Image display device having camera on under image display panel
By setting the back panel of the anti-reflection layer and the low-reflection layer on the lower part of the display panel of the mobile terminal, the color spots and rainbow spots in the surrounding area are suppressed, and the problem of image quality degradation in the mobile terminal is solved, and high quality is achieved image display.
Patent Information
- Application Number
- CN202380028792.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-23
- Filing Date
- 2023-03-16
- Publication Date
- 2024-11-15
AI Technical Summary
When a selfie camera is installed on the lower part of the display panel of the mobile terminal, color spots or rainbow-like spots are likely to appear on the peripheral part, especially when shooting in wide-angle cameras and outdoor shooting, which affects the image quality.
An image display device is designed, in which the light receiving side of the camera module faces the image display panel, and a back panel with an anti-reflection layer or a low-reflection layer is provided on the panel, the reflectivity of the back panel is less than 2% and the haze is 5%. The following is an antistatic layer, the in-plane retardation of the substrate film is between 300 and 30,000 nm, the slow axis direction of the substrate film of the back plate is between 80 and 90 degrees and the long side direction of the display screen, and the NZ coefficient is between 1.2 and 4.0 Between these technical means, the transmittance difference of polarized light is suppressed and the occurrence of rainbow spots is reduced.
It effectively suppresses the color spots and rainbow spots in the surrounding area, ensuring high-quality image display, especially when shooting in wide-angle cameras and outdoor shooting, without widening the border, and increasing the image display area of the mobile terminal.
Smart Images

Figure CN118974801A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a camera-built-in image display device, and more particularly to an image display device having a camera built-in below an image display panel. Background Art
[0002] As the display screens of mobile terminals such as smart phones are gradually becoming larger, it is proposed to make the entire front of the terminal a display screen. In such a terminal where the entire front is a display screen, microphones, speakers, recognition sensors, selfie cameras (selfie cameras, in-cameras), etc. cannot be set in the conventional frame part, and therefore need to be set at the bottom of the image display panel, etc.
[0003] For mobile terminals, a selfie camera is indispensable for taking selfies, video calls, etc., and is sometimes also used as a facial recognition system. Therefore, the following solution has been proposed: in a terminal in which the entire front side serves as a display screen, a selfie camera is set at the bottom of the display panel, and pictures are taken through the gaps in the image display unit of the display panel, tiny holes set in the display panel, etc.
[0004] Prior art literature
[0005] Patent Literature
[0006] Patent Document 1: Japanese Patent Application Laid-Open No. 2022-41886 Summary of the invention
[0007] Problem that the invention aims to solve
[0008] However, it is known that in the image captured by the display panel, color spots or rainbow spots sometimes occur in the peripheral part. In particular, wide-angle cameras have appeared in recent years, and the quality has been gradually improved. However, the inventors have found that such peripheral spots sometimes occur more obviously in wide-angle cameras. In addition, spots are also likely to occur when taking pictures of yourself or your friends with beautiful scenery as the background at sunny tourist attractions. In this way, the inventors have regarded such rainbow spots as a major issue in the mobile terminal where the Selfie camera is set at the bottom of the panel, and solved it to achieve the present invention.
[0009] The present invention is used to solve the above-mentioned problems, and provides an image display device that can capture high-quality images with suppressed color spots and rainbow spots in the peripheral area even when the image is captured through a display panel. In particular, an image display device that can capture beautiful images even when shooting with a wide-angle camera or outdoors is provided.
[0010] Solutions for solving problems
[0011] [Item 1]
[0012] An image display device, wherein, in the image display device including a housing, an image display panel and a camera module,
[0013] The camera module is disposed in a space formed by the housing and the image display panel so that a light receiving side of the camera module faces the image display panel.
[0014] The image display panel has a back plate on the camera module side.
[0015] The back sheet has an anti-reflection layer or a low-reflection layer on the camera module side.
