non-reactive additive is a fluorescent labeling compound.
[0018] The above-mentioned liquid evaluation method comprises:
[0019] a fluorescence spectrum observation step of obtaining a fluorescence spectrum of the liquid substance at an arbitrary excitation wavelength, and
[0020] A spectrum analysis step of acquiring data related to a peak intensity shift degree based on an interaction between the fluorescent labeling compound in the liquid substance and the inspection object from the acquired fluorescence spectrum.
[0021] 2. The method for evaluating a liquid substance according to item 1, wherein a difference ΔSP in solubility parameters between the fluorescent labeled compound in the liquid substance and the object of inspection is within a range of 6 to 22.
[0022] 3. The method for evaluating a liquid material according to item 1 or 2, wherein the non-reactive additive is contained in an amount within a range of 1 to 5000 ppm by mass based on the liquid material.
[0023] 4. The method for evaluating a liquid material according to any one of items 1 to 3, wherein the spectral analysis step is performed online.
[0024] 5. The method for evaluating a liquid substance according to any one of items 1 to 4, further comprising a data processing step of calculating the content of the inspection object using a calibration curve based on the peak intensity included in the data related to the peak intensity shift degree.
[0025] 6. A liquid material evaluation device, comprising at least a solvent, a resin and a non-reactive additive,
[0026] The non-reactive additive is a fluorescent labeling compound.
[0027] The liquid material evaluation device comprises:
[0028] a fluorescence spectrum observation unit for obtaining the fluorescence spectrum of the liquid substance at an arbitrary excitation wavelength, and
[0029] A spectrum analysis unit acquires data related to a peak intensity shift degree based on an interaction between the fluorescent labeling compound in the liquid substance and the inspection object from the acquired fluorescence spectrum.
[0030] 7. The liquid material evaluation device according to item 6, further comprising a data processing unit for calculating the content of the inspection object using a calibration curve based on the peak intensity included in the data related to the peak intensity deviation.
[0031] 8. The liquid material evaluation device according to item 6 or 7, further comprising an information display unit for displaying data related to the peak intensity shift degree.
[0032] The above-mentioned means of the present invention can provide a method and apparatus for evaluating a liquid material that can detect minute changes in the amount of water, impurities, etc. in the liquid material at any time without using a reactive fluorescent labeling agent.
[0033] The mechanism of expression or action of the effect of the present invention is not clear, but can be inferred as follows.
[0034] For example, regarding the variation in film quality (haze), it is considered that the cause thereof is the following variation.
[0035] (i) The impurities and stabilizers in the purchased raw materials are different during production;
[0036] (ii) seasonal changes during storage, differences in the moisture content of resins and additives or the pH of solvents during film production;
[0037] (iii) Outflow of metal ions due to differences in piping equipment between factories or differences in the degree of deterioration of piping due to changes over time after the factory is built.
[0038] Therefore, in order to detect the above-mentioned changes without adding a reactive fluorescent labeling agent that may deteriorate performance, a non-reactive additive (non-reactive fluorescent labeling compound) is added to a liquid containing a raw material and a solute, and the fluorescence spectrum is measured.
[0039] Furthermore, when the liquids of (i) to (iii) above were prepared and the fluorescence spectrum of each liquid was measured and compared with the fluorescence spectrum of a reference sample, it was found that the peak intensity of the non-reactive fluorescent labeling compound was shifted.
[0040] Here, the reasons why a high-precision evaluation method is achieved without causing a chemical reaction between the resin, the non-reactive fluorescent labeling compound, and the inspection object are as follows.
[0041] Compared to the case where only two components, the non-reactive fluorescent labeling compound and the inspection object, exist in the liquid, if the resin enters the liquid, the density becomes higher than that of the above two components, and it is easier to significantly interact with each other. In addition, it is inferred that the interaction between the resin and the inspection object can indirectly detect the non-reactive fluorescent labeling compound even if the signal is small.
[0042] In addition, the amount of information obtained from signals of multiple wavelengths of non-reactive fluorescent labeling compounds, inspection objects, and resins increases compared to a single wavelength, making it easier to capture changes in fluorescence intensity.
[0043] As described above, by adding a fluorescent labeling compound as a non-reactive additive to a liquid substance and measuring the change in the peak intensity of the fluorescence spectrum of the liquid substance, it is possible to detect minute changes in the amount of water, impurities, etc. in the liquid substance at any time without using a reactive fluorescent labeling agent. As a result, the above-mentioned minute changes can be detected in real time, thereby significantly reducing the time required to obtain feedback in the manufacturing process and improving manufacturing efficiency. BRIEF DESCRIPTION OF THE DRAWINGS
[0044] Figure 1 It is a diagram schematically showing a configuration example of a liquid material evaluation device according to the present invention.
[0045] Figure 2 This is a flowchart showing a computer control procedure executed in the liquid material evaluation device of the present invention.
[0046] Figure 3 This is a diagram schematically showing an example of a dope preparation step, a casting step, a drying step, and a winding step in a solution casting film forming method.
[0047] Figure 4 It is a schematic diagram which shows an example of the hard-coat layer forming apparatus. DETAILED DESCRIPTION
[0048] The evaluation method of a liquid substance of the present invention is a method for evaluating a liquid substance containing at least a solvent, a resin and a non-reactive additive, wherein the non-reactive additive is a fluorescent labeling compound, and comprises: a fluorescence spectrum observation step of obtaining a fluorescence spectrum of the liquid substance at an arbitrary excitation wavelength, and a spectrum analysis step of obtaining data related to a peak intensity deviation degree based on the interaction between the fluorescent labeling compound in the liquid substance and an inspection object from the obtained fluorescence spectrum.
[0049] This feature is a common or corresponding technical feature of the following embodiments.
[0050] As an embodiment of the present invention, from the viewpoint of facilitating the interaction between the fluorescent labeled compound and the inspection object and facilitating the peak intensity shift, it is preferred that the difference ΔSP between the solubility parameters of the fluorescent labeled compound and the inspection object in the liquid is within a range of 6 to 22. In addition, it is also preferred from the viewpoint of facilitating the transparency of a product using the liquid.
[0051] Furthermore, from the viewpoint of achieving a balance between the haze of an optical film using a liquid substance and the measurement sensitivity of a fluorescence spectrum, the non-reactive additive is preferably contained in an amount within a range of 1 to 5000 ppm by mass based on the liquid substance.
[0052] Furthermore, it is preferred to perform the spectral analysis step online from the viewpoint that the amount of water or impurities mixed in the liquid can be detected in real time, the time required to obtain feedback in the production process can be significantly reduced, and production efficiency can be improved.
[0053] In addition, from the viewpoint of being able to detect changes in the content of the inspection object and improving manufacturing efficiency, it is preferable to have a data processing step of calculating the content of the inspection object using a calibration curve based on the peak intensity included in the data related to the peak intensity deviation.
[0054] The evaluation device of the present invention is an evaluation device for a liquid containing at least a solvent, a resin and a non-reactive additive, wherein the non-reactive additive is a fluorescent labeling compound, and comprises: a fluorescence spectrum observation unit for acquiring a fluorescence spectrum of the liquid at an arbitrary excitation wavelength, and a spectrum analysis unit for acquiring data related to a peak intensity shift degree based on the interaction between the fluorescent labeling compound in the liquid and an inspection object from the acquired fluorescence spectrum. Thus, it is possible to detect minute changes in the amount of water, impurities, etc. in the liquid at any time without using a reactive fluorescent labeling agent.
[0055] Furthermore, the evaluation apparatus of the present invention preferably comprises a data processing unit for calculating the content of the inspection object using a calibration curve based on the peak intensity included in the data related to the peak intensity shift, or an information display unit for displaying the data related to the peak intensity shift.
[0056] Hereinafter, the present invention and its constituent elements and forms and modes for carrying out the present invention will be described. It should be noted that in the present application, "to" is used to mean that the numerical values described before and after it are included as the lower limit and the upper limit.
[0057] [Overview of the evaluation method of the liquid material of the present invention]
[0058] The evaluation method of a liquid substance of the present invention is a method for evaluating a liquid substance containing at least a solvent, a resin and a non-reactive additive, wherein the non-reactive additive is a fluorescent labeling compound, and comprises: a fluorescence spectrum observation step of obtaining a fluorescence spectrum of the liquid substance at an arbitrary excitation wavelength, and a spectrum analysis step of obtaining data related to a peak intensity deviation degree based on the interaction between the fluorescent labeling compound in the liquid substance and an inspection object from the obtained fluorescence spectrum.
[0059] In addition, from the perspective of being able to detect changes in the content of the inspection object and improving manufacturing efficiency, the liquid material evaluation method of the present invention preferably has a data processing step for calculating the content of the above-mentioned inspection object using a calibration curve based on the peak intensity included in the data related to the above-mentioned peak intensity deviation.
[0060] In the present invention, the “liquid substance” may contain at least a solvent, a resin, and a non-reactive additive, and the residual solvent content may be 1000 ppm by mass or more.
[0061] Specific examples of such liquid substances include, for example, coatings for producing optical films, adhesives for bonding optical films to polarizers, coating solutions for forming hard coat layers for protective films, coating solutions for forming antistatic layers, aqueous coating solutions that can be used for forming near-infrared reflective films (e.g., coating solutions for forming high refractive index layers, coating solutions for forming low refractive index layers), or residual solvents after applying these coating solutions, coating materials for coating products used in ink applications, electrolytes in batteries, coating solutions for protecting positive electrode active materials, coating solutions for coating automotive parts, motor oils, photosensitive materials before ultraviolet curing in the semiconductor field, solutions containing polymers such as gelatin in the food field, and the like.
[0062] The coating material, the coating liquid for forming a hard coat layer, the coating liquid for forming an antistatic layer, and the coating liquids for forming a high refractive index layer and a low refractive index layer are described in detail below.
[0063] In the present invention, the "non-reactive additive" involved in the present invention refers to a compound that does not form a covalent bond or an ionic bond with the inspection object (does not undergo a structural change). However, the non-reactive additive involved in the present invention is a compound that can interact with the inspection object by hydrogen bonding or van der Waals force, etc., so as to change the peak intensity shift degree.
[0064] Specifically, when the non-reactive additive is a compound that does not have single-wavelength absorption in the visible light region, it does not color the liquid and is therefore preferably used in the optical field.
[0065] As the non-reactive additive, for example, a non-reactive fluorescent labeling compound can be cited. In addition, as the non-reactive fluorescent labeling compound, as long as it can emit fluorescence, antioxidants, pigments, phase difference adjusting agents, wavelength adjusting agents, size adjusting agents, and compounds having functions derived from additives can be used.
