Cured product and printed wiring board
By adjusting the content and water absorption of inorganic filler in the photosensitive resin composition and controlling the elastic modulus and water absorption of the cured product, the resolution and warping problems in the printed circuit board are solved, and high resolution and low warping are achieved. Printed circuit board manufacturing.
Patent Information
- Application Number
- CN202380031228.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-28
- Filing Date
- 2023-03-27
- Publication Date
- 2024-11-15
AI Technical Summary
In the manufacturing process of printed circuit boards, although using a photosensitive resin composition containing an inorganic filler can reduce the warpage of the substrate, the resolution is easily reduced, and the prior art is difficult to simultaneously increase the resolution and suppress warpage.
By adjusting the content and water absorption of the inorganic filler in the photosensitive resin composition, the elastic modulus of the cured product is within the range of 4 to 12 GPa, and the water absorption rate is controlled under a specific humidity environment to form a high resolution and low warping Cured substance.
The high resolution and low warpage of the substrate when installing electronic components are achieved, ensuring the installation quality and performance of the printed circuit board.
Smart Images

Figure BDA0005063934840000091 
Figure BDA0005063934840000101 
Figure BDA0005063934840000231
Abstract
Description
Technical Field
[0001] The present invention relates to a cured product, and more particularly to a cured product of a photosensitive resin composition that can be suitably used for an insulating layer such as a solder resist, and a printed wiring board using the cured product. Background Art
[0002] Generally, in a printed circuit board used in electronic equipment, when electronic components are mounted on the printed circuit board, a solder resist layer is formed on the substrate with a circuit pattern except for the area of the connection hole in order to prevent solder from adhering to the unnecessary part of the printed circuit board in the process such as reflow soldering. The solder resist layer is mainly formed by a so-called photosensitive solder resist, that is, a photosensitive resin composition is applied to the substrate, dried, and a pattern is formed by exposure and development, and then the resin with the pattern is mainly cured by heating or light irradiation. In addition, it has been proposed to use a photosensitive dry film to form a solder resist layer instead of using a liquid photosensitive resin composition as described above.
[0003] These photosensitive resin compositions or photosensitive dry films contain alkali-soluble photosensitive resin components to enable exposure and development, and contain other photopolymerizable monomers as needed, and contain thermosetting components such as epoxy resins in consideration of heat resistance and substrate adhesion, etc. In addition, in order to reduce the linear expansion coefficient and suppress the peeling of the solder resist layer or the warping of the substrate, an inorganic filler is sometimes added to the photosensitive resin composition (Patent Document 1, etc.).
[0004] On the other hand, as the amount of inorganic filler increases, a cured product with a low linear expansion coefficient can be obtained, but the resolution during exposure tends to decrease. Therefore, as a photosensitive resin composition containing an inorganic filler and having a high resolution, a specific photopolymerization initiator or a sensitizer is used in combination (Patent Document 2, etc.).
[0005] Prior art literature
[0006] Patent Literature
[0007] Patent Document 1: Japanese Patent Application Publication No. 2001-72834;
[0008] Patent document 2: International Publication No. 2015-16362 pamphlet. Summary of the invention
[0009] The printed wiring board manufactured as described above is placed in a low humidity environment by bag packaging or the like, and is taken out of the bag packaging and used at the stage of mounting electronic components. When a certain time passes from taking out the substrate from the bag packaging to mounting electronic components on the substrate, the substrate warps and poor mounting occurs. On the other hand, when a photosensitive resin composition having a large amount of inorganic filler as described above is used, although the substrate is not prone to warping when mounting electronic components, there is a tendency for the resolution to decrease.
[0010] Therefore, an object of the present invention is to provide a cured product of a photosensitive resin composition having high resolution and capable of suppressing warping of a substrate when mounting an electronic component.
[0011] The inventors of the present invention have studied the above-mentioned subject and found that, by setting the content of the inorganic filler contained in the photosensitive resin composition to be below a certain value and the water absorption rate of the cured product cured under the prescribed curing conditions to be below a certain value, it is possible to maintain excellent resolution and reduce warpage even when used as a printed circuit board. The present invention is completed based on this understanding. That is, the gist of the present invention is as follows.
[0012] [1] A cured product of a photosensitive resin composition comprising at least an alkali-soluble resin, a photopolymerization initiator, and an inorganic filler, characterized in that:
[0013] The inorganic filler is contained in a ratio of 85 mass % or less relative to the entire photosensitive resin composition,
[0014] The elastic modulus of the solidified material is 4 to 12 GPa,
[0015] The water absorption rate of the cured product after being placed in an environment of 25° C. and a relative humidity of 10% for 60 minutes is defined as A (%).
[0016] When the water absorption rate of the cured product after being left in an environment of 25° C. and a relative humidity of 60% for 60 minutes is defined as B (%),
[0017] A≤0.3%, and
[0018] BA≤0.3.
[0019] [2] The cured product according to [1], wherein the inorganic filler is contained in an amount of 45 to 65% by mass based on the entire photosensitive resin composition.
[0020] [3] The cured product according to [1], wherein the inorganic filler is surface-treated with a silane coupling agent.
[0021] [4] The cured product according to [1], wherein the photosensitive resin composition further contains a sensitizer in an amount of 0.01 to 10% by mass based on the entire photosensitive resin composition.
[0022] [5] The cured product according to [4], wherein the sensitizer is an anthraquinone-based sensitizer having an ester bond.
[0023] [6] A printed wiring board comprising: a substrate; and a cover film provided on the substrate and composed of the cured product according to any one of [1] to [5].
[0024] According to the present invention, by forming a cured product containing an inorganic filler in a ratio not exceeding a predetermined amount and having predetermined water absorption characteristics, a cured product of a photosensitive resin composition having high resolution and capable of suppressing warping of a substrate when mounting electronic components can be achieved even if the inorganic filler is contained. DETAILED DESCRIPTION
[0025] [cured material]
[0026] The present invention provides a cured product, which is a cured product of a photosensitive resin composition containing at least an alkali-soluble resin, a photopolymerization initiator and an inorganic filler, wherein the elastic modulus of the cured product is 4 to 12 GPa, and when the water absorption rate of the cured product after being placed in an environment at 25° C. and a relative humidity of 10% for 60 minutes is set as A (%), and the water absorption rate of the cured product after being placed in an environment at 25° C. and a relative humidity of 60% for 60 minutes is set as B (%),
[0027] A≤0.3, and
[0028] BA≤0.3.
[0029] By including an inorganic filler at a ratio of 85% by mass or less relative to the entire photosensitive resin composition and adjusting the composition or curing conditions of the photosensitive resin composition so that the water absorption of the cured product is within the above-mentioned specified range, the resolution can be high and the warping of the substrate when mounting electronic components can be suppressed. The reason is not clear but is presumed as follows.
[0030] The water absorption of the cured product when the photosensitive resin composition is cured depends on the components constituting the photosensitive resin composition, but is not only related to the water absorption of the component types, but also to the interaction of the components constituting the cured product, such as the degree of crosslinking. In the present invention, by making the elastic modulus of the cured product within the range of 4 to 12 GPa, the lower the water absorption of the cured product, the more the warping of the printed wiring board is suppressed, and the photosensitive resin composition with a lower water absorption when used as such a cured product can reduce the warping of the substrate when the photosensitive resin composition is applied to the substrate or the dried coating film (dry film) of the photosensitive resin composition is attached to the substrate. As a result, it is believed that the reduction in resolution caused by the influence of the warping of the substrate is suppressed. That is, it can be considered that by adjusting the composition and curing conditions of the photosensitive resin composition so that the elastic modulus of the cured product is within a specified range and the water absorption is below a certain value, the warping of the substrate before the curing of the photosensitive resin composition and the warping of the substrate after curing can be reduced at the same time.