[0016] [Item 2]
[0017] The image display device according to item 1, wherein the backplane has a base film and an antireflection layer or a low-reflection layer, and the in-plane retardation of the base film is 300 to 30,000 nm.
[0018] [Item 3]
[0019] The image display device according to item 1 or 2, wherein the reflectance of the backplane measured from the anti-reflection layer or the low-reflection layer side is 2% or less.
[0020] [Item 4]
[0021] The image display device according to any one of items 1 to 3, wherein the haze of the back plate is 5% or less.
[0022] [Item 5]
[0023] The image display device according to any one of items 1 to 4, wherein the back plate has an antistatic layer.
[0024] [Item 6]
[0025] The image display device according to any one of items 2 to 5, wherein the angle formed by the slow axis direction of the substrate film of the backplane and the long side direction of the display screen of the image display device is 80 to 90 degrees on the acute angle side.
[0026] [Item 7]
[0027] The image display device according to any one of items 2 to 6, wherein the in-plane retardation of the substrate film of the backplane is 2500 to 30000 nm, and the ratio (Re / Rth) of the in-plane retardation to the retardation in the thickness direction (Rth) is 0.3 to 1.2.
[0028] [Item 8]
[0029] The image display device according to any one of items 2 to 7, wherein the in-plane retardation of the substrate film of the backplane is 2500 to 30000 nm, and the NZ coefficient is 1.2 to 4.0.
[0030] [Item 9]
[0031] The image display device according to any one of items 2 to 6, wherein the in-plane retardation of the substrate film of the backplane is 300 to 9000 nm, and the ratio (Re / Rth) of the in-plane retardation to the retardation in the thickness direction (Rth) is 0.5 or less.
[0032] [Item 10]
[0033] The image display device according to any one of items 2 to 6 or item 9, wherein the substrate film of the backplane has an in-plane retardation of 300 to 9000 nm and an NZ coefficient of 2.5 or more.
[0034] [Item 11]
[0035] The image display device according to any one of items 1 to 10, wherein a polarizing plate is provided at a position farther from the back plate when viewed from the camera module of the camera module.
[0036] Effects of the Invention
[0037] According to the present invention, even when a camera disposed at the bottom of the display panel is used, the image captured through the display panel can suppress the occurrence of color spots and rainbow spots in the peripheral portion, and high-quality natural color photography can be performed. In particular, even when a wide-angle camera is used or when shooting outdoors, beautiful images can be captured. In addition, there is no need to widen the frame portion in order to set up the camera, and a mobile terminal can be made that increases the area of the image display portion even if the size is small. BRIEF DESCRIPTION OF THE DRAWINGS
[0038] Figure 1 This is an example of the image display device of the present invention.
[0039] Figure 2 This is an example of a structure closer to the image display panel than the camera in the image display device of the present invention. DETAILED DESCRIPTION
[0040] The present invention relates to an image display device having the following structure: a camera module is arranged at the lower part of an image display panel, that is, the camera module is arranged on the opposite side of an image observer across the image display panel, and the camera module takes a picture through the image display panel. A schematic diagram of a mobile terminal, which is an example of the structure of such an image display device, is shown in Figure 1The camera module 2 is disposed in a space surrounded by the housing 3 and the image display panel 4, and is disposed so that the light receiving side of the camera module 2 faces the image display panel 4. Such a camera facing the same direction as the visual recognition side of the image display panel is called a selfie camera, a selfie camera, an in-camera, etc. In the present invention, when it is simply referred to as a camera, it means this selfie camera.
[0041] The light receiving side of the camera module 2 is provided with a lens, etc., which is a light collecting part side that absorbs external light for shooting. The camera module 2 may have a function of moving the lens for focusing and a zoom function for changing the focal length. In addition, the absorbed light is captured by a camera element such as a CCD or CMOS to form an electrical image signal.