[0066] As the antioxidant (AO agent), a commonly known antioxidant can be used, and it is particularly preferred to use each of lactone-based, sulfur-based, phenol-based, double-bond-based, hindered amine-based, and phosphorus-based compounds. As the phenol-based compound, it is preferred to have a structure of 2,6-dialkylphenol, and examples thereof include "Irganox 1076" and "Irganox 1010" commercially available from BASF Japan Co., Ltd., and "ADEKA STAB AO-50" commercially available from ADEKA Co., Ltd.
[0067] Examples of the dye include compounds having an absorption wavelength in the near infrared region and compounds having an absorption wavelength in the near ultraviolet region.
[0068] As a compound having an absorption wavelength in the above-mentioned near-infrared region (also referred to as a "near-infrared absorbing composition"), from the viewpoint of spectral characteristics, it is preferred to add at least one near-infrared absorbing modifier having a maximum absorption wavelength in the wavelength region of 650 to 800 nm as an additive for adjusting the absorption waveform. As a near-infrared absorbing modifier suitable for the present invention, a near-infrared absorbing pigment having a maximum absorption wavelength in the wavelength region of 650 to 800 nm is preferably used.
[0069] Examples of near infrared absorbing pigments (NIR pigments) suitable for the present invention include cyanine pigments, squarylium pigments, Pigment, ketoacid Pigments, azo pigments, anthraquinone pigments, naphthoquinone pigments, phthalocyanine pigments, naphthalocyanine pigments, quaternaryl pigments, dithiol metal complex pigments, etc. Among them, cyanine pigments, squarylium pigments, and squarylium pigments are preferred from the viewpoint of detecting changes in fluorescence intensity according to the amount of change in the object of inspection. Pigment, particularly preferably squaric acid pigment.
[0070] As a compound having an absorption wavelength in the above-mentioned near-ultraviolet region (also referred to as a "near-ultraviolet absorbing composition"), from the viewpoint of spectral characteristics, it is preferred to add at least one near-ultraviolet absorbing modifier having a maximum absorption wavelength in the wavelength region of 300 to 400 nm as an additive for adjusting the added absorption waveform. As a near-ultraviolet absorbing modifier suitable for the present invention, a near-ultraviolet absorbing pigment having a maximum absorption wavelength in the wavelength region of 300 to 400 nm is preferably used.
[0071] As the near ultraviolet absorbing pigment (NUV pigment) suitable for the present invention, for example, there can be mentioned merocyanine pigments, benzotriazole ultraviolet absorbers, benzophenone ultraviolet absorbers, salicylate ultraviolet absorbers, cyanoacrylate ultraviolet absorbers, triazine ultraviolet absorbers, oxalic acid anilide ultraviolet absorbers, nickel complex salt ultraviolet absorbers, inorganic ultraviolet absorbers, etc. Among them, merocyanine pigments are particularly preferred from the viewpoint of detecting changes in fluorescence intensity according to the amount of change in the inspection object.
[0072] The "resin" in the present invention can be appropriately changed according to the use of the liquid material, and can be a thermoplastic resin or a thermosetting resin. Specifically, cycloolefin resin (COP resin), triacetyl cellulose resin (TAC resin), acrylic resin, polyurethane resin, polyvinyl alcohol resin, polyimide resin, etc. can be mentioned.
[0073] The "solvent" in the present invention can be appropriately changed according to the application of the liquid material, and examples thereof include organic solvents and water.
[0074] As the organic solvent, for example, chloroform, dichloromethane and other chlorine-based solvents; toluene, xylene, benzene and mixed solvents thereof and other aromatic solvents; methanol, ethanol, isopropanol, n-butanol, 2-butanol and other alcohol solvents; methyl cellosolve, ethyl cellosolve, butyl cellosolve, dimethylformamide, dimethyl sulfoxide, dimethyl ether ... Alkane, cyclohexanone, tetrahydrofuran, acetone, methyl ethyl ketone (MEK), ethyl acetate, diethyl ether, etc. These solvents may be used alone or in combination of two or more.
[0075] In the present invention, the "test object" refers to a compound having an element ion and a charge (ionic compound and polar compound), and by mixing the element ion or compound having a charge into the above-mentioned liquid, an interaction occurs between the non-reactive additive and the test object, which has the effect of changing the peak intensity deviation of the non-reactive additive. In other words, the test object refers to a compound that changes the fluorescence intensity at the excitation wavelength and the fluorescence wavelength at the maximum fluorescence intensity in the obtained fluorescence spectrum by exciting the above-mentioned non-reactive additive at an arbitrary excitation wavelength and measuring a part or all of the fluorescence wavelength of 250 to 950 nm using a fluorescence spectrophotometer.
[0076] Examples of inspection objects suitable for the present invention include water, lithium, sodium, potassium, magnesium, calcium, strontium, or metal ions such as chromium, iron, and copper, halogen element ions such as fluorine, chlorine, and bromine, benzene, acetone, ethanol, methanol, and formamide.
[0077] In the present invention, "peak intensity shift" refers to the amount of change in the fluorescence intensity of the peak that changes when the fluorescence wavelength and fluorescence intensity of the characteristic peak of the non-reactive additive (fluorescent labeling compound) change according to the change in the amount of the test object in the liquid.
[0078] Based on the peak intensity shift, not only the amount of change in the content of the inspection object can be estimated, but also the inspection object can be identified.
[0079] In addition, in the liquid of the present invention, the difference ΔSP in the solubility parameter between the non-reactive additive (fluorescently labeled compound) and the inspection object is preferably in the range of 6 to 22, and more preferably in the range of 14 to 22. By making the difference ΔSP in the solubility parameter within the above range, the interaction between the non-reactive additive and the inspection object is easy to occur, and the peak intensity shift is easy to obtain. In addition, the transparency of the product using the liquid is easy to obtain. It should be noted that if the SP value of the fluorescently labeled compound and the inspection object is close, the compatibility of the fluorescently labeled compound and the inspection object is excellent, so the fluorescently labeled compound and the inspection object will associate without structural changes, and the peak intensity shift corresponding to the mixing amount of the inspection object cannot be correctly obtained. In order to prevent such a situation from occurring, ΔSP is set to 6 or more.
[0080] The solubility parameter is an index for evaluating the physical properties of a substance, especially the dissolution behavior of a solvent, and Hildebrand's SP value (solubility parameter; δ) has been used in the past. The "SP value" is a physical property value inherent to a substance expressed by the square root of the cohesive energy density of the substance.
[0081] The SP value adopts the Hansen solubility parameter (HSP value) proposed by Hansen, which is a parameter that takes the polarity of the substance into consideration and is divided into three components: dispersion term (δD), polar term (δP), and hydrogen bonding term (δH). It is represented by the following formula.
[0082] SP value = (δD 2 +δP 2 +δH 2 ) 0.5
[0083] The Hansen Solubility Parameter (HSP value) is based on the theory that "two substances with similar molecular interactions tend to dissolve each other easily." It consists of the following three parameters, which can be regarded as coordinates in a three-dimensional space (also called "Hansen space."). It is believed that the closer the distance between the coordinates of two substances is, the higher the mutual affinity is, and the easier it is to dissolve.
[0084] δD: Energy based on the dispersion force between molecules
[0085] δP: Energy based on dipole interactions between molecules
[0086] δH: Energy based on hydrogen bonds between molecules
[0087] It should be noted that the method for calculating δD, δP and δH in the Hansen solubility parameters is not particularly limited, and the calculation may be performed by inputting the chemical structure into software or by experimental calculation, but it is preferred to input the chemical structure into software for calculation.
[0088] The HSP value can be a registered value or an estimated value in the commercially available software HSPiP 5th Edition 5.0.10.1. The software can be obtained from a website such as https: / / www.hansen-solubility.com / . In addition, the method for estimating HSP based on such software is based on, for example, the document "Hansen Solubility Parameters: A User's Handbook, Second Edition" by CM Hansen et al. (CRC Press, 2007).
[0089] The SP value of the fluorescent labeling compound contained in the liquid of the present invention is preferably in the range of 5 to 10, the SP value of the above-mentioned resin is preferably in the range of 10 to 20, the SP value of the above-mentioned solvent is preferably in the range of 10 to 20, and the SP value of the above-mentioned inspection object is preferably in the range of 9 to 30.
[0090] Furthermore, the difference ΔSP in solubility parameter between the solvent and the resin is preferably within a range of 6-22.
[0091] <Fluorescence spectrum observation process>
[0092] The fluorescence spectrum observation step is a step of obtaining a fluorescence spectrum of the liquid substance at an arbitrary excitation wavelength.
[0093] The "arbitrary excitation wavelength" is to obtain in advance the fluorescence fingerprint of the liquid substance or the fluorescence spectrum when the excitation wavelength is changed by a few nanometers, and select the excitation wavelength that shows the fluorescence spectrum effective for the measurement from the obtained fluorescence spectrum as the arbitrary excitation wavelength. In particular, it is preferable to select the excitation wavelength with high intensity from the obtained fluorescence spectrum as the arbitrary excitation wavelength, but it is not limited to the excitation wavelength that shows the fluorescence spectrum with high intensity, and the wavelength absorbed by the inspection object can also be used as the excitation wavelength.
[0094] Such an excitation wavelength is, for example, preferably within the range of 200 to 900 nm, and more preferably within the range of 200 to 400 nm and 680 to 900 nm.
[0095] As a means for irradiating a liquid substance with light of an arbitrary excitation wavelength to obtain a fluorescence spectrum, it is preferable to have an irradiation unit for irradiating the liquid substance with light of the excitation wavelength and a light receiving unit for receiving fluorescence emitted from the liquid substance excited by the light of the excitation wavelength.
[0096] The details of the irradiation unit and the light receiving unit will be described using the liquid material evaluation device described later.
[0097] Specifically, in the fluorescence spectrum observation step, the liquid is irradiated with light of an arbitrary excitation wavelength from the irradiation unit, and the fluorescence emitted from the liquid excited by the irradiation is received by the light receiving unit. In the fluorescence spectrum observation step, a plurality of excitation wavelengths may be used to obtain respective fluorescence spectra.
[0098] <Spectral analysis process>
[0099] The spectrum analysis step is a step of obtaining data related to the peak intensity shift degree based on the interaction between the fluorescent labeling compound in the liquid substance and the inspection object from the fluorescence spectrum obtained in the fluorescence spectrum observation step.
[0100] As "data related to the peak intensity deviation", the data of the fluorescence intensity of the changed peak and the amount of change in the fluorescence intensity, the fluorescence wavelength of the changed peak and the amount of change in the fluorescence wavelength can be cited. In addition, the spectrum analysis step can only obtain the above data, or can also include analyzing the obtained data.