[0031] From the viewpoint of resolution and suppression of substrate warpage, the elastic modulus of the cured product of the present invention is preferably in the range of 6 to 12 GPa, and more preferably in the range of 7 to 9 GPa. It should be noted that the elastic modulus of the cured product in the present invention refers to a value calculated from a stress-strain curve measured based on JIS K 7127. Specifically, a tensile test is performed on the cured product using a tensile testing machine at 25°C under a tensile speed of 1 mm / min. Based on the obtained stress-strain curve, the slope of the straight line calculated when the stress is 2N to 7N is used as the elastic modulus.
[0032] For the cured product of the present invention, from the viewpoint of resolution and suppression of substrate warping, the value of A is preferably 0.25% or less, and more preferably 0.2% or less. That is, the water absorption of the cured product in a dry state (relative humidity 10%) is preferably low. In addition, the value of BA is preferably 0.25% or less, and more preferably 0.2%. It should be noted that in the present invention, the water absorption of the cured product can be specifically measured as follows.
[0033] First, the photosensitive resin composition is coated on the entire surface of a copper-clad laminate (MCL-E-770G, manufactured by Showa Denko K.K., copper thickness 18 μm) with a thickness of 200 μm and a size of 100×100 mm as a support so that the film thickness after curing becomes 20 μm to form a dry coating film, and then the dry coating film is exposed, and then the coating film is heated to cure, and the cured coating film is peeled off from the support to obtain a cured product. The peeled cured product is distributed to a weighing dish, and the mass of the cured product when the cured product is placed in an environment of 100°C for 1 hour (absolutely dry state) is defined as W0. It should be noted that the amount of the sample distributed to the weighing dish can be about 10 to 50 mg.
[0034] Next, the mass of the cured product after being left in an environment of 25° C. and 10% relative humidity for 60 minutes was measured (the mass at this time was referred to as W). 10 ).
[0035] In addition, the mass of the cured product after being left in an environment of 25°C and 60% relative humidity for 60 minutes was measured (the mass at this time was referred to as W). 60 ).
[0036] The water absorption rates A and B of the cured product are defined as follows.
[0037] Water absorption rate A(%)=(W 10 -W0) / W0×100
[0038] Water absorption rate B (%) = (W 60 -W0) / W0×100
[0039] The measurement exemplified above shows the measurement sequence of the water absorption rate of the cured product when the cured product is formed from the photosensitive resin composition. Of course, the measurement can be performed in the same manner when a film of the cured product is provided on a support such as a copper-clad laminate in advance. For example, when a film of the cured product is provided on a support in advance, the surface of the cured product film is peeled off or scraped off and used as a sample, and W0, W1, W2, W3, W4, W5, W6, W7, W8, W9, W10, W11, W12, W13, W14, W15, W16, W17, W18, W20, W21, W22, W34, W19, W23, W24, W25, W26, W36, W40, W5 10 , W 60 The value of water absorption A and water absorption B can be measured.
[0040] The elastic modulus and water absorption of the cured product can be controlled by appropriately adjusting the constituent components of the photosensitive resin composition, the blending ratio of the respective components, the curing conditions, etc. Next, the respective components constituting the photosensitive resin composition of the present invention will be described.
[0041] <Alkali-soluble resin>
[0042] As long as the alkali-soluble resin is a resin soluble in alkali, known and commonly used resins can be used. Alkali-soluble resins can be used alone or in combination of two or more. As examples, water-soluble resins such as carboxyl-containing resins and phenolic hydroxyl-containing resins can be cited. Among them, based on excellent developability, carboxyl-containing resins or phenolic hydroxyl-containing resins are preferred, and carboxyl-containing resins are more preferred. The alkali-soluble resin contains a carboxyl group, so that it can have alkali developability. In addition, from the viewpoint of photosensitivity, it is preferred that the molecule has an ethylenically unsaturated double bond in addition to the carboxyl group, but it is also possible to use only a carboxyl-containing resin that does not have an ethylenically unsaturated double bond. When the carboxyl-containing resin does not have an ethylenically unsaturated double bond, it is necessary to use a photopolymerizable monomer in combination in order to make the composition photocurable. As an ethylenically unsaturated double bond, it is preferably derived from acrylic acid or methacrylic acid or their derivatives.
[0043] Specific examples of carboxyl group-containing resins include the following compounds (either oligomers or polymers). It should be noted that in the present specification, (meth)acrylate refers to a general term for acrylate, methacrylate and a mixture thereof, and the same applies to other similar expressions.
[0044] (1) Carboxyl group-containing resins obtained by copolymerization of an unsaturated carboxylic acid such as (meth)acrylic acid and a compound containing an unsaturated group such as styrene, α-methylstyrene, a lower alkyl (meth)acrylate, or isobutylene.
[0045] (2) Carboxyl-containing urethane resins produced by the addition polymerization of diisocyanates such as aliphatic diisocyanates, branched aliphatic diisocyanates, alicyclic diisocyanates, and aromatic diisocyanates with diol compounds containing carboxyl groups such as dimethylol propionic acid and dimethylol butyric acid, and diol compounds such as polycarbonate polyols, polyether polyols, polyester polyols, polyolefin polyols, acrylic polyols, bisphenol A-based alkylene oxide adduct diols, and compounds having phenolic hydroxyl groups and alcoholic hydroxyl groups.
[0046] (3) Partially anhydride-modified products of the reaction products of diisocyanate and difunctional epoxy resins such as bisphenol A epoxy resin, hydrogenated bisphenol A epoxy resin, bisphenol F epoxy resin, bisphenol S epoxy resin, biphenyl epoxy resin and monocarboxylic acid compounds having ethylenically unsaturated double bonds such as (meth)acrylic acid, carboxyl-containing diol compounds and carboxyl-containing photosensitive urethane resins produced by the addition polymerization reaction of diol compounds.
[0047] (4) A carboxyl group-containing photosensitive urethane resin having a terminal (meth)acryloylation by adding a compound having one hydroxyl group and one or more (meth)acryloyl groups in the molecule such as hydroxyalkyl (meth)acrylate during the resin synthesis of (2) or (3).
[0048] (5) In the synthesis of the resin of (2) or (3), a carboxyl group-containing photosensitive urethane resin having its terminal (meth)acryloylated is added with a compound having one isocyanate group and one or more (meth)acryloyl groups in the molecule, such as an equimolar reaction product of isophorone diisocyanate and pentaerythritol triacrylate.
[0049] (6) A carboxyl group-containing photosensitive resin obtained by reacting a bifunctional or higher polyfunctional (solid) epoxy resin with (meth)acrylic acid to add a dibasic acid anhydride to the hydroxyl group present in the side chain.
[0050] (7) A carboxyl group-containing photosensitive resin obtained by adding a dibasic acid anhydride to the hydroxyl groups generated by reacting a polyfunctional epoxy resin obtained by epoxidizing the hydroxyl groups of a bifunctional (solid) epoxy resin with epichlorohydrin and (meth)acrylic acid.
[0051] (8) A carboxyl-containing polyester resin obtained by adding a dibasic acid anhydride such as phthalic anhydride, tetrahydrophthalic anhydride or hexahydrophthalic anhydride to the primary hydroxyl group generated by reacting a bifunctional oxetane resin with a dicarboxylic acid such as adipic acid, phthalic acid or hexahydrophthalic acid.
[0052] (9) A carboxyl-containing photosensitive resin obtained by reacting an epoxy compound having a plurality of epoxy groups in one molecule with a compound having at least one alcoholic hydroxyl group and one phenolic hydroxyl group in one molecule such as p-hydroxyphenylethanol, or a monocarboxylic acid containing an unsaturated group such as (meth)acrylic acid, so that the alcoholic hydroxyl group of the resulting reaction product reacts with a polyacid anhydride such as maleic anhydride, tetrahydrophthalic anhydride, trimellitic anhydride, pyromellitic anhydride, adipic acid, or the like.