[0042] The present invention can suitably cope with wide-angle shooting cameras with large viewing angles. The viewing angle is an angle used to represent the shooting range of a camera, and is usually represented by an angle in a diagonal direction. In the present invention, the viewing angle of the camera is preferably 65 degrees or more, more preferably 70 degrees or more, further preferably 73 degrees or more, particularly preferably 76 degrees or more, and most preferably 78 degrees or more. If further limited, it can be preferably 80 degrees or more, and the effect of the present invention can be exerted at a high level. It should be noted that even cameras with a viewing angle of less than 65 degrees are preferably used in the present invention without any hindrance.
[0043] The upper limit of the viewing angle of the camera is not particularly limited, but is preferably 130 degrees or less, more preferably 120 degrees or less, and further preferably 110 degrees or less. When the viewing angle exceeds the above, the amount of light in the peripheral portion may be reduced due to reflection at the panel, etc., resulting in a dark image in the peripheral portion.
[0044] A cover plate 5 may be provided on the viewer side of the image display panel 4. The cover plate 5 is made of, for example, glass or resin, and can prevent the image display panel 4 from being damaged when a strong impact is applied.
[0045] A surface protection film 6 may be provided on the outermost surface on the observer side of the image display device 1. The surface protection film 6 may be provided on the cover plate, or may be provided on the image display unit 4 without using the cover plate 5. The surface protection film 6 can mitigate impacts and prevent damage to the display screen. It can also be made in a way that the user of the image display device can replace it by himself when the surface of the surface protection film 6 is damaged. In order to be able to peel off the cover plate 5 and the surface protection film 6, it is preferably pasted with an adhesive. This structure is called an under-panel camera (UPC) or an under-display camera (UDC).
[0046] Figure 2Detailed Description of the Invention As a preferred example of the image display device of the present invention, an example of a structure closer to the organic EL display panel side than the camera in the organic EL image display device is shown.
[0047] The organic EL panel has an organic EL unit 420. The organic EL unit 420 has an EL layer 423 between a substrate 421 provided with an electrode 422. Glass, resin, etc. are used for the substrate 421. In order to protect the back surface and prevent scattering when the substrate 421 is glass, the organic EL unit 420 is bonded with a back plate 430. The back plate is preferably a transparent resin.
[0048] A circular polarization plate 440 may be provided on the observer side of the organic EL unit. The circular polarization plate 440 has a function of reducing reflection occurring between electrodes or layers and producing a high-contrast image.
[0049] The circular polarizing plate has a polarizer 441, a λ / 4 phase difference layer 442, and a polarizer protective film 443. Examples of the polarizer 441 include uniaxially stretched films obtained by adsorbing iodine and dichroic organic pigments on polyvinyl alcohol; and cured products of polymerizable liquid crystal compounds and organic dichroic pigments. Examples of the λ / 4 phase difference layer include oriented films of polycarbonate, polycyclic olefin, triacetyl cellulose, and the like, polymerizable liquid crystal compounds, and the like. The λ / 4 phase difference layer may be a composite layer of a λ / 4 phase difference layer and a λ / 2 phase difference layer, or a composite λ / 4 phase difference layer obtained by further adding a phase difference layer of a C plate. The backplane and the circular polarizing plate are preferably bonded to the organic EL unit and the backplane using an adhesive.
[0050] In the above-mentioned configuration, the camera module can take pictures through the pixel gap of the image display unit, the hole opened in the image display unit, etc. In addition, when taking pictures, only the part directly above the lens part of the camera module of the image display unit can be made transparent.
[0051] We studied the causes and solutions to these problems and found the following.
[0052] During imaging, light from the peripheral portion of the captured image obliquely crosses the image display panel, the surface protection film, and the like.
[0053] When light passes through an interface at an angle, polarized light is generated by reflection. The larger the angle, the greater the effect.
[0054] The larger the camera's shooting angle, the larger the angle of the tilted traverse, and the greater the polarization effect.
[0055] When a member having retardation exists in an image display panel, a surface protection film, or the like, polarized light becomes elliptically polarized light due to the influence of retardation.
[0056] The state of elliptically polarized light varies depending on the wavelength.