[0101] As a means for acquiring the data related to the peak intensity shift degree, for example, a general computer or the like can be cited.
[0102] <Data processing process>
[0103] The data processing step is a step including at least a step of calculating the content of the inspection object based on the peak intensity included in the data related to the peak intensity shift degree obtained in the spectrum analysis step using a calibration curve prepared in advance.
[0104] The calibration curve is prepared by using a liquid substance with a known content of an inspection object and a fluorescent labeling compound, irradiating the liquid substance with light of an arbitrary excitation wavelength, obtaining data of fluorescence intensity and fluorescence wavelength from the fluorescence spectrum emitted from the liquid substance excited by the irradiation in advance, and preparing the calibration curve based on the obtained data. In the calibration curve, for example, the vertical axis represents the fluorescence peak intensity, and the horizontal axis represents the content of the inspection object.
[0105] As a means for calculating the content of the inspection object, for example, a general computer or the like can be cited.
[0106] After the above-mentioned data processing step, the calculated data such as the content of the inspection object, the excitation wavelength of the irradiated light, the fluorescence wavelength and the fluorescence intensity of the liquid substance are preferably displayed on the information display unit.
[0107] [Configuration of Liquid Material Evaluation Device]
[0108] The liquid material evaluation device of the present invention (hereinafter also referred to as "evaluation device") can be used in a manufacturing process using liquid materials in various forms according to the purpose, measure the fluorescence spectrum of the liquid material online at any time, identify the change in the content of the inspection object in the liquid material or the inspection object, and evaluate the liquid material.
[0109] The evaluation device of the present invention is an evaluation device for a liquid substance containing at least a solvent, a resin and a non-reactive additive, wherein the non-reactive additive is a fluorescent labeling compound, and comprises: a fluorescence spectrum observation unit for obtaining a fluorescence spectrum of the liquid substance at an arbitrary excitation wavelength, and a spectrum analysis unit for obtaining data related to a peak intensity deviation degree based on the interaction between the fluorescent labeling compound in the liquid substance and an inspection object from the obtained fluorescence spectrum.
[0110] Furthermore, the evaluation device preferably includes a data processing unit for calculating the content of the inspection object using a calibration curve based on the peak intensity included in the data related to the peak intensity shift degree, and an information display unit for displaying the data related to the peak intensity shift degree.
[0111] Figure 1 It is a diagram schematically showing a configuration example of a liquid material evaluation device according to the present invention.
[0112] like Figure 1 As shown, the evaluation device 100 is installed in-line in a production process using a liquid material, and includes a fluorescence spectrum observation unit 110 and a computer 120 having a spectrum analysis unit, a data processing unit, and an information display unit.
[0113] <Fluorescence spectroscopy department>
[0114] The fluorescence spectrum observation unit 110 preferably includes an irradiation unit 111 for irradiating a liquid substance with light of an arbitrary excitation wavelength, and a light receiving unit 112 for receiving fluorescence emitted from the liquid substance excited by the light of the excitation wavelength to measure a fluorescence spectrum.
[0115] The irradiation unit 111 irradiates the liquid with light of an arbitrary excitation wavelength, and generates fluorescence from the fluorescent labeled compound.
[0116] The irradiation unit 111 is preferably composed of, for example, an LED driver 111a, an LED light source 111b, and an irradiation optical fiber collimator 111c, etc. The LED driver 111a supplies a current for lighting the LED light source 111b, whereby light of an arbitrary excitation wavelength emitted from the LED light source 111b via the irradiation optical fiber collimator 111c is irradiated to the liquid.
[0117] As the irradiation unit, commercially available products may be used, and examples thereof include a high-output LED light source (LSM series, manufactured by Ocean Photonics) and a high-output UV-Vis fiber light source unit (L10290, manufactured by Hamamatsu Photonics).
[0118] In addition, the range of the excitation light wavelength is preferably within the range of visible light. Here, the wavelength of the excitation light irradiated from the irradiation unit is a plurality of excitation wavelengths showing a fluorescence spectrum effective for measurement input by the user using a keyboard, a mouse, etc., and can be arbitrarily changed. The plurality of excitation wavelengths showing a fluorescence spectrum effective for the above-mentioned measurement is preferably selected from the fluorescence spectrum obtained by pre-acquiring the fluorescence fingerprint of the liquid or the fluorescence spectrum when the excitation wavelength is changed by several nanometers in a step.
[0119] The light receiving unit 112 receives fluorescence emitted from the fluorescent labeled compound by irradiation with excitation light, measures the excitation light wavelength, fluorescence wavelength, and fluorescence intensity from the received fluorescence, and transmits the measured data to the spectrum analysis unit (computer 120).
[0120] The light receiving unit 112 is preferably composed of, for example, a spectrometer 112a and a light receiving fiber collimator 112b, etc. Then, the fluorescence wavelength and fluorescence intensity of the fluorescence received by the spectrometer 112a via the light receiving fiber collimator 112b are measured, and the data are sent to the spectrum analysis unit (computer 120).
[0121] As the above-mentioned optical splitter, a commercially available product can be used, and examples thereof include a small fiber optical splitter (USB2000 manufactured by Ocean Photonics Corporation) and a multi-channel optical splitter (PMA-12 manufactured by Hamamatsu Photonics Corporation).
[0122] It should be noted that the irradiation optical fiber collimator 111c connected to the LED light source 111b is arranged in a pipe (for example, Figure 1 Symbol P1 in the figure), near the liquid delivery pump P2. In addition, the optical fiber collimator 112b for receiving light connected to the spectrometer 112a is arranged near the pipe P1 through which the liquid flows and the liquid delivery pump P2 in a manner capable of receiving fluorescence emitted from the liquid. In addition, the optical fiber collimator 111c for irradiation and the optical fiber collimator 112b for receiving light are preferably covered by a light shielding cover 113.
[0123] <Spectral Analysis Department>
[0124] The spectrum analysis unit obtains data related to the peak intensity shift degree from the fluorescence spectrum obtained by the spectrum observation unit according to the interaction between the fluorescent labeling compound in the liquid and the inspection object, and then sends the obtained data related to the peak intensity shift degree to the data processing unit.
[0125] <Data Processing Department>
[0126] The data processing unit calculates the content of the inspection object based on the data related to the peak intensity shift degree obtained by the spectrum analysis unit using a pre-made calibration curve, and sends the calculated content or the data related to the peak intensity shift degree to the information display unit.
[0127] <Information display section>
[0128] The information display unit displays information according to the display signal input from the data processing unit, specifically, the data related to the peak intensity shift and the content of the inspection object. Specifically, the data related to the peak intensity shift include the excitation wavelength of the light irradiated on the liquid, the fluorescence spectrum at the excitation wavelength, the peak intensity shift (the fluorescence wavelength of the characteristic peak and the change in the fluorescence intensity), etc.
[0129] The information display unit is configured to include, for example, an LCD (Liquid Crystal Display) and performs display using, for example, a dot matrix method.
[0130] As the spectrum analysis unit, data processing unit and information display unit, for example, a general computer (computer) 120 can be used. In the case of processing a very large amount of data or in applications requiring ultra-high-speed processing, a dedicated integrated circuit (ASIC) can be provided.
[0131] The computer 120 can centrally control the entire operation of the evaluation device 100 and includes a memory, a control unit, a calculation processing unit, etc. The user can input measurement processing conditions, etc., into the computer 120 using a keyboard and a mouse.
[0132] Next, refer to Figure 2 An example of a process of acquiring data related to the peak intensity shift degree of a liquid material in the liquid material evaluation apparatus 100 configured as described above will be described.
[0133] Figure 2 This is a flowchart showing a control procedure of the computer 120 executed in the liquid material evaluation device.
[0134] like Figure 2 As shown, for the fluorescent labeled compound in the liquid object to be measured, the fluorescent fingerprint or excitation wavelength is changed in advance by a few nanometers (for example, 5 nm each time) and measured using a spectrophotometer. Based on the measured fluorescence spectrum group, the LED light source is switched to irradiate the excitation wavelength selected by the user that is effective for the measurement (step S1).
[0135] Next, the liquid is irradiated with excitation light from the switched LED light source (irradiation unit) (step S2). The irradiation time and irradiation intensity of the excitation light are appropriately set according to the fluorescent labeled compound in the liquid. In addition, at this time, the liquid can be transported by a transport mechanism in a manner of irradiation at a desired position. When the liquid is a coating or a coating liquid, it is preferably carried out online by a film forming device.
[0136] Next, the liquid substance is irradiated with excitation light, and the fluorescence emitted from the fluorescent labeled compound in the liquid substance excited by the light of the excitation wavelength is received by the spectrometer (light receiving unit) as a spectroscopic spectrum, that is, the fluorescence spectrum is observed (step S3), and the peak wavelength or intensity is measured based on the fluorescence spectrum, that is, data related to the peak intensity deviation (spectral analysis) is obtained (step S4), and the obtained data is sent to a computer.
[0137] The content of the inspection object is calculated from the data related to the peak intensity shift sent to the computer based on a calibration curve prepared in advance, that is, data processing is performed (step S5).
[0138] It is determined whether the calculated content of the inspection object is within the range of the specified value (step S6). If it is within the range (step S6; yes), it is determined that there is no abnormality and the process ends. If it is outside the range (step S6; no), it is determined to be abnormal, and a warning is issued by display or sound (step S7), and the abnormality occurrence record such as the place, time and type of abnormality is obtained (step S8), and the process ends.
[0139] <Application examples of liquid material evaluation equipment>
[0140] (Application Example 1)
[0141] A description will be given of a case where the liquid material evaluation apparatus of the present invention is used in a film forming process of an optical film.
[0142] The optical film can be formed by a solution casting method or a melt casting method. In the following description, the case of using the solution casting method is described as an example.
[0143] Figure 3 This is a diagram schematically showing an example of a dope preparation step, a casting step, a drying step, and a winding step in a solution casting film forming method.
[0144] The fine particle dispersion obtained by dispersing the solvent and the matting agent by a disperser is stored in the storage tank 42 from the feed tank 41 through the filter 44. On the other hand, the cycloolefin resin as the main coating is dissolved in the dissolving tank 1 together with the solvent (solvent) and the fluorescent labeling compound involved in the present invention, and the matting agent stored in the storage tank 42 is appropriately added and mixed to form the main coating. The obtained main coating is filtered from the filter 3 and the storage tank 4 by the filter 6, and the additive is added by the confluence pipe 20, and the mixture is sent to the pressure mold 30 after mixing by the mixer 21.
[0145] Meanwhile, additives (such as ultraviolet absorbers) are dissolved in a solvent, passed through filter 12 from additive feed tank 10, and stored in storage tank 13. Thereafter, the additives are passed through filter 15, pipe 16, and mixed with the main coating material by confluence pipe 20 and mixer 21.