[0053] (10) A carboxyl group-containing photosensitive resin obtained by reacting a compound having a plurality of phenolic hydroxyl groups in one molecule with an alkylene oxide such as ethylene oxide or propylene oxide, and reacting the reaction product obtained by reacting the reaction product with a monocarboxylic acid containing an unsaturated group and further reacting the reaction product with a polyacid anhydride.
[0054] (11) A carboxyl group-containing photosensitive resin obtained by reacting a compound having a plurality of phenolic hydroxyl groups in one molecule with a cyclic carbonate compound such as ethylene carbonate or propylene carbonate, reacting the resulting reaction product with a monocarboxylic acid containing an unsaturated group, and then reacting the resulting reaction product with a polyacid anhydride.
[0055] (12) A carboxyl group-containing photosensitive resin obtained by further adding a compound having one epoxy group and one or more (meth)acryloyl groups in one molecule to the resins of (1) to (11).
[0056] The use of these carboxyl group-containing resins is not limited to the above-mentioned resins, and they may be used alone or in combination of plural types.
[0057] The acid value of the carboxyl-containing resin is preferably 40 to 150 mgKOH / g. When the acid value of the carboxyl-containing resin is 40 mgKOH / g or more, alkali development becomes good. In addition, by setting the acid value to 150 mgKOH / g or less, a good solder resist pattern can be easily drawn. More preferably, it is 50 to 130 mgKOH / g.
[0058] The weight average molecular weight of the carboxyl-containing resin varies depending on the resin skeleton, but is generally preferably 2000 to 150000. By setting the weight average molecular weight to 2000 or more, it is possible to improve the tackiness or resolution. In addition, by making the weight average molecular weight 150000 or less, it is possible to improve the developability and storage stability. It is more preferably 5000 to 15000. It should be noted that the weight average molecular weight can be measured by gel permeation chromatography (GPC).
[0059] In the photosensitive resin composition, the amount of carboxyl resin is preferably 10 to 50% by mass in terms of solid content. By setting the amount of carboxyl resin to 10% by mass or more, the coating strength can be improved. In addition, by setting the amount of carboxyl resin to 50% by mass or less, the viscosity becomes suitable and the printability is improved. More preferably, 10 to 30% by mass.
[0060] <Photopolymerization initiator>
[0061] The photosensitive resin composition according to the present invention contains a photopolymerization initiator for photopolymerization. As the photopolymerization initiator, a known material can be used, for example, α-aminoacetophenone-based photopolymerization initiators such as 2-methyl-1-[4-(methylthio)phenyl]-2-morpholino-1-propanone, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butane-1-one, 2-(dimethylamino)-2-[(4-methylphenyl)methyl]-1-[4-(4-morpholino)phenyl]-1-butanone, and N,N-dimethylaminoacetophenone; 1-hydroxy-cyclohexylphenyl ketone, 1-[4-(2-hydroxyethoxy)-phenyl]-2-hydroxy-2-methyl-1-propane-1-one, 2-hydroxy-1-{4-[4-(2-hydroxy-2-methyl bis-(2,6-dichlorobenzoyl)phenylphosphine oxide, bis-(2,6-dichlorobenzoyl)-2,5-dimethylphenylphosphine oxide, bis-(2,6-dichlorobenzoyl)-4-propylphenylphosphine oxide, bis-(2,6-dichlorobenzoyl)-1-naphthylphosphine oxide, bis-(2,6-dimethoxybenzoyl)phenylphosphine oxide, bis-(2,6-dimethoxybenzoyl)-2,4,4-trimethylpentylphosphine oxide, bis-(2,6-dimethoxybenzoyl)-2,5- Acylphosphine oxide-based photopolymerization initiators such as dimethylphenylphosphine oxide, bis-(2,4,6-trimethylbenzoyl)-phenylphosphine oxide, 2,6-dimethoxybenzoyldiphenylphosphine oxide, 2,6-dichlorobenzoyldiphenylphosphine oxide, 2,4,6-trimethylbenzoylphenyl methyl hypophosphite, 2-methylbenzoyldiphenylphosphine oxide, pivaloylphenyl isopropyl hypophosphite, 2,4,6-trimethylbenzoyldiphenylphosphine oxide; benzoin-based photopolymerization initiators such as benzoin, benzyl, benzoin methyl ether, benzoin ethyl ether, benzoin n-propyl ether, benzoin isopropyl ether, benzoin n-butyl ether; benzoin alkyl ether-based photopolymerization initiators; benzophenone, p-methylbenzophenone, rice Chloride, etc. Benzophenone-based photopolymerization initiators such as benzophenone, methyl benzophenone, 4,4'-dichlorobenzophenone, and 4,4'-bisdiethylaminobenzophenone; acetophenone-based photopolymerization initiators such as acetophenone, 2,2-dimethoxy-2-phenylacetophenone, 2,2-diethoxy-2-phenylacetophenone, 1,1-dichloroacetophenone, 1-hydroxycyclohexyl phenyl ketone, and 2-methyl-1-[4-(methylthio)phenyl]-2-morpholino-1-propanone; thioxanthone-based photopolymerization initiators such as thioxanthone, 2-ethylthioxanthone, 2-isopropylthioxanthone, 2,4-dimethylthioxanthone, 2,4-diethylthioxanthone, 2-chlorothioxanthone, and 2,4-diisopropylthioxanthone;Anthraquinone-based photopolymerization initiators such as anthraquinone, chloroanthraquinone, 2-methylanthraquinone, 2-ethylanthraquinone, 2-tert-butylanthraquinone, 1-chloroanthraquinone, 2-amylanthraquinone, and 2-aminoanthraquinone; ketal-based photopolymerization initiators such as acetophenone dimethyl ketal and benzyl dimethyl ketal; benzoate-based photopolymerization initiators such as ethyl 4-dimethylaminobenzoate, ethyl 2-(dimethylamino)benzoate, and ethyl p-dimethylbenzoate; 1,2-octanedione, 1-[4-(phenylthio)phenyl]-, 2-(O- Oxime ester photopolymerization initiators such as bis(η5-2,4-cyclopentadien-1-yl)-bis(2,6-difluoro-3-(1H-pyrrol-1-yl)phenyl)titanium and bis(cyclopentadienyl)-bis[2,6-difluoro-3-(2-(1-pyrrol-1-yl)ethyl)phenyl]titanium. These photopolymerization initiators may be used alone or in combination of two or more.
[0062] Examples of commercially available α-aminoacetophenone-based photopolymerization initiators include Omnirad 907, 369, 369E, and 379 manufactured by IGM Resins.
[0063] Examples of commercially available acylphosphine oxide-based photopolymerization initiators include Omnirad 819 manufactured by IGM Resins.
[0064] Examples of commercially available titanocene-based photopolymerization initiators include JMT-784 manufactured by Yueyang Kimoutain Sci-tech Co., Ltd. and GR-FMT manufactured by Hubei Gurun Technology Co., Ltd.
[0065] Furthermore, a photopolymerization initiator having two oxime ester groups in the molecule can also be used appropriately. Specifically, an oxime ester compound having a carbazole structure represented by the following general formula (I) can be mentioned.