[0057] The elliptically polarized light further functions as a polarizer through the interface, and the transmittance differs depending on the wavelength according to the state of the elliptically polarized light.
[0058] When a polarizing plate is present on the image display panel side of the camera module, the amount of polarized light penetrating into the member having retardation and the difference in transmittance after being converted into elliptically polarized light become extremely large due to the strong polarization generating effect of the polarizing plate having a polarization rate of 98% or more.
[0059] Since retardation varies depending on the position, wavelengths with high or low transmittance vary depending on the position, causing rainbow spots and color spots in the peripheral area.
[0060] The imaging element separates colors using color filters and records images in the form of the intensity of each color. By increasing the delay, the repetition frequency of the wavelength and transmittance diagram caused by the delay is increased, thereby suppressing the variation of the light reception intensity of each color separated by the color filter caused by the delay.
[0061] In addition, the following reasons are presumed to be the cause of the apparent occurrence of rainbow spots in outdoor photography.
[0062] When shooting outdoors on a sunny day, the background scenery is also bright, and even slight spots are easily noticeable.
[0063] In particular, from the perspective of strength, oriented resin films are often used for backplanes, and from the perspective of price and quality stability, stretched polyester films are often used for backplanes. Stretched polyester films have a high refractive index and have large interface reflections between the camera module side and the air.
[0064] The high reflectivity is a major factor causing rainbow spots. By reducing the reflection, rainbow spots can be reduced.
[0065] As a specific countermeasure, in the image display device of the UPC structure as described above, the reflectivity of the backplane measured from the surface opposite to the unit is preferably set to 2% or less. The upper limit of the reflectivity is more preferably 1.5%, further preferably 1.2%, particularly preferably 1%, most preferably 0.9%, and further most preferably 0.8%. A low reflectivity is preferred, so the lower limit is not particularly limited, and the actual lower limit is 0.05%.
[0066] In order to set the reflectivity of the backplane to the above range, it is preferred to provide an anti-reflection layer or a low-reflection layer on the surface of the backplane, especially on the surface on the camera module side. In addition, it is preferred that an easy-adhesion layer is provided on at least the surface of the film used for the backplane on which the anti-reflection layer or the reflection-reducing layer is provided. The specific description of the anti-reflection layer and the reflection-reducing layer is provided together in the section of the high-Re film described later.
[0067] The preferred values of the total light transmittance and haze of the backplane are described below. It should be noted that, with respect to the reflectivity, total light transmittance, and haze of the backplane, only the portion directly above the camera, that is, the portion through which the light received by the camera passes, may be within the preferred range specified in the specification, and the other portions may be outside the range. For example, the portion other than the light receiving portion may be colored black, or may be matte finished. In addition, for example, when the backplane is coated black except for the light receiving portion, and the portion where the camera receives light is provided with a mesh or a plurality of small holes, the reflectivity, total light transmittance, and haze of the portion where the camera receives light may be within the specified preferred range.
[0068] [Thin films used in UPC type image display devices]
[0069] As described above, in the UPC type image display device of the present invention, a film can be used in various parts. The following is an explanation of the film used in the UPC type image display device. First, as the film used, a film having no in-plane phase difference or a film having an in-plane phase difference of less than 300nm (zero Re film) and an oriented film having an in-plane phase difference of more than 300nm can be listed.
[0070] Examples of the zero Re film include films claimed to have zero retardation, such as triacetyl cellulose (TAC), acrylic resin, and polycyclic olefin.
[0071] As oriented films, films obtained by stretching a resin having birefringence can be listed. The resin having birefringence is preferably polyester, polycarbonate, polystyrene, polyamide, polyimide, polyamideimide, polyphenylene sulfide, etc., more preferably polyester, and among polyesters, polyethylene terephthalate and polyethylene naphthalate are further preferred.
[0072] As a film used in the optical path of a camera, an oriented film is often used from the perspectives of economic efficiency, film production and quality stability, mechanical strength, and dimensional stability against temperature and humidity changes.