[0146] The main coating material sent to the pressure die 30 is cast onto a metal belt-shaped support 31 to form a base film 32, and after a predetermined drying, it is peeled off at a peeling position 33 to obtain a raw material film. The peeled base film 32 is passed through a plurality of conveying rollers and dried to a predetermined residual solvent amount, and then stretched by a stretching device 34 to a predetermined stretching ratio in the longitudinal direction or the width direction, and heated to a predetermined residual solvent amount. After stretching, it is passed through a conveying roller 36, dried by a drying device 35 to a predetermined residual solvent amount, and wound into a roll by a winding device 37.
[0147] In the solution casting film forming method as described above, the evaluation device for the liquid substance of the present invention is preferably configured as follows, for example, depending on the purpose of detecting the nature of the liquid substance.
[0148] (1) When the purpose is to detect the state of the paint before filtration, it is preferably arranged between the liquid feeding pump 2 and the filter 3.
[0149] (2) When the purpose is to detect the state of the paint before the junction pipe 20, it is preferably arranged between the filter 6 and the conduit 8 or between the filter 15 and the conduit 16.
[0150] (3) When the purpose is to detect the state of the coating material after merging, it is preferably arranged between the mixer 21 and the pressure die 30 .
[0151] By configuring the liquid material evaluation device of the present invention in the solution casting film forming process, for example, the fluorescence spectrum of the coating (liquid material) can be measured at any time, and even slight changes in the water content, impurities, etc. in the coating can be easily and quickly detected.
[0152] The coating material used in the solution casting film forming method may contain at least a solvent, a resin, and a non-reactive additive (fluorescent labeling compound).
[0153] Preferred resins used in the coating material of the present invention include cycloolefin resins, acrylic resins, triacetyl cellulose resins, etc. The cycloolefin resins will be described below.
[0154] 《Cyclic olefin resins》
[0155] The cycloolefin resin contained in the coating of the present invention is preferably formed by a resin composition containing at least one hydrogen bond accepting group. Generally speaking, the cycloolefin resin is a hydrophobic resin, so if there is water during film formation, it is easy to separate, which is not preferred from the viewpoint of transparency. By forming it with a resin composition containing at least one hydrogen bond accepting group, it can form a hydrogen bond with the hydroxyl group of the alcohol or the hydroxyl group of the hindered phenol compound, so even if it contains a little water, it can maintain transparency, and on the contrary, the film strength is improved by hydrogen bonding.
[0156] The "hydrogen bond accepting group" refers to a functional group that accepts a hydrogen atom when forming a hydrogen bond.
[0157] Examples of the hydrogen bond accepting group include an alkoxy group having 1 to 10 carbon atoms, an acyloxy group having 1 to 10 carbon atoms, an alkoxycarbonyl group having 2 to 10 carbon atoms, an allyloxycarbonyl group, a cyano group, an amide group, a group containing an imide ring, a triorganosiloxy group, a triorganosilyl group, an acyl group, an alkoxysilyl group having 1 to 10 carbon atoms, a group containing a sulfonyl group, and a carboxyl group. When these polar groups are further specifically described, as the above-mentioned alkoxy group, for example, methoxy, ethoxy and the like can be mentioned; as the acyloxy group, for example, alkylcarbonyloxy groups such as acetoxy and propionyloxy, and arylcarbonyloxy groups such as benzoyloxy can be mentioned; as the alkoxycarbonyl group, for example, methoxycarbonyl, ethoxycarbonyl and the like can be mentioned; as the allyloxycarbonyl group, for example, phenoxycarbonyl, naphthoxycarbonyl, fluorenyloxycarbonyl, biphenyloxycarbonyl and the like can be mentioned; as the triorganosiloxy group, for example, trimethylsilyloxy, triethylsilyloxy and the like can be mentioned; as the triorganosilyl group, for example, trimethylsilyl, triethylsilyl and the like can be mentioned; as the alkoxysilyl group, for example, trimethoxysilyl, triethoxysilyl and the like can be mentioned.
[0158] The amount of the cycloolefin resin containing the hydrogen bond accepting group contained in the resin component is not particularly limited, and the content ratio is preferably 10 to 100% by mass. If it is 10% by mass or more, the obtained ring-opening copolymer is easy to show solubility in solvents such as toluene and dichloromethane, so it is preferred. In addition, from the viewpoint of solubility, film strength, and transparency, it is more preferably in the range of 30 to 100% by mass.
[0159] Examples of the cycloolefin-based resin according to the present invention include the following (co)polymers.
[0160] General formula (I)
[0161]
[0162] [In the formula, p is 0 or 1, and m is an integer of 0 or more. R 1 ~R 4 Each independently represents a hydrogen atom, a hydrocarbon group, a halogen atom or a hydrogen bond accepting group. 1 ~R 4 Two or more of them may be bonded to each other to form an unsaturated bond, a monocyclic ring or a polycyclic ring. The monocyclic ring or polycyclic ring may have a double bond and may form an aromatic ring.
[0163] In the present invention, the preferred hydrogen bond accepting group retention ratio of the cycloolefin resin is preferably 1 ~R 4 1 to 2 of them have hydrogen bond accepting groups.
[0164] The ratio of hydrogen bond accepting groups in the cycloolefin resin can be determined, for example, by carbon-13 nuclear magnetic resonance ( 13 CNMR) spectroscopy was used for identification.
[0165] In the general formula (I), R 1 and R 3 is a hydrogen atom or a hydrocarbon group having 1 to 10 carbon atoms, more preferably 1 to 4 carbon atoms, and particularly preferably 1 to 2 carbon atoms, and R 2 and R 4 At least one of them represents a polar hydrogen bond accepting group other than a hydrogen atom and a hydrocarbon group, and from the viewpoint of a high glass transition temperature and excellent mechanical strength, p and m are preferably m=1 and p=0.
[0166] Examples of the halogen atom include fluorine, chlorine, and bromine atoms. Examples of the hydrocarbon group having 1 to 30 carbon atoms include alkyl groups such as methyl, ethyl, and propyl; cycloalkyl groups such as cyclopentyl and cyclohexyl; alkenyl groups such as vinyl, allyl, and propenyl; and aromatic groups such as phenyl, biphenyl, naphthyl, and anthracenyl. These hydrocarbon groups may be substituted, and examples of the substituent include halogen atoms such as fluorine, chlorine, and bromine atoms, and phenylsulfonyl.
[0167] The preferred molecular weight of the cycloolefin resin of the present invention is 0.2 to 5 cm in terms of intrinsic viscosity [η] inh. 3 / g, more preferably 0.3 to 3 cm 3 / g, particularly preferably 0.4 to 1.5 cm 3 / g, the number average molecular weight (Mn) measured by gel permeation chromatography (GPC) in terms of polystyrene is preferably 8,000 to 100,000, more preferably 10,000 to 80,000, particularly preferably 12,000 to 50,000, and the weight average molecular weight (Mw) is preferably 20,000 to 300,000, more preferably 30,000 to 250,000, particularly preferably 40,000 to 200,000.
[0168] When the intrinsic viscosity [η]inh, the number average molecular weight and the weight average molecular weight are within the above ranges, the heat resistance, water resistance, chemical resistance and mechanical properties of the cycloolefin resin and the moldability of the cycloolefin resin film of the present invention become good.
[0169] The glass transition temperature (Tg) of the cycloolefin resin of the present invention is usually 110°C or higher, preferably 110 to 350°C, more preferably 120 to 250°C, and particularly preferably 120 to 220°C. When Tg is 110°C or higher, deformation caused by use under high temperature conditions or secondary processing such as coating and printing can be suppressed, so it is preferred. In addition, when Tg is 350°C or lower, resin degradation caused by molding or heat during molding can be suppressed, so it is preferred.
[0170] The cycloolefin resin described above can be preferably a commercial product. Examples of the commercial product include Arton G, Arton F, Arton R, and Arton RX, which are sold by JSR Corporation. These commercial products can be used.
[0171] Solvents
[0172] Examples of the solvent contained in the coating material according to the present invention include organic solvents.
[0173] Examples of the organic solvent include chlorine-based solvents such as chloroform and dichloromethane; aromatic solvents such as toluene, xylene, benzene and mixed solvents thereof; alcohol-based solvents such as methanol, ethanol, isopropanol, n-butanol and 2-butanol; methyl cellosolve, ethyl cellosolve, butyl cellosolve, dimethylformamide, dimethyl sulfoxide, dimethicone ... Alkane, cyclohexanone, tetrahydrofuran, acetone, methyl ethyl ketone (MEK), ethyl acetate, diethyl ether, etc. These solvents may be used alone or in combination of two or more.
[0174] In addition, the organic solvent is preferably a mixed solvent of a good solvent and a poor solvent. For the good solvent, for example, as a chlorine-based organic solvent, dichloromethane can be mentioned, and as a non-chlorine-based organic solvent, methyl acetate, ethyl acetate, amyl acetate, acetone, methyl ethyl ketone, tetrahydrofuran, 1,3-dioxolane, 1,4-dioxolane, The good solvent is preferably used in an amount of 55% by mass or more, more preferably 70% by mass or more, and still more preferably 80% by mass or more relative to the total amount of the solvent.
[0175] The poor solvent is preferably an alcohol solvent. From the viewpoint of improving the stripping property and enabling high-speed casting, the alcohol solvent is preferably selected from methanol, ethanol and butanol. Among them, methanol or ethanol is preferably used. If the ratio of alcohol in the coating increases, the base film is gelled and easily peeled off from the metal support. In addition, when the ratio of alcohol is small, it also has the effect of promoting the dissolution of cycloolefin resin and other compounds in the non-chlorine organic solvent system.
[0176] In the present invention, from the viewpoint of improving the planarity of the obtained optical film, it is preferred to form the film using a coating material having an alcohol concentration within a range of 0.5 to 15.0% by mass.
[0177] 《Non-reactive additives》
[0178] Examples of the non-reactive additive (fluorescent labeling compound) contained in the coating material according to the present invention include the above-mentioned antioxidant (for example, Irganox 1076 (manufactured by BASF Japan Co., Ltd.), pigments (NIR pigments, NUV pigments), and the like.
[0179] Other additives
[0180] The coating material according to the present invention may further contain a matting agent such as a plasticizer, a phase difference enhancing agent, and silica particles described in JP-A-2017-90872.
[0181] (Application Example 2)
[0182] Next, a description will be given of a case where the liquid material evaluation apparatus of the present invention is used in a step of applying a hard coat layer coating liquid to a functional film.
[0183] Figure 4 This is a schematic diagram showing an example of a hard coat layer forming apparatus used when producing a functional film.