[0066]
[0067] In the above formula, X represents a hydrogen atom, an alkyl group having 1 to 17 carbon atoms, an alkoxy group having 1 to 8 carbon atoms, a phenyl group, a phenyl group (substituted by an alkyl group having 1 to 17 carbon atoms, an alkoxy group having 1 to 8 carbon atoms, an amino group, an alkylamino group having an alkyl group having 1 to 8 carbon atoms, or a dialkylamino group), or a naphthyl group (substituted by an alkyl group having 1 to 17 carbon atoms, an alkoxy group having 1 to 8 carbon atoms, an amino group, an alkylamino group having an alkyl group having 1 to 8 carbon atoms, or a dialkylamino group), and Y and Z represent a hydrogen atom, an alkyl group having 1 to 17 carbon atoms, an alkoxy group having 1 to 8 carbon atoms, a halogen group, a phenyl group, a phenyl group (substituted by an alkyl group having 1 to 17 carbon atoms, an alkoxy group having 1 to 8 carbon atoms, a halogen group, wherein Ar represents an alkylene group having 1 to 10 carbon atoms, a vinylene group, a phenylene group, a biphenylene group, a pyridylene group, a naphthyl group, a thiophenylene group, an anthracene group, a thiophenylene group, a furylene group, a 2,5-pyrrole-diyl group, a 4,4'-stilbene-diyl group, a 4,2'-stilbene-diyl group, and n is an integer of 0 or 1.
[0068] In particular, preferred are oxime ester photopolymerization initiators in which, in the above formula, X1 and Y1 are each methyl or ethyl, Z is methyl or phenyl, n is 0, and Ar is phenylene, naphthylene, thienyl or thienylene.
[0069] The amount of the photopolymerization initiator in the photosensitive resin composition is preferably 1 to 50 parts by mass, more preferably 1 to 20 parts by mass, based on 100 parts by mass of the carboxyl group-containing resin, as calculated on a solid basis. This can improve the curability of the deep region.
[0070] <Sensitizer>
[0071] The photosensitive resin composition of the present invention preferably contains a sensitizer and is used in combination with the above-mentioned photopolymerization initiator. By using a sensitizer in combination, the water absorption of the cured product can be reduced without increasing the amount of the inorganic filler described below, and a cured product with good resolution can be obtained.
[0072] As the sensitizer, conventionally known materials can be used, such as benzoin compounds, anthraquinone compounds, thioxanthene compounds, ketal compounds, benzophenone compounds, tertiary amine compounds, and xanthone compounds, etc. Among them, thioxanthene compounds or anthraquinone compounds are preferably used from the viewpoint of deep region curability.
[0073] In addition, among the above-described sensitizers, compounds having functional groups such as an ester group and an amino group are considered to react with the above-described alkali-soluble resin or the photopolymerizable monomer described later, and a crosslinked structure is partially formed in the cured product of the photosensitive resin composition. As a result, the water absorption rate of the cured product can be further reduced.
[0074] As a sensitizer having such a functional group, for example, an anthraquinone-based sensitizer represented by the following formula can be cited.
[0075]
[0076] The above anthraquinone-based sensitizer can use commercially available materials. For example, anthracure UVS-581 (manufactured by Kawasaki Chemical Industry Co., Ltd.) can be cited.
[0077] The blending amount of the sensitizer is preferably 0.01 to 10% by mass, more preferably 0.01 to 3% by mass, based on the whole photosensitive resin composition. Thereby, excellent resolution is maintained and the water absorption of the cured product can be reduced.
[0078] <Inorganic filler>
[0079] The photosensitive resin composition according to the present invention contains an inorganic filler. By blending the inorganic filler, the water absorption rate of the cured product is reduced, and the required strength is imparted to the cured product, and the coefficient of thermal expansion can be reduced. As the inorganic filler, known materials can be used, and in particular, silica, talc, mica, alumina, calcium oxide, magnesium oxide, zinc oxide, calcium carbonate, magnesium carbonate, fly ash, dehydrated sludge, kaolin, clay, calcium hydroxide, aluminum hydroxide, magnesium hydroxide, hydrotalcite, aluminum silicate, magnesium silicate, calcium silicate, wollastonite, potassium titanate, magnesium sulfate, calcium sulfate, magnesium phosphate, sepiolite, vermiculite, boron nitride, aluminum borate, silica spheres, glass flakes, glass balloons, steelmaking slag, copper, iron, iron oxide, sendust, alnico magnets, various ferrite magnetic powders, cement, glass powder, Neuburg silica, diatomaceous earth, antimony trioxide, magnesium oxysulfate, hydrated aluminum, hydrated gypsum, alum, and barium sulfate, etc. These inorganic fillers can be used alone or in combination of two or more. Among them, silica is preferred.
[0080] From the viewpoints of dispersibility and the like, the average particle diameter (D50) of the inorganic filler is preferably 0.1 to 100 μm, more preferably 0.1 to 50 μm. It should be noted that the average particle diameter refers to the particle diameter at 50% of the cumulative volume obtained by the laser diffraction scattering type particle size distribution measurement method. In addition, the average particle diameter of the filler refers to the value measured for the filler as described above before preparing (pre-stirring, kneading) the photosensitive resin composition.
[0081] From the viewpoint of the elastic modulus of the cured product and the water absorption and resolution, the amount of inorganic filler in the photosensitive resin composition needs to be 85% by mass or less relative to the photosensitive resin composition as a whole. When it exceeds 85% by mass, the water absorption in the case of the cured product is reduced, and although the warping is suppressed, the resolution is insufficient. The amount of inorganic filler is preferably 45 to 85% by mass, and more preferably 45 to 65% by mass.
[0082] The filler may be a material that is surface treated in order to improve the dispersibility in the photosensitive resin composition. By using a surface-treated inorganic filler, the water absorption of the cured product can be further reduced, and as a result, the warping of the printed circuit board can be reduced. The surface treatment method is not particularly limited, and a known and conventional method can be used, but it is preferred to use a surface treatment agent having a curable reactive group, such as a coupling agent having a curable reactive group as an organic group to treat the surface of the inorganic filler.
[0083] As the curable reactive group, a photocurable reactive group or a thermosetting reactive group can be mentioned. As the photocurable reactive group, ethylenically unsaturated groups such as vinyl, styryl, methacryloyl, and acryloyl can be mentioned. Among them, at least any one of vinyl and (meth) acryloyl is preferred. As the thermosetting reactive group, a hydroxyl, carboxyl, isocyanate, amino, imino, epoxy, oxetanyl, mercapto, methoxymethyl, methoxyethyl, ethoxymethyl, ethoxyethyl, oxazoline, etc. can be mentioned. Among them, at least one of amino and epoxy is preferred. It should be noted that the surface-treated inorganic filler can also have a photocurable reactive group on the basis of the thermosetting reactive group.
[0084] As coupling agents, coupling agents of silane, titanate, aluminate and aluminozirconate can be used. Among them, silane coupling agents are preferred. As examples of silane coupling agents involved, vinyl trimethoxysilane, vinyl triethoxysilane, N-(2-aminomethyl)-3-aminopropyl methyl dimethoxy silane, N-(2-aminoethyl)-3-aminopropyl trimethoxy silane, 3-aminopropyl triethoxy silane, 3-anilinopropyl trimethoxy silane, 3-glycidoxypropyl trimethoxy silane, 3-glycidoxypropyl methyl dimethoxy silane, 2-(3,4-epoxycyclohexyl)ethyl trimethoxy silane, 3-methacryloxypropyl trimethoxy silane, 3-mercaptopropyl trimethoxy silane, etc. can be cited, which can be used alone or in combination. These silane coupling agents are preferably pre-adsorbed on the surface of the filler or fixed on the surface of the filler by reaction. Here, the treatment amount of the coupling agent is preferably 0.5 to 10 parts by mass based on 100 parts by mass of the spherical silica.