[0073] In most cases, the oriented film has a phase difference (delay) in the plane. Especially in the case of stretched polyester film, it is difficult to suppress the occurrence of delay. The upper limit of the delay of the oriented film can be less than 30000nm. If the more preferred upper limit of the delay is listed, it becomes 20000nm, 15000nm, 12000nm, 10000nm, 9000, 8500nm, 8000nm, 7500nm, 7200nm, 7000nm. By being set to the above or below, the thinning of the terminal can be achieved. In addition, by being set to the above or below, the necessary thickness in each application is ensured, and the excessive presentation of uniaxiality is prevented. Therefore, the film is not easy to break, and the film strength in each application can be ensured. The lower limit of the delay is preferably 300nm, more preferably 500nm, further preferably 800nm, and particularly preferably 1000nm. Especially in the case of stretched polyester film, by being set to the above or above, it is easy to ensure the thickness of various applications and achieve stable quality production.
[0074] The oriented film preferably has an in-plane retardation (Re) of 2500 to 30000 nm. Hereinafter, the film having an in-plane retardation (Re) of 2500 to 30000 nm may be referred to as a high Re film. By using a high Re film, rainbow spots caused by the oriented film can be suppressed.
[0075] In addition, in contrast to the high Re thin film, an oriented film having Re of 300 nm or more and less than 2500 is referred to as a medium Re thin film. Preferred properties of the high Re thin film and the medium Re thin film will be described together below.
[0076] The oriented film can be a biaxially stretched film. Specifically, in the case of a biaxially stretched film, the in-plane delay is preferably less than 9000nm, and more preferably less than 7000nm, less than 6000nm, less than 5000nm, less than 4500nm, and less than 4000nm in sequence. Even if it is a biaxially stretched film, by reducing the stretching ratio in the direction orthogonal to the main stretching direction, a film with a large in-plane delay can be made. If the stretching ratio becomes smaller, it becomes difficult to stretch uniformly. In order to ensure the uniformity of stretching, it is preferred that the stretching ratio in both directions is more than about 2.5 times, and more preferably more than about 3 times. From the viewpoint of being set to the appropriate in-plane delay in the appropriate thickness range in response to thinning in each application, the in-plane delay is preferably less than 5000nm, more preferably less than 4500nm, and more preferably less than 4000nm. The preferred lower limit during biaxial stretching film is as described above.
[0077] When the oriented film is made into a biaxially stretched film, the NZ coefficient is preferably 2.5 or more, more preferably 3.0 or more, further preferably 3.5 or more, particularly preferably 4.0 or more, and most preferably 4.5 or more. The upper limit of the NZ coefficient is infinite in theory, so it is not necessary to limit it, but as a range that can be actually controlled, it is preferably 100, and more preferably 70.
[0078] When the oriented film is made into a biaxially stretched film, Re / Rth is preferably 0.5 or less, more preferably 0.4 or less, further preferably 0.35 or less, particularly preferably 0.3 or less, and most preferably 0.25 or less. The lower limit of Re / Rth is theoretically zero, but as a range that can be actually controlled, it is preferably 0.005, and more preferably 0.01.
[0079] When the oriented film is made into a biaxially stretched film, the plane orientation degree is preferably 0.14 or more, more preferably 0.143 or more, further preferably 0.145 or more, particularly preferably 0.148 or more, and most preferably 0.15 or more. The upper limit of the plane orientation degree is preferably 0.25 or less, more preferably 0.2 or less, and further preferably 0.18 or less.
[0080] By setting the NZ coefficient, Re / Rth, and plane orientation degree within the above ranges, a stretching ratio that can easily ensure in-plane retardation and stretching uniformity in both directions can be adopted within an appropriate thickness range for thinning.
[0081] The slow axis direction of the oriented film is not particularly limited. From the perspective of productivity, it is preferably 0 degrees or 90 degrees to the long side direction of the screen. In addition, in order to further suppress rainbow spots, it is preferably 90 degrees. In addition, it can be 45 degrees. The reason is explained in the following high Re film.