[0184] The hard coating forming device is a so-called roll-to-roll type device. The hard coating forming device 130 includes: a delivery roller 132a, conveying rollers 133a, 133b, 133c, 133d, 133e, a coating liquid coating device 134 for forming a hard coating, a heating and drying section 135, a conveying roller 136, an ultraviolet irradiation device 137, and a winding roller 132b.
[0185] In such a hard coat forming device 130, a substrate and a film 131 having a functional layer are fed out from a feed roller 132a. Then, a coating liquid for forming a hard coat is applied on the functional layer of the film 131 fed out by the roller or on the substrate by a coating liquid coating device 134. It should be noted that before applying the coating liquid for forming a hard coat, it is preferable to remove static electricity from the film.
[0186] Examples of the coating liquid coating apparatus include a die coater, a gravure coater, and a comma coater.
[0187] The substrate coated with the coating liquid for forming a hard coat layer is transported to the heating and drying section 135 via the transport rollers 133b and 133c. In the drying section, the solvent in the coating liquid is dried. There is no particular limitation on the drying means, and warm air drying, infrared drying, and microwave drying can be used. It should be noted that Figure 4 , it is described that there are four drying devices in the heating and drying section 135, but it is not limited to the form of using multiple drying devices for drying, and only one drying device can be used for drying. As the drying temperature at this time, it can be appropriately set to a temperature that can remove the used solvent, usually 70 to 120°C.
[0188] In order to irradiate ultraviolet rays by the ultraviolet irradiation device 137 , the substrate coated with the coating liquid for forming a hard coat layer is transported via the transport roller 133 d .
[0189] The ultraviolet curing resin is cured by the irradiated ultraviolet rays in the ultraviolet irradiation device 137. As the ultraviolet irradiation device, for example, an ultraviolet lamp such as a high-pressure UV lamp (high-pressure mercury lamp) or a metal halide lamp can be used. Figure 4 The figure shows an ultraviolet irradiation device, but other curing devices such as a heating device may also be used depending on the curing resin used. In the case of a polysiloxane hard coating material, after the solvent is dried after coating, it is preferably subjected to heat treatment at a temperature range of 50 to 150° C. for 30 minutes to several days in order to promote the curing and crosslinking of the hard coating material.
[0190] When using active energy rays to cure resins, the reactivity will change depending on the wavelength, illuminance, and light quantity of the active energy rays, and it is necessary to select the best conditions according to the resin used. For example, when using active energy rays as ultraviolet lamps, the illuminance is preferably 50 to 1500 mW / cm 2 The irradiation energy is preferably 50 to 1500 mJ / cm 2 .
[0191] By the ultraviolet irradiation treatment, a hard coat layer is formed on the substrate or the functional layer.
[0192] The thickness of the hard coating layer is preferably 0.1 to 20 μm, more preferably 1 to 15 μm, and still more preferably 3 to 10 μm. If it is 0.1 μm or more, the hard coating property tends to be improved, and if it is 20 μm or less, the curling of the hard coating layer tends to be small and the bending resistance tends to be maintained.
[0193] In addition, although the above description is made on the form in which the hard coat layer is formed on the substrate or the functional layer, the present invention is not limited to this form, and the hard coat layer may be formed on other intermediate layers or the like.
[0194] In the hard coating forming device as described above, the evaluation device for the liquid material of the present invention is preferably arranged, for example, near the coating liquid coating device 134 or the conveying roller 133b just after the coating liquid for hard coating forming is applied, between the conveying roller 133c and the conveying roller 133d during drying in the drying section, or near the conveying roller 133d just after drying.
[0195] By configuring the liquid evaluation device of the present invention in the hard coating formation process, for example, the fluorescence spectrum of the coating liquid for forming the hard coating or the coating film of the applied hard coating can be measured at any time, and slight changes in the water content, impurities, etc. of the above-mentioned coating liquid for forming the hard coating or the coating film can be easily and quickly detected.
[0196] The hard coat layer-forming coating liquid used in the hard coat layer-forming step may contain at least a solvent, a resin, and a non-reactive additive (fluorescent labeling compound).
[0197] Resin
[0198] As the resin used in the coating solution for forming the hard coat layer involved in the present invention, thermosetting resins and active energy ray curing resins can be cited. From the perspective of easy molding, active energy ray curing resins are preferred. Such curing resins can be used alone or in combination of two or more. In addition, the curing resin can use a commercial product or a synthetic product.
[0199] The active energy ray-curable resin refers to a resin that is cured through a crosslinking reaction or the like by irradiation with active energy rays such as ultraviolet rays or electron beams.
[0200] As the active energy ray curing resin, it is preferred to use a component containing a monomer having an ethylenically unsaturated double bond, and to cure it by irradiating active energy rays such as ultraviolet rays or electron beams to form an active energy ray hard coating. As the active energy ray curing resin, resins represented by ultraviolet curing resins and electron beam curing resins can be cited, preferably ultraviolet curing resins cured by ultraviolet irradiation. The active energy ray curing resin can be used alone or in combination of two or more.
[0201] As the ultraviolet curable resin, for example, ultraviolet curable urethane acrylate resin, ultraviolet curable polyester acrylate resin, ultraviolet curable epoxy acrylate resin, ultraviolet curable polyol acrylate resin, or ultraviolet curable epoxy resin, etc. are preferably used. Among them, ultraviolet curable urethane acrylate resin and ultraviolet curable polyol acrylate resin are preferred.
[0202] UV curable polyurethane acrylate resin can be easily obtained by reacting the product obtained by reacting polyester polyol with isocyanate monomer or prepolymer with monomers of acrylate system having hydroxyl group such as 2-hydroxyethyl acrylate, 2-hydroxyethyl methacrylate (hereinafter, only represented as acrylate when methacrylate is included in acrylate), 2-hydroxypropyl acrylate, etc. For example, a mixture of 100 parts of UNIDIC 17-806 (made by Dainippon Ink Co., Ltd.) and 1 part of CORONATE L (made by Nippon Polyurethane Industry Co., Ltd.) recorded in Japanese Patent Publication No. 59-151110 is preferably used. As UV curable polyurethane acrylate resin, commercially available products can be used, and as commercially available products, BEAMSET (registered trademark) 575, 577 (made by Arakawa Chemical Industries, Ltd.), purple light (registered trademark) UV series, etc. can be cited.
[0203] Examples of the ultraviolet curable polyester acrylate resin generally include resins formed by reacting polyester polyol with dihydroxyethyl acrylate or 2-hydroxyacrylate monomers, and resins described in Japanese Patent Application Laid-Open No. 59-151112 can be used.
[0204] Examples of the ultraviolet curable epoxy acrylate resin include a resin obtained by converting epoxy acrylate into an oligomer, adding a reactive diluent and a photopolymerization initiator thereto, and reacting the oligomer. The resin described in Japanese Patent Application Laid-Open No. 1-105738 can be used.
[0205] As the ultraviolet curing polyol acrylate resin, ethylene glycol (meth) acrylate, polyethylene glycol di(meth) acrylate, glycerol tri(meth) acrylate, trimethylolpropane triacrylate, pentaerythritol triacrylate, pentaerythritol tetraacrylate, dipentaerythritol pentaacrylate, dipentaerythritol hexaacrylate, alkyl-modified dipentaerythritol pentaacrylate, etc. can be mentioned. As the ultraviolet curing polyol acrylate resin, commercially available products can be used, and as commercially available products, Sartomer SR295, SR399 (manufactured by Sartomer Co., Ltd.) and the like can be mentioned.
[0206] In addition, a polymerizable organic silicon compound may be used in combination with (or alone with) an ultraviolet curable resin. The polymerizable organic silicon compound is preferably used in combination with the above-mentioned ultraviolet curable resin.
[0207] The polymerizable organic silicon compound is a compound having a main skeleton (organic silicon skeleton) and a polymerizable group formed via a siloxane bond in the molecule.
[0208] The polymerizable group is a group that can polymerize with the above-mentioned ultraviolet curable resin, and examples thereof include groups having polymerizable double bonds such as (meth)acryloyl and (meth)acryloyloxy. (Meth)acryloyl is preferred. Therefore, the preferred polymerizable organosilicon compound is preferably organosilicon (meth)acrylate or organosilicon (meth)acrylate oligomer (hereinafter collectively referred to as organosilicon (meth)acrylate).
[0209] In addition, from the viewpoint of improving compatibility with the above-mentioned ultraviolet curing resin, the polymerizable organic silicon compound is preferably an organic modified polymerizable organic silicon compound containing a portion in the molecule that improves compatibility with the ultraviolet curing resin. As such an organic modified polymerizable organic silicon compound, for example, urethane modified, amino modified, alkyl modified, epoxy modified, carboxyl modified, alcohol modified, fluorine modified, alkyl aralkyl polyether modified, epoxy·polyether modified or polyether modified polymerizable organic silicon compounds can be cited.
[0210] For example, when the ultraviolet curable resin includes an ultraviolet curable polyurethane acrylate resin, the polymerizable organic silicon compound is preferably a urethane modified organic silicon (meth) acrylate. The urethane modified organic silicon (meth) acrylate is obtained by, for example, reacting an organic silicon compound having OH at both ends with a polyisocyanate to obtain a terminal isocyanate organic silicon compound, and reacting the terminal isocyanate organic silicon compound with the above-mentioned hydroxyl-containing (meth) acrylate.
[0211] A commercially available product may be used as the polymerizable organic silicon compound. Examples of the commercially available product include EBECRYL 1360, EBECRYL 350, and KRM 8495 (manufactured by DAICEL-ALLNEX), and CN 9800 and CN 990 (manufactured by Arkema).
[0212] In addition, since the polymerizable organic silicon compound can also form a polymer, it can become a polymerizable component of the resin.
[0213] The ultraviolet curable resin preferably uses a photopolymerization initiator (free radical polymerization initiator). As the photopolymerization initiator, benzoin and its alkyl ethers such as benzoin, benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether, and benzyl methyl ketal can be used; acetophenones such as acetophenone, 2,2-dimethoxy-2-phenylacetophenone, and 1-hydroxycyclohexyl phenyl ketone; anthraquinones such as methyl anthraquinone, 2-ethyl anthraquinone, and 2-amyl anthraquinone; thioxanthones such as thioxanthone, 2,4-diethyl thioxanthone, and 2,4-diisopropyl thioxanthone; acetophenone dimethyl ketal, benzoin dimethyl ether, and benzophenones and azo compounds such as benzophenone and 4,4-dimethylaminobenzophenone can be used. They can be used alone or in combination of two or more. In addition, it can also be used in combination with tertiary amines such as triethanolamine and methyldiethanolamine; photoinitiator aids such as benzoic acid derivatives such as 2-dimethylaminoethylbenzoic acid and 4-dimethylaminobenzoic acid ethyl ester. Commercially available photopolymerization initiators can be used, for example, Irgacure (registered trademark) -184, 819, 907, 651, 1700, 1800, 819, 369, 261, DAROCUR-TPO (manufactured by BASF Japan Co., Ltd.), Darocure (registered trademark) -1173 (manufactured by Merck Co., Ltd.), Esacure-KIP150, TZT (manufactured by DKSH Japan Co., Ltd.), KAYACURE (registered trademark) BMS, DMBI (manufactured by Nippon Kayaku Co., Ltd.), etc. The amount of these photopolymerization initiators used is preferably 0.5 to 30 parts by weight, and more preferably 1 to 25 parts by weight relative to 100 parts by weight of the polymerizable component of the resin.