[0085] The surface-treated inorganic filler can be contained in the resin layer in the surface-treated state. The inorganic filler and the silane coupling agent can also be separately added to the photosensitive resin composition so that the inorganic filler is surface-treated in the composition, but it is preferred to add the inorganic filler that has been surface-treated in advance. By adding the inorganic filler that has been surface-treated in advance, it is possible to suppress the occurrence of cracks caused by the silane coupling agent that is not consumed in the surface treatment and that may remain in the case of separate additions. In the case of pre-surface treatment, it is preferred to add a pre-dispersion liquid in which the inorganic filler is pre-dispersed in an alkali-soluble resin or solvent, etc., and it is more preferred that the surface-treated inorganic filler is pre-dispersed in a solvent and the pre-dispersion liquid is added to the composition, or when the inorganic filler that has not been surface-treated is pre-dispersed in a solvent, the pre-dispersion liquid is added to the composition after the surface treatment is fully performed.
[0086] <Photopolymerizable monomer>
[0087] The photosensitive resin composition of the present invention may contain a photopolymerizable monomer. A photopolymerizable monomer is a monomer having an ethylenically unsaturated double bond. Examples of such photopolymerizable monomers include conventionally known polyester (meth)acrylates, polyether (meth)acrylates, urethane (meth)acrylates, carbonate (meth)acrylates, epoxy (meth)acrylates, and the like. Specifically, it can be appropriately selected from alkyl acrylates such as 2-ethylhexyl acrylate and cyclohexyl acrylate; hydroxyalkyl acrylates such as 2-hydroxyethyl acrylate and 2-hydroxypropyl acrylate; monoacrylates or diacrylates of alkylene oxide derivatives such as ethylene glycol, propylene glycol, diethylene glycol, and dipropylene glycol; acrylamides such as N,N-dimethylacrylamide, N-hydroxymethylacrylamide, and N,N-dimethylaminopropylacrylamide; aminoalkyl acrylates such as N,N-dimethylaminoethyl acrylate and N,N-dimethylaminopropyl acrylate; polyols such as hexylene glycol, trimethylolpropane, pentaerythritol, ditrimethylolpropane, dipentaerythritol, trihydroxyethyl isocyanurate, or these cycloalkyl acrylates. Polyacrylates such as oxirane adducts or ε-caprolactone adducts; polyacrylates such as phenols such as phenoxy acrylate and bisphenol A diacrylate or these oxirane adducts; at least one of the acrylates of glycidyl ethers such as glycerol diglycidyl ether, trimethylolpropane triglycidyl ether, and isocyanuric acid triglycidyl ether; not limited to the above materials, and can also be appropriately selected from polyols such as polyether polyols, polycarbonate diols, terminal hydroxyl polybutadiene, polyester polyols, etc., directly acrylated or urethane acrylated via diisocyanate, and melamine acrylates, and at least one of the methacrylates corresponding to the acrylates. This photopolymerizable monomer can also be used as a reactive diluent.
[0088] The photopolymerizable monomer can be used alone or in combination of two or more. The amount of the photopolymerizable monomer is preferably 0.5 to 30 parts by mass relative to 100 parts by mass of the carboxyl-containing resin, calculated on a solid basis. When the amount is 0.5 parts by mass or more, the photocurability is good, and a pattern is easily formed in the alkali development after the active energy ray irradiation. In addition, when the amount is 30 parts by mass or less, halo is not easily generated and good resolution can be obtained.
[0089] <Thermosetting ingredients>
[0090] The photosensitive resin composition of the present invention may contain a thermosetting component. Examples of the thermosetting component include isocyanate compounds, blocked isocyanate compounds, amino resins, maleimide compounds, benzoxazine resins, carbodiimide resins, cyclocarbonate compounds, epoxy compounds, oxetane compounds, episulfide resins, and other commonly known materials. Among them, the preferred thermosetting component is epoxy resin.
[0091] Examples of the epoxy resin include bisphenol A epoxy resin, bisphenol F epoxy resin, hydrogenated bisphenol A epoxy resin, brominated bisphenol A epoxy resin, bisphenol S epoxy resin, phenol novolac epoxy resin, cresol novolac epoxy resin, bisphenol A novolac epoxy resin, biphenyl epoxy resin, naphthalene epoxy resin, dicyclopentadiene epoxy resin, triphenylmethane epoxy resin, and the like. One of these may be used alone or two or more may be used in combination.
[0092] Examples of commercially available epoxy resins include jER 828, 806, 807, YX8000, YX8034, and 834 manufactured by Mitsubishi Chemical Corporation, YD-128, YDF-170, ZX-1059, and ST-3000 manufactured by Nippon Steel Chemical & Material Co., Ltd., EPICLON 830, 835, 840, 850, N-730A, and N-695 manufactured by DIC Corporation, and RE-306 manufactured by Nippon Kayaku Group.
[0093] The equivalent of the epoxy group of the epoxy resin in the photosensitive resin composition is preferably 0.5 to 2.5 in terms of solid content relative to 1 equivalent of the carboxyl group of the carboxyl group-containing resin. By making it 0.5 equivalents or more, it is possible to prevent the carboxyl group from remaining in the cured product, and good heat resistance or alkali resistance, electrical insulation, etc. can be obtained. In addition, by making the above-mentioned amount of 2.5 equivalents or less, it is possible to prevent low molecular weight cyclic (sulfide) ether groups from remaining in the dried coating film, and it is possible to ensure the strength of the cured product.
[0094] <Thermosetting catalyst>
[0095] The photosensitive resin composition of the present invention may contain a thermosetting catalyst for accelerating the curing of the thermosetting component. Examples of the thermosetting catalyst include imidazole derivatives such as imidazole, 2-methylimidazole, 2-ethylimidazole, 2-ethyl-4-methylimidazole, 2-phenylimidazole, 4-phenylimidazole, 1-cyanoethyl-2-phenylimidazole, and 1-(2-cyanoethyl)-2-ethyl-4-methylimidazole; amine compounds such as dicyandiamide, benzyldimethylamine, 4-(dimethylamino)-N,N-dimethylbenzylamine, 4-methoxy-N,N-dimethylbenzylamine, and 4-methyl-N,N-dimethylbenzylamine; hydrazide compounds such as adipic acid dihydrazide and sebacic acid dihydrazide; and phosphorus compounds such as triphenylphosphine. In addition, commercially available materials include, for example, 2MZ-A, 2MZ-OK, 2PHZ, 2P4BHZ, 2P4MHZ (all trade names of imidazole compounds) manufactured by Shikoku Kasei Kogyo Co., Ltd., U-CAT 3513N (trade name of dimethylamine compound) manufactured by San-Apro Co., Ltd., DBU, DBN, U-CAT SA 102 (all bicyclic amidine compounds and salts thereof), etc.
[0096] Not limited to the above-mentioned compound, as long as it is the heat curing catalyst of epoxy resin or oxetane compound or promotes the material of at least any 1 kind of reaction with carboxyl in epoxy group and oxetane group, can be used alone and can also mix 2 or more and use.In addition, can use guanamine, acetoguanamine, benzoguanamine, melamine, 2,4-diamino-6-methacryloyloxyethyl-S-triazine, 2-vinyl-2,4-diamino-S-triazine, 2-vinyl-4,6-diamino-S-triazine / isocyanuric acid adduct, 2,4-diamino-6-methacryloyloxyethyl-S-triazine / isocyanuric acid adduct S-triazine derivatives, preferably these also as the compound that close adhesion imparting agent plays a role and heat curing catalyst and use.
[0097] The heat curing catalyst can be used alone or in combination of two or more. From the viewpoint of the storage stability of the resin composition or the heat resistance of the cured film, the amount of the heat curing catalyst is preferably 0.01 to 30 parts by mass, more preferably 0.1 to 20 parts by mass, relative to 100 parts by mass of the carboxyl-containing resin, in terms of solid content.