[0082] It should be noted that the above angle allows a deviation of 25 degrees or less, preferably 20 degrees or less, and more preferably 15 degrees or less. When the oriented film is uniaxially stretched, it is preferably 10 degrees or less, more preferably 5 degrees or less, and especially 3 degrees or less.
[0083] (High retardation film)
[0084] The angle of the slow axis of the high Re film relative to the absorption axis of the polarizer is not limited, and is preferably any one of 0 degrees, 45 degrees, and 90 degrees. In addition, the angle of the slow axis of the high Re film relative to the long side of the screen is not limited, and is preferably any one of 0 degrees, 45 degrees, and 90 degrees. From the perspective of productivity, 0 degrees or 90 degrees is preferred.
[0085] Among them, it is preferable that the slow axis of the high Re film is 90 degrees with respect to the long side of the screen from the viewpoint of suppressing rainbow spots. This is considered to be mainly due to the following reasons.
[0086] Generally, a captured image is processed in a rectangular form similar to the screen shape, so the light reaching the ends in the long side direction has a larger angle with respect to the normal line of the high Re film than the light reaching the ends in the short side direction.
[0087] The difference in reflectivity between S-wave and P-wave at the interface increases as the angle from the normal increases. Therefore, if the film surface functions as a polarizer, rainbow spots are more likely to appear at the ends in the long-side direction.
[0088] The retardation in the tilted direction of the film increases as it gradually tilts from the normal line of the high Re film toward the fast axis direction, and decreases as it gradually tilts toward the slow axis direction. Therefore, if the slow axis of the high Re film is set to 90 degrees relative to the long side of the screen, the retardation reduction from the tilted direction will not occur at the end of the long side of the screen where rainbow spots are likely to appear as described above.
[0089] On the contrary, if the slow axis of the high Re film is set at 0 degrees with respect to the long side of the screen, the retardation from the oblique direction decreases at the end of the long side direction of the screen where rainbow spots are likely to appear as described above, so the front retardation needs to be further increased.
[0090] It should be noted that the above angle allows a deviation of less than 10 degrees, further allows a deviation of less than 5 degrees, and particularly allows a deviation of less than 3 degrees.
[0091] The lower limit of the NZ coefficient of the high Re film is preferably 1.2, more preferably 1.3, further preferably 1.4, particularly preferably 1.45, and most preferably 1.5. By setting it above or above, the mechanical strength required for various uses and production can be ensured. The upper limit of the NZ coefficient is preferably 4.0, more preferably 3.5, further preferably 3.0, particularly preferably 2.5, and most preferably 2.3. By setting it below the above, even if the high Re film is thinned, rainbow spots can be effectively suppressed during shooting.
[0092] The lower limit of Re / Rth of the high Re film is preferably 0.3, more preferably 0.4, further preferably 0.5, particularly preferably 0.6, and most preferably 0.7. By setting it to above or above, even if the high Re film is thinned, rainbow spots can be effectively suppressed during shooting. The upper limit of Re / Rth is preferably 1.20, more preferably 1.10, further preferably 1.00, particularly preferably 0.98, and most preferably 0.96. By setting it to below or above, mechanical strength can be maintained.
[0093] The lower limit of the plane orientation degree of the high Re film is preferably 0.08, more preferably 0.10, further preferably 0.11, and particularly preferably 0.113. By setting it above or above, the thickness unevenness can be reduced and the mechanical strength can be maintained. The upper limit of the plane orientation degree is preferably 0.148, more preferably 0.145, further preferably 0.142, particularly preferably 0.140, and most preferably 0.137. By setting it below the above, even if the high Re film is thinned, rainbow spots can be effectively suppressed during shooting.