[0214] Examples of the thermosetting resin include silicone-based hard coating agents.
[0215] The polysiloxane hard coating agent uses a compound represented by the general formula RmSi(OR')n as a starting material. R and R' represent an alkyl group having 1 to 10 carbon atoms, and m and n are integers satisfying the relationship of m+n=4. Compounds in which hydrolyzable groups such as methoxy and ethoxy in the starting material are substituted by hydroxyl groups are generally called polyorganosiloxane hard coating agents. By applying and heating to cure, the dehydration condensation reaction is promoted, and the hard coating agent is formed into a film by curing and cross-linking.
[0216] As the polyorganosiloxane hard coating agent, commercially available products may be used, such as SarCoat series (Dongken), SR2441 (Toray Dow Corning Co.), KF-86 (Shin-Etsu Silicone Co.), Perma-New (registered trademark) 6000 (California Hardcoating Company), and the like.
[0217] In the case of a polysiloxane hard coating agent, after the solvent is dried after coating, a heat treatment at 50°C to 150°C for 30 minutes to several days is required to promote the curing and crosslinking of the hard coating agent. In view of the heat resistance of the coated substrate and the stability of the substrate when rolled, it is preferably treated at 40°C to 80°C for 2 days or more.
[0218] The content of the curable resin (including the polymerizable organosilicon compound) in the hard coat layer-forming coating liquid is preferably 40 to 90% by mass, more preferably 50 to 85% by mass, based on 100% by mass (solid content) of the total hard coat layer.
[0219] Solvents
[0220] The solvent contained in the coating liquid for forming a hard coat layer involved in the present invention can be appropriately selected from, for example, hydrocarbons (toluene, xylene), alcohols (methanol, ethanol, isopropanol, butanol, cyclohexanol), ketones (acetone, methyl ethyl ketone, methyl isobutyl ketone), esters (methyl acetate, ethyl acetate, methyl lactate), glycol ethers, and other organic solvents, or they can be mixed and used.
[0221] The amount of the solvent in the coating liquid for forming a hard coat layer is appropriately set to an amount capable of dissolving and dispersing the curable resin, and is about 20 to 80% by mass based on 100% by mass of the coating liquid.
[0222] 《Non-reactive additives》
[0223] Examples of the non-reactive additive (fluorescent labeling compound) contained in the hard coat layer-forming coating liquid of the present invention include the above-mentioned antioxidant (for example, Irganox 1076 (manufactured by BASF Japan Co., Ltd.), pigments (NIR pigments, NUV pigments), and the like.
[0224] Other additives
[0225] For the purpose of imparting an infrared shielding function to the hard coat layer and improving mechanical strength, the coating liquid for forming a hard coat layer preferably contains metal oxide particles described in Japanese Patent Application Laid-Open No. 2018-196322.
[0226] In addition, a surfactant can be added to the coating solution for forming the hard coat layer to impart leveling properties, water resistance, lubricity, etc. There are no particular restrictions on the type of surfactant, and acrylic surfactants, silicone surfactants, fluorine-based surfactants, etc. can be used. From the viewpoint of leveling properties, water resistance, and lubricity, it is particularly preferred to use a fluorine-based surfactant. As examples of fluorine-based surfactants, for example, commercially available products such as MEGAFAC (registered trademark) F series (F-430, F-477, F-552 to F-559, F-561, F-562, etc.) manufactured by DIC Corporation, MEGAFAC (registered trademark) RS series (RS-76-E, etc.) manufactured by DIC Corporation, Surflon (registered trademark) series manufactured by AGC SEIMI CHEMICAL Co., Ltd., POLYFOX series manufactured by OMNOVA SOLUTIONS, ZX series manufactured by T&K TOKA Co., Ltd., Optool series manufactured by DAIKIN INDUSTRIES Co., Ltd., and FTERGENT (registered trademark) series (602A, 650A, etc.) manufactured by Neos Corporation can be used.
[0227] The method for preparing the coating solution for forming a hard coat layer is not particularly limited, and the coating solution is obtained by adding each component to a solvent and mixing appropriately. The order and method of addition are not particularly limited, and each component can be added sequentially and mixed while stirring, or can be added all at once and mixed while stirring.
[0228] In the hard coat forming step of the present invention, there is no particular limitation on the substrate used. From the viewpoint of bendability, a resin substrate is preferred, which may be transparent or opaque. In applications such as automotive applications that require transparency under visible light from a design perspective, it is preferably transparent in the visible light region.
[0229] As a resin substrate, for example, polyolefin films (polyethylene, polypropylene, etc.), polyester films (polyethylene terephthalate, polyethylene naphthalate, etc.), polyvinyl chloride, triacetyl cellulose, etc., preferably polyester films can be used. As a polyester film (hereinafter referred to as polyester), it is not particularly limited, preferably a polyester with dicarboxylic acid components and diol components as main components and film-forming properties. In polyester, from the viewpoints of transparency, mechanical strength, dimensional stability, etc., it is preferred to use terephthalic acid or 2,6-naphthalene dicarboxylic acid as a dicarboxylic acid component, ethylene glycol or 1,4-cyclohexanedimethanol as a diol component as a polyester as a main component. Among them, preferably a polyester with polyethylene terephthalate or polyethylene naphthalate as a main component, a copolymerized polyester consisting of terephthalic acid and 2,6-naphthalene dicarboxylic acid and ethylene glycol, and a polyester with a mixture of two or more of these polyesters as a main component.
[0230] The thickness of the substrate is preferably 10 to 300 μm, more preferably 20 to 150 μm. The substrate may be a structure in which two or more sheets are stacked, and in this case, the types of the substrates may be the same or different.
[0231] The resin substrate can be manufactured by a conventional method. The resin substrate can be an unstretched film, a stretched film in which one side is stretched, or a biaxially stretched film. From the viewpoint of improving strength and suppressing thermal expansion, a stretched film is preferred.
[0232] The functional layer formed on the substrate may be any functional layer as long as it is a thin film that imparts a certain function to the substrate. As the functional layer, for example, an optical film that transmits or reflects and absorbs specific light (for example, an antireflection film, an infrared shielding film, an ultraviolet shielding film, etc.), a barrier film that inhibits the transmission of oxygen and / or water vapor, a polarizing film, a phase difference film, a photosensitive film, etc. can be cited.
[0233] Here, the film having a substrate and a functional layer only needs to have a substrate and a functional layer, and includes not only a form in which the functional layer is directly provided on the substrate, but also a form in which other intermediate layers are provided on the substrate and the functional layer is provided on the intermediate layers, a form in which other intermediate layers are provided on the side of the substrate opposite to the functional layer, a form in which other intermediate layers are included on the functional layer, etc.
[0234] The material constituting the functional layer can be appropriately selected according to the functional layer of the target. For example, metal oxides such as aluminum, silicon dioxide, zirconium oxide, tantalum oxide, titanium oxide, tin oxide, and indium oxide doped with tin, metal nitride oxides such as silicon oxynitride, metals such as silver, gold, and copper, metal fluorides such as magnesium fluoride, and conductive polymers such as polymers and polythiophenes can be cited. From the perspective of low conductivity and easier acquisition of the effects of the present invention, it is preferred that the functional layer contains a polymer.
[0235] The functional layer may contain various additives as required. Specifically, it may contain various anionic, cationic or nonionic surfactants; dispersants such as polycarboxylic acid ammonium salts, allyl ether copolymers, benzene sulfonic acid sodium salts, graft compound dispersants, polyethylene glycol type nonionic dispersants; pH adjusters; defoamers and other well-known additives.
[0236] The thickness of the functional layer is appropriately set so as to satisfy the required function, and is, for example, about 10 nm to 100 μm.
[0237] (Application Example 3)
[0238] Furthermore, the liquid material evaluation device of the present invention is also suitably used in a step of applying a coating liquid for forming an antistatic layer provided on a near-infrared reflective film.
[0239] It should be noted that in this case, the coating liquid for the antistatic layer can be applied by a coating liquid coating device (gravure coater, etc.) as in the above-mentioned Application Example 2. Specifically, in the device for forming the antistatic layer, it is preferred that the evaluation device for the liquid of the present invention is arranged near the conveying roller just after the coating liquid coating device or the coating liquid for forming the antistatic layer is applied, and in the drying of the drying section after the coating, near the conveying roller just after the drying.
[0240] By configuring the evaluation device of the liquid of the present invention in the process of forming the antistatic layer, for example, the fluorescence spectrum of the coating liquid for forming the antistatic layer or the coating film of the coated antistatic layer can be measured at any time, and slight changes in the water content, impurities, etc. of the above-mentioned coating liquid for forming the antistatic layer or the coating film can be easily and quickly detected.
[0241] As the antistatic layer-forming coating liquid, a coating liquid containing a known conductive composition can be used, and it is only necessary to contain at least a solvent, a resin, and a non-reactive additive (fluorescent labeling compound).
[0242] Resin
[0243] As the resin used in the coating solution for forming the antistatic layer involved in the present invention, preferably polyester resin, acrylic acid modified polyester resin, polyurethane, acrylic resin, vinyl resin, vinylidene chloride resin, polyethylene imine vinylidene resin, polyethylene imine, polyvinyl alcohol, modified polyvinyl alcohol, cellulose ester resin and gelatin etc. It should be noted that the details of these resins are recorded in Japanese Patent Gazette No. 5811536.
[0244] Solvents
[0245] Examples of the solvent contained in the antistatic layer-forming coating liquid of the present invention include water and organic solvents. Examples of the organic solvent include methyl ethyl ketone, acetone, and acetylacetone.
[0246] 《Non-reactive additives》
[0247] Examples of the non-reactive additive (fluorescent labeling compound) contained in the antistatic layer-forming coating solution of the present invention include the above-mentioned antioxidant (for example, Irganox 1076 (manufactured by BASF Japan Co., Ltd.), pigments (NIR pigments, NUV pigments), and the like.