[0098] <Other ingredients>
[0099] In addition to the above components, the photosensitive resin composition of the present invention may also be combined with colorants, elastomers, mercapto compounds, carbamate catalysts, thixotropic agents, adhesion promoters, block copolymers, chain transfer agents, polymerization inhibitors, copper corrosion inhibitors, antioxidants, rust inhibitors, organic bentonite, montmorillonite and other thickeners, silicon-based, fluorine-based, polymer-based defoamers and leveling agents, hypophosphites, phosphate derivatives, phosphorus compounds such as phosphazene compounds and other flame retardants and other components as needed. These can use materials known in the field of electronic materials.
[0100] From the viewpoint of ease of preparation or coating properties, an organic solvent may be added to the photosensitive resin composition of the present invention. As the organic solvent, ketones such as methyl ethyl ketone and cyclohexanone; aromatic hydrocarbons such as toluene, xylene, and tetramethylbenzene; glycol ethers such as cellosolve, methyl cellosolve, butyl cellosolve, carbitol, methyl carbitol, butyl carbitol, propylene glycol monomethyl ether, dipropylene glycol monomethyl ether, dipropylene glycol diethyl ether, diethylene glycol monomethyl ether acetate, and tripropylene glycol monomethyl ether; esters such as ethyl acetate, butyl acetate, butyl lactate, cellosolve acetate, butyl cellosolve acetate, carbitol acetate, butyl carbitol acetate, propylene glycol monomethyl ether acetate, dipropylene glycol monomethyl ether acetate, and propylene carbonate; aliphatic hydrocarbons such as octane and decane; petroleum-based solvents such as petroleum ether, naphtha, and solvent naphtha, and other well-known and commonly used organic solvents. These organic solvents may be used alone or in combination of two or more.
[0101] The amount of the organic solvent in the photosensitive resin composition can be appropriately changed depending on the material constituting the photosensitive resin composition, and can be, for example, 30 to 300 parts by mass based on solid content per 100 parts by mass of the (A) carboxyl group-containing resin.
[0102] The photosensitive resin composition of the present invention may be used in the form of a dry film or in the form of a liquid. When used in the form of a liquid, it may be one liquid or two liquids.
[0103] <Dry film>
[0104] The photosensitive resin composition may be in the form of a dry film including a first film and a resin layer formed on the first film and composed of the photosensitive resin composition. The cured product of the present invention is a cured product obtained by curing the photosensitive resin composition or the resin layer of the dry film.
[0105] The first film in the dry film of the present invention refers to a film that is at least bonded to the resin layer when the first film is laminated by heating or the like in such a manner that the resin layer side composed of the photosensitive resin composition formed on the dry film is in contact with the substrate such as a substrate and integrally formed. The first film can be peeled off from the resin layer in a process after lamination. In particular, in the present invention, it is preferably peeled off from the resin layer in a process after exposure.
[0106] When preparing a dry film, the photosensitive resin composition of the present invention is diluted with an organic solvent and adjusted to a suitable viscosity, and is applied to the first film with a comma coater, a knife coater, a lip coater, a rod coater, an extrusion coater, a reverse coater, a conveyor roll coater, a gravure coater, a spray coater, etc. in a uniform thickness, and is usually dried at a temperature of 50 to 130° C. for 1 to 30 minutes to obtain a film. The coating film thickness is not particularly limited, but is usually appropriately selected within the range of 1 to 150 μm, preferably 10 to 60 μm after drying.
[0107] As the first film, any known film can be used without particular limitation, and for example, films made of thermoplastic resins such as polyester films such as polyethylene terephthalate or polyethylene naphthalate, polyimide films, polyamide-imide films, polypropylene films, and polystyrene films can be preferably used. Among them, polyester films are preferred from the viewpoints of heat resistance, mechanical strength, and operability. In addition, a laminate of these films can also be used as the first film.
[0108] Furthermore, from the viewpoint of improving mechanical strength, the thermoplastic resin film as described above is preferably a film stretched in a uniaxial direction or a biaxial direction.
[0109] The thickness of the first film is not particularly limited, but can be, for example, 10 μm to 150 μm.
[0110] After forming the resin layer of the photosensitive resin composition of the present invention on the first film, it is preferred to further laminate a peelable second film on the surface of the resin layer in order to prevent dust from adhering to the surface of the resin layer. The second film in the dry film according to the present invention refers to a film that is peeled off from the resin layer before lamination when laminating and integrally molding by heating or the like in a manner that the resin layer side of the dry film is in contact with a base material such as a substrate.
[0111] As the second film that can be peeled off from the resin layer, for example, a polyethylene film, a polytetrafluoroethylene film, a polypropylene film, a surface-treated paper, etc. can be used. A film in which the bonding force between the resin layer and the second film is smaller than the bonding force between the resin layer and the first film when peeling off the second film can be used.
[0112] The thickness of the second film is not particularly limited, but may be, for example, 10 μm to 150 μm.
[0113] [Printed Circuit Board]
[0114] The printed wiring board of the present invention comprises a substrate and a cured coating film composed of a cured product disposed on the substrate. As described above, the cured product of the present invention can be obtained from a photosensitive resin composition or a resin layer of a dry film. As a method for manufacturing a printed wiring board of the present invention, for example, the photosensitive resin composition of the present invention is adjusted to a viscosity suitable for a coating method with the above-mentioned organic solvent, and after being coated on a substrate by a dip coating method, a flow coating method, a roller coating method, a rod coating method, a screen printing method, a curtain coating method, etc., the organic solvent contained in the composition is volatilized and dried (temporarily dried) at a temperature of 60 to 100° C., thereby forming a non-sticky (tackfree) resin layer. In addition, in the case of a dry film, after being bonded to the substrate by a laminator or the like so that the resin layer is in contact with the substrate, the first film is peeled off to form a resin layer on the substrate.
[0115] As the above-mentioned substrate, in addition to printed wiring boards and flexible printed wiring boards in which circuits are pre-formed using copper or the like, there can be cited copper-clad laminates for high-frequency circuits using materials such as paper phenol, paper epoxy resin, glass cloth epoxy resin, glass polyimide, glass cloth / non-woven epoxy resin, glass cloth / paper epoxy resin, synthetic fiber epoxy resin, fluororesin-polyethylene-polyphenylene ether, polyphenylene oxide-cyanate ester, and the like, as well as copper-clad laminates of all grades (FR-4, etc.), as well as metal substrates, polyimide films, polyethylene terephthalate films, polyethylene naphthalate (PEN) films, glass substrates, ceramic substrates, chip boards, and the like.
[0116] In the case of a dry film, lamination to a substrate is preferably performed under pressure and heating using a vacuum laminator or the like. By using such a vacuum laminator, when a substrate having a circuit is used, even if the circuit substrate surface has irregularities, since the dry film is in close contact with the circuit substrate, the filling property of the recessed portion on the substrate surface can be improved without mixing in bubbles because the dry film is in close contact with the circuit substrate. The pressurization condition is preferably about 0.1 to 2.0 MPa, and the heating condition is preferably 40 to 120°C.
[0117] When the photosensitive resin composition of the present invention contains an organic solvent, it is preferred to volatilize and dry the photosensitive resin composition after coating the surface of the substrate. The volatilization drying can be performed using a hot air circulation drying furnace, an IR furnace, a hot plate, a convection oven, etc. (a method in which a device having a heat source using a steam-based air heating method is used to make the hot air in the dryer contact with convection, and a method in which the hot air is sprayed onto the substrate through a nozzle).
[0118] After forming a resin layer on the substrate, it is selectively exposed with active energy rays through a photomask having a predetermined pattern, and the unexposed portion is developed with a dilute alkali aqueous solution (e.g., a 0.3-3% by mass sodium carbonate aqueous solution) to form a pattern of a cured product. In the case of a dry film, the first film is peeled off from the dry film after exposure and developed, thereby forming a patterned cured product on the substrate. It should be noted that, in the case of a dry film, the first film can be peeled off from the dry film before exposure, and the exposed resin layer can be exposed and developed as long as it does not damage the characteristics. In addition, after the active energy rays are irradiated to the cured product, it is heated and cured (e.g., 100-220°C), or after the heat curing, the active energy rays are irradiated, or only the heat curing is performed to complete the curing (main curing), so that a cured film with excellent characteristics such as adhesion and hardness can be formed.