[0094] The lower limit of the thickness of the high Re film is preferably 20 μm, more preferably 30 μm, more preferably 35 μm, further preferably 40 μm, particularly preferably 45 μm, and most preferably 45 μm. By setting it to above, a certain stiffness can be ensured during use, and the protective function when used for backplanes, protective films, etc. is ensured. The upper limit of the thickness is preferably 200 μm, and if more preferred upper limits are listed, they are 150 μm, 130 μm, 110 μm, 100 μm, 90 μm, 80 μm, and 70 μm. By setting it to below the above, the terminal can be thinned. It should be noted that the optimal range of thickness can be selected according to the purpose.
[0095] Furthermore, Re / Rth, NZ coefficient, and plane orientation degree can be adjusted within a thickness range suitable for the application in order to obtain appropriate in-plane retardation.
[0096] Furthermore, even if the retardation is the same, if the NZ coefficient becomes higher, rainbow spots tend to be more likely to occur. Therefore, it is preferable to satisfy the following relational expression 1.
[0097] Re(nm)≥NZ×1500(nm)+a(nm) (Formula 1)
[0098] Re: In-plane retardation of high Re film
[0099] NZ: NZ coefficient of high-Re film
[0100] Constant a: 500
[0101] In Formula 1, the constant a is more preferably 800, further preferably 1000, particularly preferably 1200, and most preferably 1500.
[0102] (Medium retardation film)
[0103] The upper limit of the in-plane retardation of the medium Re film is preferably 2400 nm, more preferably 2300 nm, further preferably 2200 nm, particularly preferably 2100 nm, and most preferably 2000 nm, and the lower limit is preferably 400 nm, further preferably 500 nm, and particularly preferably 600 nm.
[0104] The lower limit of the thickness of the medium Re thin film is preferably 5 μm, more preferably 10 μm, further preferably 15 μm, and particularly preferably 20 μm.
[0105] The upper limit of the thickness of the medium Re film is preferably 300 μm, more preferably 200 μm, further preferably 200 μm, particularly preferably 150 μm, and most preferably 130 μm.
[0106] The preferred ranges of the NZ coefficient, Re / Rth, and plane orientation degree of the medium Re film are the same as those of the biaxially stretched film.
[0107] The oriented film can be obtained by a general film production method. The following description is made by taking the case where the film is PET as an example. In the following description of the production method, the oriented film may be referred to as a polyester film.
[0108] The polyester film can be produced by a method in which a non-oriented polyester obtained by melting and extruding a polyester resin into a sheet is stretched in the longitudinal direction and the width direction at a temperature not lower than the glass transition temperature and subjected to a heat treatment.
[0109] The polyester film can be uniaxially stretched or biaxially stretched according to the optical properties as the target. In the case of a high Re film, it is preferably uniaxially stretched because it is easy to ensure the necessary Re within the appropriate thickness range consistent with the purpose, and it is easy to set the Re / Rth and NZ coefficients to the appropriate range. In addition, even if it is biaxially stretched, it is also preferred to reduce the stretching ratio of one to strengthen the orientation in one direction.
[0110] The main orientation axis of the polyester film can be the traveling direction of the film (sometimes also referred to as the longitudinal direction or MD direction), or it can be the direction orthogonal to the longitudinal direction (sometimes also referred to as the orthogonal direction, TD direction). In the case of MD stretching, roller stretching is preferred, and in the case of TD stretching, tenter stretching is preferred. In addition, a tenter can be used to perform MD stretching using a simultaneous biaxial stretching machine. From the perspectives of less damage to the film surface and productivity, the preferred method is tenter-based stretching.
[0111] During stretching, the unstretched polyester film is preheated and stretched preferably at 80 to 130° C., more preferably 90 to 120° C. The stretch ratio in the main stretching direction is preferably 3.0 to 7.0 times, more preferably 3.3 to 6.5 times, and further preferably 3.5 to 6.2 times.
[0112] In order to further improve the uniaxiality, it is also preferred to shrink in a direction perpendicular to the stretching direction during stretching. In the case of TD stretching using a tenter, shrinking can be performed by, for example, narrowing the tenter clip interval. The shrinkage treatment is preferably 1 to 20%, more preferably 2 to 15%.