[0248] 《Conductive composition》
[0249] Examples of the conductive composition contained in the antistatic layer-forming coating liquid of the present invention include polyaniline and its derivatives, preferably water-soluble sulfonated polyaniline, organic solvent-soluble polypyrrole, i.e., polypyrrole bonded with a long-chain alkyl substituent, polythiophene and its derivatives.
[0250] In addition, metal oxides are also preferably used as conductive compositions. Examples of metal oxides include ZnO, TiO2, SnO2, Al2O3, In2O3, SiO2, MgO, BaO, MoO2, V2O5, etc., or composite oxides thereof. From the perspectives of compatibility with the binder, conductivity, transparency, etc., SnO2 (tin oxide) is particularly preferred. As examples of heterogeneous elements, Sb, Nb, halogen elements, etc. may be added relative to SnO2. The addition amount of these heterogeneous elements is preferably in the range of 0.01 to 25 mol%, and particularly preferably in the range of 0.1 to 15 mol%.
[0251] Specific examples of the above-mentioned conductive composition are described in Japanese Patent No. 5811536.
[0252] (Application Example 4)
[0253] In addition, the evaluation device for the liquid of the present invention can also be used in the process of forming a near-infrared reflective film. That is, it can be used in the process of applying a coating liquid for a high refractive index layer and a low refractive index layer formed on a transparent support. In this case, as in the above-mentioned Application Example 2, the coating liquid for the high refractive index layer or the low refractive index layer can also be applied using a coating liquid coating device (gravure coater, etc.).
[0254] Specifically, in an apparatus for forming a high refractive index layer and a low refractive index layer, the evaluation apparatus for the liquid of the present invention is preferably arranged, for example, in a coating liquid coating apparatus or near a conveying roller just after coating a coating liquid for forming a high refractive index layer or a low refractive index layer, or near a conveying roller just after drying in a drying section after coating.
[0255] By configuring the evaluation device for the liquid material of the present invention in the process of forming the high refractive index layer or the low refractive index layer, it is possible to measure the fluorescence spectrum of, for example, the coating liquid for forming the high refractive index layer or the low refractive index layer or the coating film of the applied high refractive index layer or the low refractive index layer at any time, and it is possible to easily and quickly detect slight changes in the water content, impurities, etc. of the coating liquid for forming the high refractive index layer or the low refractive index layer or the coating film.
[0256] As the coating liquid for forming a high refractive index layer and the coating liquid for forming a low refractive index layer, known coating liquids for forming a high refractive index layer and coating liquids for forming a low refractive index layer (for example, refer to Japanese Patent No. 5593916) can be used, as long as they contain at least a solvent, a resin and a non-reactive additive (fluorescent labeling compound).
[0257] Resin
[0258] Examples of the resin used in the coating liquid for forming a high refractive index layer according to the present invention include hydrophilic resins.
[0259] As the hydrophilic resin, water-soluble resin, water-dispersible resin, colloid-dispersed resin or mixtures thereof can be enumerated. As a specific example of the hydrophilic resin, resins such as acrylic acid, polyester, polyamide, polyurethane, and fluorine can be enumerated, for example, polymers such as polyvinyl alcohol, gelatin, polyethylene oxide, polyvinyl pyrrolidone, casein, starch, agar, carrageenan, polyacrylic acid, polymethacrylic acid, polyacrylamide, polymethacrylamide, polystyrene sulfonic acid, cellulose, hydroxyethyl cellulose, carboxymethyl cellulose, hydroxyethyl cellulose, dextran, dextrin, pullulan, and water-soluble polyvinyl butyral can be enumerated, and polyvinyl alcohol is preferred among these.
[0260] The polymer used as the binder resin may be used alone or in combination of two or more, as required.
[0261] The molecular weight of the polymer used as the binder resin of the high refractive index layer is not particularly limited, but polyvinyl alcohol obtained by hydrolyzing vinyl acetate preferably has an average polymerization degree of 1000 or more, and particularly preferably has a degree of 1500 to 5000. The saponification degree is preferably 70 to 100%, particularly preferably 80 to 99.5%.
[0262] Solvents
[0263] When a water-soluble resin is used, a mixture containing water as a main component and a hydrophilic organic solvent added as necessary can be used as the solvent.
[0264] As the hydrophilic solvent, for example, alcohols such as methanol, ethanol, 2-propanol, and 1-butanol, esters such as ethyl acetate, butyl acetate, propylene glycol monomethyl ether acetate, and propylene glycol monoethyl ether acetate, ethers such as diethyl ether, propylene glycol monomethyl ether, and ethylene glycol monoethyl ether, amides such as dimethylformamide and N-methylpyrrolidone, ketones such as acetone, methyl ethyl ketone, acetylacetone, and cyclohexanone, aromatic hydrocarbons such as benzene, toluene, and xylene, aliphatic hydrocarbons such as heptane, hexane, pentane, decane, and cyclohexane, etc., can be cited, and one or more of these can be used. From an environmental perspective, water and alcohols are particularly preferably used as solvents for the coating solution.
[0265] 《Non-reactive additives》
[0266] Examples of the non-reactive additive (fluorescent labeling compound) contained in the high refractive index layer-forming coating solution of the present invention include the above-mentioned antioxidant (for example, Irganox 1076 (manufactured by BASF Japan Co., Ltd.), pigments (NIR pigments, NUV pigments), and the like.
[0267] 《Metal Oxides》
[0268] The coating liquid for forming a high refractive index layer according to the present invention preferably contains a metal oxide.
[0269] Examples of such metal oxides include TiO2 (titanium oxide), SiO2, ZrO2, Al2O3, ZnO, Sb2O3, ZrSiO4, and zeolite.
[0270] As the coating liquid for forming a low refractive index layer, a known coating liquid for forming a low refractive index layer can be used, as long as it contains at least a solvent, a resin, and a non-reactive additive (fluorescent labeling compound).
[0271] Resin
[0272] As the resin contained in the coating liquid for forming a low refractive index layer, a small amount of the hydrophilic binder resin contained in the above-mentioned coating liquid for forming a high refractive index layer can be used.
[0273] Solvents
[0274] The solvent contained in the coating liquid for forming a low refractive index layer may be the same as the solvent contained in the coating liquid for forming a high refractive index layer.
[0275] 《Non-reactive additives》
[0276] Examples of the non-reactive additive (fluorescent labeling compound) contained in the low refractive index layer-forming coating liquid of the present invention include the above-mentioned antioxidant (for example, Irganox 1076 (manufactured by BASF Japan Co., Ltd.), pigments (NIR pigments, NUV pigments), and the like.
[0277] 《Metal Oxides》
[0278] The coating liquid for forming a low refractive index layer according to the present invention preferably also contains the metal oxide contained in the coating liquid for forming a high refractive index layer.
[0279] Example
[0280] The present invention is specifically described below with reference to the following examples, but the present invention is not limited thereto. It should be noted that, in the following examples, unless otherwise specified, the operation is performed at room temperature (25° C.). In addition, unless otherwise specified, “%” and “parts” represent “mass %” and “mass parts”, respectively.
[0281] [Sample 1]
[0282] (Resin 1)
[0283] As the resin containing a cycloolefin polymer, a hydrogenated norbornene resin ("Arton G7810" manufactured by JSR Corporation) was used. Hereinafter, this cycloolefin resin is referred to as "COP".
[0284] (Preparation of Liquid 1)
[0285] A liquid (coating for optical film) 1 having the following composition was prepared. First, dichloromethane was added to a pressure dissolving tank. Then, COP was added to the pressure dissolving tank while stirring. Next, an antioxidant ("Irganox 1076" manufactured by BASF Japan Co., Ltd.) was added as a fluorescent labeling compound and stirred to completely dissolve.
[0286] COP: 100 parts by mass
[0287] Dichloromethane: 280 parts by mass
[0288] Irganox 1076: 100 mass ppm
[0289] [Sample 2]
[0290] (Preparation of Liquid Material 2)
[0291] In the preparation of the liquid material 1, a liquid material (optical film coating material) 2 was prepared in the same manner except that the solvent (methylene chloride) was not added.
[0292] [Sample 3]
[0293] (Preparation of Liquid 3)
[0294] In the preparation of the liquid material 1, a liquid material (coating material for an optical film) 3 was prepared in the same manner as in the preparation of the liquid material 1, except that COP was not added.
[0295] [Sample 4]
[0296] (Preparation of Liquid 4)
[0297] In the preparation of liquid 1, liquid (optical film coating material) 4 was prepared in the same manner except that the fluorescent labeling compound was changed to ELECUT S-418 (manufactured by Takemoto Oil & Fats Co., Ltd.) (reaction additive: chelating agent).
[0298] [Sample 5]
[0299] (Preparation of Liquid Material 5)
[0300] A liquid (coating for optical film) 5 of the following composition was prepared. First, dichloromethane and ethanol (92% by mass of dichloromethane and 8% by mass of ethanol) were added to a pressure dissolving tank. Next, COP was added to the pressure dissolving tank while stirring. Next, an antioxidant ("Irganox 1076" manufactured by BASF Japan Co., Ltd.) was added as a fluorescent labeling compound and stirred to completely dissolve it.
[0301] COP: 100 parts by mass
[0302] Dichloromethane: 260 parts by mass
[0303] Ethanol: 22 parts by mass
[0304] Irganox 1076: 100 mass ppm
[0305] [Sample 6]
[0306] (Preparation of Liquid 6)
[0307] In the preparation of the liquid material 5, a liquid material (coating material for an optical film) 6 was prepared in the same manner except that the resin was changed to cellulose acylate (acetyl substitution degree: 2.80).
[0308] [Sample 7]
[0309] (Preparation of Liquid Material 7)
[0310] In the preparation of the liquid material 5, a liquid material (coating material for an optical film) 7 was prepared in the same manner except that the resin was changed to DELPET 80N (polymethyl methacrylate, manufactured by Asahi Kasei Chemicals Co., Ltd.).
[0311] [Sample 8]
[0312] (Preparation of Liquid 8)
[0313] In the preparation of the liquid material 5, a liquid material (optical film coating material) 8 was prepared in the same manner as above except that the fluorescent labeling compound was changed to the following compound A (NIR dye) (100 mass ppm).
[0314]
[0315] [Sample 9]
[0316] (Preparation of Liquid Material 9)
[0317] In the preparation of liquid material 5, a liquid material (optical film coating material) 9 was prepared in the same manner except that the fluorescent labeling compound was changed to the following compound B (NUV dye) (100 mass ppm).
[0318]
[0319] [Sample 10]
[0320] (Preparation of Liquid Material 10)
[0321] A liquid material (coating material for an optical film) 10 was prepared with the same composition as that of the liquid material 5 .