[0119] When a cured product is prepared as described above, the elastic modulus of the cured product can be adjusted according to the curing conditions. The elastic modulus is a physical property value indicating the ease of deformation of the cured product. For example, according to the conditions of light curing and heat curing, the degree of cross-linking reaction of the reactive group changes, and the result also affects the elastic modulus of the cured product. That is, when the degree of cross-linking reaction is different, the strain of the cured product when stress is applied changes, so that the value of the elastic modulus is different.
[0120] As an exposure machine for the above-mentioned active energy ray irradiation, any device equipped with a high-pressure mercury lamp, an ultra-high-pressure mercury lamp, a metal halide lamp, a mercury arc lamp, etc. and irradiating ultraviolet rays in the range of 350 to 450 nm can be used. In addition, a direct drawing device (for example, a laser direct imaging device that directly draws an image with a laser using CAD data from a computer) can also be used. The lamp light source or laser light source of the direct drawing device can be a device with a maximum wavelength in the range of 350 to 450 nm. Although the exposure amount used to form an image varies depending on the film thickness, etc., it can usually be set to 10 to 1000 mJ / cm 2 , preferably 20 to 800 mJ / cm 2 within the range.
[0121] As the above-mentioned development method, an immersion method, a shower method, a spray method, a brush method, etc. can be used, and as the developer, an alkaline aqueous solution such as potassium hydroxide, sodium hydroxide, sodium carbonate, potassium carbonate, sodium phosphate, sodium silicate, ammonia, amines, etc. can be used.
[0122] After forming the cured film on the substrate as described above, components such as electronic components are mounted on the substrate by reflow treatment. The reflow treatment can be performed by a conventionally known method. In addition, the reflow treatment is usually performed under treatment conditions such as 245 to 260° C. and 5 to 10 seconds.
[0123] The photosensitive resin composition or dry film of the present invention can be suitably used in the manufacture of electronic components such as printed circuit boards, and is more suitable for forming a permanent coating. In this case, the photosensitive resin composition or dry film of the present invention is used to form a cured product by the above-mentioned method. When the resin layer of the photosensitive resin composition or dry film of the present invention is insulating, it is preferably used to form a solder resist, a cover layer or an interlayer insulating layer. It should be noted that the photosensitive resin composition according to the present invention can be used to form a solder dam.
[0124] Example
[0125] The present invention will be described in detail below with reference to Examples, but the present invention is not limited to these Examples. It should be noted that, unless otherwise specified, the following "parts" and "%" are based on mass.
[0126] <Synthesis Example 1 (Synthesis of Carboxyl Group-Containing Resin A)>
[0127] Into an autoclave equipped with a thermometer, a nitrogen introduction device, an alkylene oxide introduction device, and a stirring device, 119.4 parts by mass of a novolac type cresol resin (trade name "Shonol CRG 951", manufactured by Aica Kogyo Company, Limited, OH equivalent: 119.4), 1.19 parts by mass of potassium hydroxide, and 119.4 parts by mass of toluene were introduced, and the system was replaced with nitrogen while stirring, and the temperature was raised. Then, 63.8 parts by mass of propylene oxide was slowly added dropwise, and the mixture was heated at 125 to 132°C and 0 to 4.8 kg / cm 2 The reaction was carried out for 16 hours. Then, the mixture was cooled to room temperature, and 1.56 parts by mass of 89% phosphoric acid was added and mixed to the reaction solution, and potassium hydroxide was neutralized to obtain a propylene oxide reaction solution of a novolac type cresol resin [solid content: 62.1%; hydroxyl value: 182.2 mgKOH / g (307.9 g / eq.)]. In the propylene oxide reaction solution, an average of 1.08 mol of propylene oxide was added per equivalent of phenolic hydroxyl groups.
[0128] 293.0 parts by mass of the propylene oxide reaction solution of the obtained novolac type cresol resin, 43.2 parts by mass of acrylic acid, 11.53 parts by mass of methanesulfonic acid, 0.18 parts by mass of methylhydroquinone and 252.9 parts by mass of toluene were introduced into a reactor equipped with a stirrer, a thermometer and an air blowing tube, and air was blown in at a rate of 10 ml / min, and the mixture was reacted at 110°C for 12 hours while stirring. 12.6 parts by mass of water generated by the reaction was distilled off as an azeotropic mixture with toluene. Then, the mixture was cooled to room temperature, and the obtained reaction solution was neutralized with 35.35 parts by mass of a 15% sodium hydroxide aqueous solution, followed by water washing. Then, the toluene was replaced with 118.1 parts by mass of diethylene glycol monoethyl ether acetate in an evaporator while being distilled off to obtain a novolac type acrylate resin solution.
[0129] Next, 332.5 parts by mass of the obtained novolac type acrylate resin solution and 1.22 parts by mass of triphenylphosphine were introduced into a reactor equipped with a stirrer, a thermometer and an air blowing tube, and air was blown into the reactor at a rate of 10 ml / min. While stirring, 60.8 parts by mass of tetrahydrophthalic anhydride was slowly added thereto, and the mixture was reacted at 95 to 101° C. for 6 hours, and the mixture was cooled and taken out.
[0130] In this manner, a solution of carboxyl group-containing resin A (solid content: 65%; acid value of solid content: 87.7 mgKOH / g) was obtained.
[0131] <Preparation of inorganic filler>
[0132] The following two kinds of inorganic fillers were prepared.
[0133] 70 g of spherical silica (SFP-30M manufactured by Denka Company Limited, average particle size: 600 nm), 28 g of PMA (propylene glycol monomethyl ether acetate) as a solvent, and 2 g of a silane coupling agent having a methacryloyl group (KBM-503 manufactured by Shin-Etsu Chemical Co., Ltd.) were uniformly dispersed to obtain a surface-treated inorganic filler (solid content 70%).
[0134] 70 g of spherical silica (SFP-30M manufactured by Denka Co., Ltd., average particle size: 600 nm) and 28 g of PMA (propylene glycol monomethyl ether acetate) as a solvent were uniformly dispersed to obtain an inorganic filler (solid content 70%) that was not subjected to surface treatment.
[0135] <Preparation of photosensitive resin composition>
[0136] The components described in Table 1 below were blended and mixed at room temperature using a three-roll mill to obtain the photosensitive resin compositions described in the table (Examples 1 to 6 and Comparative Examples 1 and 2). In addition, the numerical values in the table represent parts by mass.
[0137] In addition, each component *1 to *7 in the following Table 1 is as follows.
[0138] *1: Acylphosphine oxide-based photopolymerization initiator (Omnirad 819 manufactured by IGM Resins).
[0139] *2: ANTHRACURE UVS-581 (manufactured by Kawasaki Kasei Chemicals Ltd.).
[0140] *3: KAYACURE DETX-S (Nippon Kayaku Co., Ltd.).
[0141] *4: Dipentaerythritol hexaacrylate (manufactured by Sanyo Chemical Industries, Ltd.).
[0142] *5: Novolac type epoxy resin (manufactured by DIC Corporation).
[0143] *6: Melamine (manufactured by Nissan Chemical Co., Ltd., D50 = 0.5 μm, solid content 55%).
[0144] *7: Dicyandiamide (manufactured by Mitsubishi Chemical Corporation, solid content 73%).
[0145] *8: A mixture of Phthalocyanine Blue and Pigment Yellow 147 (content ratio 57:43, solid content 10%).
[0146] In addition, the numerical value in a table|surface shows the compounding quantity in the solution containing a solid component and a solvent.