[0322] [Sample 11]
[0323] (Preparation of Liquid Material 11)
[0324] In the preparation of the liquid material 5, a liquid material (optical film coating material) 11 was prepared in the same manner except that the amount of the fluorescent labeling compound added was 5000 mass ppm.
[0325] [Sample 12]
[0326] (Preparation of Liquid Material 12)
[0327] In the preparation of the liquid material 5, a liquid material (optical film coating material) 12 was prepared in the same manner except that the amount of the fluorescent labeling compound added was 10000 mass ppm.
[0328] [Samples 13 to 15 and 17]
[0329] (Preparation of Liquids 13 to 15 and 17)
[0330] Liquids (optical film coating materials) 13 to 15 and 17 were prepared with the same composition as that of the liquid 5.
[0331] [Sample 16]
[0332] (Preparation of Liquid Material 16)
[0333] A liquid material (optical film coating material) 16 was prepared with the same composition as that of the liquid material 9 .
[0334] [Samples 18 and 19]
[0335] (Preparation of Liquids 18 and 19)
[0336] Liquids (optical film coating materials) 18 and 19 were prepared with the same composition as that of liquid 8.
[0337] [Sample 20]
[0338] (Preparation of Liquid Material 20)
[0339] BEAMSET577 (manufactured by Arakawa Chemical Industries, Ltd.) (polyurethane resin) was used as an ultraviolet curable resin, and methyl ethyl ketone (MEK) was added as a solvent. In addition, 0.08% by mass of a fluorine-based surfactant (trade name: FTERGENT (registered trademark) 650A, manufactured by Neos Corporation) was added, and then 100 ppm by mass of Irganox 1076 as a fluorescent labeling compound was added, and the total solid content was prepared to be 40 parts by mass, thereby preparing a liquid (coating solution for forming a hard coat layer) 20.
[0340] [Sample 21]
[0341] (Preparation of Liquid Material 21)
[0342] After adding 80 parts by mass of a 5% aqueous solution of polyvinyl alcohol (PVA-117H, degree of polymerization 1700, degree of saponification 99.5 mol%, manufactured by KURARAY) as a resin to 10 parts by mass of a 3% aqueous solution of boric acid which is heated and stirred at 45°C, 1 part by mass of a 1% aqueous solution of a surfactant (RAPISOLA30, manufactured by NOF Corporation) is added, 9 parts by mass of pure water as a solvent is added, and then 100 ppm by mass of Irganox 1076 as a fluorescent marker is added to prepare a liquid (coating liquid for forming a low refractive index layer) 21.
[0343] [evaluate]
[0344] <Sensitivity of peak intensity shift>
[0345] For each of the liquid substances prepared above, the excitation wavelength showing the highest intensity fluorescence spectrum was selected from a group of fluorescence spectra previously measured using a spectrophotometer while changing the excitation wavelength by 5 nm in steps, as an excitation wavelength effective for measurement.
[0346] The spectrophotometer used was a fluorescence spectrophotometer F-7100 (manufactured by Hitachi High-Tech Science Co., Ltd.).
[0347] In liquids 1 to 3, 5 to 7, 11 and 12 using Irganox 1076 as a fluorescent labeling compound, 280 nm was selected as an excitation wavelength effective for measurement. In liquid 10 using Irganox 1076 as a fluorescent labeling compound and the inspection object being magnesium ions, 330 nm was selected as an excitation wavelength effective for measurement, in liquid 13 using benzene as the inspection object, 270 nm was selected as an excitation wavelength effective for measurement, in liquid 14 using acetone as the inspection object, 260 nm was selected as an excitation wavelength effective for measurement, in liquid 15 using strontium chloride as the inspection object, 250 nm was selected as an excitation wavelength effective for measurement, in liquid 17 using methanol as the inspection object, 290 nm was selected as an excitation wavelength effective for measurement, and in liquids 20 and 21 using sodium ions as the inspection object, 300 nm was selected as an excitation wavelength effective for measurement. In addition, when compound A was used and the liquid substance 8 was water as the inspection object, 680 nm was selected as the excitation wavelength effective for measurement, in the liquid substance 18 was formamide as the inspection object, 690 nm was selected as the wavelength effective for measurement, and in the liquid substance 19 was magnesium chloride as the inspection object, 700 nm was selected as the wavelength effective for measurement. In addition, when compound B was used and the liquid substance 9 was water as the inspection object, 330 nm was selected as the excitation wavelength effective for measurement, and in the liquid substance 16 was ethanol as the inspection object, 340 nm was selected as the wavelength effective for measurement.
[0348] Next, for each liquid, the inspection object shown in the following table is used. When the inspection object is water, water is added in a manner that the content of water becomes 0.1 mass % and 1.0 mass %. In addition, when the inspection object is magnesium ion or sodium ion, magnesium ion or sodium ion is added in a manner that the content of the magnesium ion or sodium ion becomes 0.01 mass % and 0.1 mass %. Here, in the case of magnesium ion, MgCl2 is added, and in the case of sodium ion, NaCl is added. In addition, when the inspection object is benzene, acetone or formamide, benzene, acetone or formamide is added in a manner that the content of the benzene, acetone or formamide becomes 0.1 mass % and 1.0 mass %. In addition, when the inspection object is strontium chloride, strontium chloride is added in a manner that the content of the strontium chloride becomes 0.01 mass % and 0.1 mass %. In addition, when the inspection object is ethanol or methanol, ethanol or methanol is added in a manner that the content of the ethanol or methanol becomes 1 mass % and 10 mass %.
[0349] Next, for each liquid substance to which the inspection object is added, the light of the above-mentioned effective excitation wavelength is irradiated and each fluorescence spectrum is measured, and the fluorescence wavelength and peak intensity of the peak are measured. Then, the change in fluorescence wavelength and the change in peak intensity (peak intensity deviation) caused by the change in the content of the inspection object are calculated, and the evaluation is performed according to the following criteria based on the obtained peak intensity deviation. A, AA, and AAA of the following criteria are set as levels with no practical problems.
[0350] (Benchmark)
[0351] AAA: The change in fluorescence wavelength exceeds 3.0%, and the change in peak intensity exceeds 5.0%.
[0352] AA: The change in fluorescence wavelength is more than 1.5% and less than 3.0%, and the change in peak intensity is more than 1.0% and less than 5.0%.
[0353] A: The change in fluorescence wavelength is more than 0.3% and less than 1.5%, and the change in peak intensity is more than 0.1% and less than 1.0%.
[0354] B: The change in fluorescence wavelength is 0.3% or less, and the change in peak intensity is 0.1% or less.
[0355] <Haze value>
[0356] The haze of the films obtained 1 hour after the production of the films using the liquids 1 to 14 was measured using a haze meter (NDH manufactured by Nippon Denshoku Industries Co., Ltd.), and the haze was evaluated based on the following criteria. A, AA, and AAA of the following criteria were rated as levels with no practical problems.
[0357] AAA: The haze is 0.1% or less.
[0358] AA: The haze is more than 0.1% and not more than 0.5%.
[0359] A: The haze is more than 0.5% and less than 1%.
[0360] B: The haze exceeds 1%.
[0361] In addition, the SP value and ΔSP of the solvent, resin, labeling compound and test object used in the preparation of each sample were calculated by the above-mentioned method and are shown in the following table.
[0362] [Table 1]
[0363]
[0364] *1: Dichloromethane *2: Dichloromethane / ethanol *3: AO agent (Irganox1076) *4: Present invention *5: Comparative example
[0365] [Table 2]
[0366]
[0367] *1: Dichloromethane / ethanol *2: AO agent (Irganox1076)
[0368] As shown in the above results, it is considered that by using the evaluation method of the liquid material of the present invention, the sensitivity of the peak intensity shift degree is excellent compared with the comparative example, and the quality variation of the film can be reduced.
[0369] Industrial Applicability
[0370] The present invention can be used for a method and apparatus for evaluating a liquid material, which can detect minute changes in the amount of water, impurities, etc. in the liquid material at any time without using a reactive fluorescent labeling agent.
[0371] Explanation of symbols
[0372] 1 Dissolving kettle
[0373] 3, 6, 12, 15 filters
[0374] 4.13 Storage kettle
[0375] 2, 5, 11, 14 Liquid delivery pump
[0376] 8, 16 catheter
[0377] 10 Additive feeding kettle
[0378] 20 Confluence pipe
[0379] 21 Mixer
[0380] 30 Pressure mold
[0381] 31. Metal support
[0382] 32 Basement membrane
[0383] 33 Peeling position
[0384] 34 Stretching device
[0385] 35 Drying device
[0386] 36 conveyor roller
[0387] 37 Winding device
[0388] 41 Feed kettle
[0389] 42 Storage kettle
[0390] 43 Pump
Claims
1. A method for evaluating a liquid substance, comprising at least a solvent, a resin and a non-reactive additive. The non-reactive additive is a fluorescent labeling compound, The liquid material evaluation method comprises: a fluorescence spectrum observation step of obtaining the fluorescence spectrum of the liquid substance at any excitation wavelength, and The spectrum analysis step is to obtain data related to the peak intensity shift degree based on the interaction between the fluorescent labeling compound in the liquid substance and the inspection object from the obtained fluorescence spectrum.
2. The method for evaluating a liquid substance according to claim 1, wherein: A difference ΔSP in solubility parameters between the fluorescent labeled compound and the inspection object in the liquid substance is in the range of 6-22.
3. The method for evaluating a liquid substance according to claim 1 or 2, wherein: The non-reactive additive is contained in the liquid in an amount within a range of 1 to 5000 ppm by mass.
4. The method for evaluating a liquid substance according to any one of claims 1 to 3, wherein: The spectral analysis step is performed online.
5. The method for evaluating a liquid substance according to any one of claims 1 to 4, wherein: The method further comprises a data processing step of calculating the content of the inspection object using a calibration curve based on the peak intensity included in the data related to the peak intensity shift degree.
6. A liquid material evaluation device, comprising at least a solvent, a resin and a non-reactive additive, The non-reactive additive is a fluorescent labeling compound, The liquid material evaluation device comprises: a fluorescence spectrum observation unit for obtaining a fluorescence spectrum of the liquid substance at any excitation wavelength, and The spectrum analysis unit acquires data related to the peak intensity shift degree based on the interaction between the fluorescent labeled compound in the liquid substance and the inspection object from the acquired fluorescence spectrum.
7. The liquid material evaluation device according to claim 6, wherein: The device further comprises a data processing unit for calculating the content of the inspection object using a calibration curve based on the peak intensity included in the data related to the peak intensity shift degree.
8. The liquid material evaluation device according to claim 6 or 7, wherein: The device includes an information display unit for displaying data related to the peak intensity shift degree.