[0147] <Measurement of water absorption of cured products>
[0148] The photosensitive resin composition obtained as described above (Examples 1 to 6 and Comparative Examples 1 to 2) was applied to the entire surface of a copper-clad laminate (MCL-E-770G, manufactured by Showa Denko Co., Ltd., copper thickness 18 μm) having a thickness of 200 μm and a size of 100×100 mm as a support body so that the film thickness after curing was 20 μm. Next, it was dried in a hot air circulation drying oven (DF610 manufactured by Yamato Science Co., Ltd.) at 80° C. for 30 minutes to form a dry coating film, and then an ultraviolet transmission oven (UV Conveyor) equipped with a metal halide lamp (KUV-28351-XK-DM manufactured by Toshiba Corporation) was used as a light source, and the cumulative exposure amount under the wavelength condition of 365 nm was 1000 mJ / cm 2 (38mW·cm 2 The dried coating film was exposed under the conditions of 100 × 26 s), and then heated at a temperature of 150° C. for 60 minutes to cure the coating film, and then the cured coating film was peeled off from the support to obtain a cured product.
[0149] In addition, in the photosensitive resin composition of Example 1, the cumulative exposure amount was changed to 500 mJ / cm 2 (38mW·cm 2 × 13s), and except that the heating conditions were changed to 120°C and 60 minutes, a cured coating film was formed in the same manner as in Example 1 to obtain a cured product (Example 7).
[0150] 30 mg of the obtained solidified product was dispensed into a weighing dish, and the mass of each solidified product in a state where it was left to stand in an environment of 100° C. for 1 hour (absolutely dry state) was measured (the mass at this time was referred to as W0).
[0151] Next, the weight of each cured product after leaving it in an environment of 25° C. and a relative humidity of 10% for 60 minutes was measured (the weight at this time was referred to as W). 10 ).
[0152] In addition, the weight of each cured product after leaving it in an environment of 25° C. and 60% relative humidity for 60 minutes was measured (the weight at this time was referred to as W). 60 ).
[0153] Based on the obtained mass, water absorption A and B were calculated by the following formula.
[0154] Water absorption rate A(%)=(W 10 -W0) / W0×100
[0155] Water absorption rate B (%) = (W 60-W0) / W0×100
[0156] The difference (BA) between the water absorption rates A and B is shown in Table 1 below.
[0157] <Measurement of elastic modulus of cured product>
[0158] For each cured product obtained as described above, a test piece cut into a size of 10 mm × 80 mm was prepared, and a stress-strain curve was obtained using a tensile tester under the conditions of a distance between the clamps of 40 mm, a tensile speed of 1 mm / min, and 25° C. according to JIS K 7127. For the obtained curve, the slope of the straight line calculated when the stress was between 2N and 7N was used as the elastic modulus of the cured product. The elastic modulus of each cured product is shown in Table 1.
[0159] <Evaluation of Cured Product>
[0160] (1) Substrate warping
[0161] A substrate having a 20 μm thick cured film (cured product) formed on a copper-clad laminate in the same manner as above was placed in an environment of 25° C. and 60% relative humidity for 1 hour, and the warpage at the four corners of the substrate was measured with a vernier caliper and evaluated according to the following evaluation criteria.
[0162] ○: The average value of the four warped corners is less than 5.5 mm
[0163] △: The average value of the four corners of the warp is 5.5 mm or more and less than 7.5 mm
[0164] ×: The average value of the warped four corners is 7.5 mm or more
[0165] The evaluation results are shown in Table 1 below.
[0166] (2) Resolution (undercut)
[0167] The photosensitive resin compositions were applied to the entire surface of the copper-clad laminate in the same manner as described above so that the film thickness after curing was 20 μm, and then dried in a hot air circulation drying oven (DF610 manufactured by Yamato Scientific Co., Ltd.) at 80°C for 30 minutes to form a dry coating film, and a first film (Lumirror T60 manufactured by Toray Industries, Ltd., thickness 125 μm) was laminated on the dry coating film.
[0168] An exposure device equipped with a metal halide lamp (HMW-680-GW20 manufactured by Oak Manufacturing Co., Ltd.) was used as a light source, and the dried coating film was pattern-exposed at an optimal exposure amount through a negative mask of SRO 80 μm. Here, the optimal exposure amount means: using an exposure device equipped with a metal halide lamp, the dried coating film obtained above was exposed through a step sheet with a sensitivity of 21 levels, and a 0.2 mass % Na2CO3 aqueous solution at a liquid temperature of 30°C was used. When the pattern of the step sheet remaining during development is 6 levels under the condition of a spray pressure of 0.2 MPa for 60 seconds.
[0169] Next, the first film was peeled off, developed using a 0.2 mass % Na2CO3 aqueous solution at a liquid temperature of 30°C, and washed with water. Finally, the film was cured at 150°C for 60 minutes to prepare a test piece for resolution evaluation.
[0170] In the obtained test pieces, the resolution was evaluated according to the following criteria.
[0171] ○: The ratio of the opening diameter between the opening upper portion and the opening bottom portion is 0.85 or more.
[0172] △: The ratio of the opening diameter between the opening upper portion and the opening bottom portion is 0.70 or more and less than 0.85.
[0173] ╳: The ratio of the opening diameter between the top and bottom of the opening is less than 0.70.
[0174] The evaluation results are shown in Table 1 below.
[0175]
[0176] As can be seen from Table 1, for the photosensitive resin compositions (Examples 1 to 7) having an inorganic filler content of less than 85% by mass, an elastic modulus of the cured product in the range of 4 to 12 GPa, a water absorption A of less than 0.3% by mass, and a water absorption difference (BA) of less than 0.3% by mass, the resolution is high and the warping of the printed circuit board can be suppressed.
[0177] On the other hand, in the cured product (Comparative Example 1) composed of the photosensitive resin composition with an excessive content of inorganic filler, the water absorption A is less than 0.3 mass %, and the water absorption difference (BA) is less than 0.3 mass %, but the elastic modulus exceeds the range of 4 to 12 GPa, which can suppress the warping of the printed circuit board, but the resolution is insufficient. In addition, the cured product (Comparative Example 2) composed of the photosensitive resin composition in which the amount of inorganic filler is reduced in order to maintain the resolution has improved resolution, but the elastic modulus exceeds 12 GPa, and the water absorption difference (BA) also exceeds 0.3 mass %, and the warping of the substrate cannot be suppressed.
Claims
1. A cured product, which is a cured product of a photosensitive resin composition comprising at least an alkali-soluble resin, a photopolymerization initiator and an inorganic filler, characterized in that: The inorganic filler is contained in a ratio of 85 mass % or less relative to the entire photosensitive resin composition, The elastic modulus of the solidified material is 4 to 12 GPa, The water absorption rate of the cured product after the cured product was left to stand at 25° C. and a relative humidity of 10% for 60 minutes was defined as A (%). When the water absorption rate of the cured product after the cured product is left in an environment of 25° C. and a relative humidity of 60% for 60 minutes is defined as B (%), The solidified material satisfies A≤0.3%, and BA≤0.
3.
2. The cured product according to claim 1, wherein The inorganic filler is contained in an amount of 45 to 65% by mass based on the entire photosensitive resin composition.
3. The cured product according to claim 1, wherein The inorganic filler is surface treated with a silane coupling agent.
4. The cured product according to claim 1, wherein The photosensitive resin composition further includes a sensitizer in an amount of 0.01 to 10% by mass based on the entire photosensitive resin composition.
5. The cured product according to claim 4, wherein The sensitizer is an anthraquinone-based sensitizer having an ester bond.
6. A printed circuit board, wherein: have: substrate; and A coating film is provided on the substrate and is composed of the cured product according to any one of claims 1 to 5.