[0113] If biaxial stretching is performed, stretching is also performed in a direction orthogonal to the main stretching direction. In the case of making a high Re film, the stretching ratio is less than the ratio of the main stretching direction, preferably less than 3.0 times, more preferably less than 2.5 times, further preferably less than 2.0 times, particularly preferably less than 1.7 times, and most preferably less than 1.5 times. In addition, in order to reduce stretching unevenness at a low ratio, it is preferably less than 1.3 times, more preferably less than 1.2 times, further preferably less than 1.15 times, and particularly preferably less than 1.13. The lower limit of the stretching ratio in the orthogonal direction is preferably 1.01 times, and further 1.03 times, especially 1.05 times.
[0114] The stretching in the orthogonal direction of the medium Re film can also be adjusted within the above-mentioned range of the ratio in the main stretching direction.
[0115] It is preferred that heat setting be performed after stretching. The heat setting temperature is preferably 150 to 240°C, more preferably 170 to 230°C.
[0116] During the heat fixation, it is also preferred to perform a relaxation treatment along the main stretching direction or in a direction perpendicular thereto. The relaxation treatment is preferably 0.5 to 10%, more preferably 1 to 5%.
[0117] In order to reduce the deviation in the slow axis direction of the film, it is preferable to adjust the stretching speed and temperature so as to reduce the bending phenomenon in the stretching and heat setting steps, and to adjust the air volume so as to make the film temperature in the TD direction uniform.
[0118] Regarding the oriented film, in order to ensure the slipperiness of the film, a lubricant is preferably included in the film. However, if the amount of lubricant added is too much, the haze sometimes deteriorates. The lower limit of the amount of lubricant added is preferably 0.01% by mass, more preferably 0.05% by mass, and further preferably 0.10% by mass relative to the resin of the film. The upper limit of the amount of lubricant added is preferably 2% by mass, more preferably 1.5% by mass, and further preferably 1.0% by mass.
[0119] In addition, it is also preferred that the film material does not contain a lubricant and the lubricant is added only to the easy-adhesion layer described later, or that the film material is co-extruded into a multilayer structure and the lubricant is added only to the surface layer. The preferred amount of lubricant added only to the surface layer is also as described above.
[0120] Examples of the lubricant particles include inorganic particles such as calcium carbonate, calcium sulfate, silica, alumina, and calcium phosphate; and organic polymer particles such as styrene-based, acrylic-based, melamine-based, benzoguanamine-based, and silicone-based particles.
[0121] The average particle size of the particles is preferably 0.05 μm, more preferably 0.1 μm, and further preferably 0.2 μm in terms of the value based on the Coulter counter method. The upper limit of the average particle size of the particles is preferably 5.0 μm, more preferably 3.0 μm, further preferably 2.0 μm, and particularly preferably 1.5 μm or less.
[0122] The oriented film may contain an antioxidant, an anti-thermal degradation agent, a colorant, and the like.
[0123] [Thin film properties]
[0124] The following description of the film is not limited to the high retardation film and the medium retardation film unless otherwise specified herein, and can be applied to the film used in the image display device of the present invention.
[0125] The lower limit of the total light transmittance of the film is preferably 85%, more preferably 87%, further preferably 90%, and particularly preferably 91%. By setting it to above, a clear photographic image can be obtained. In addition, as a laminated body provided with a hard coat layer and an anti-reflection coating, preferred transparency can be ensured. The upper limit of the total light transmittance is preferably 100%, more preferably 99.5%.
[0126] The upper limit of the haze of the film is preferably 5%, more preferably 3%, further preferably 2%, particularly preferably 1.5%, and most preferably 1.2%. By setting it below the above, a high-contrast, clear photographic image can be obtained. The lower limit of the haze is preferably 0.01%, and more preferably 0.1%.
[0127] 〔Easy bonding treatment〕
[0128] The film may be subjected to treatment such as corona treatment, flame treatment, plasma treatment, etc. for improving adhesion.
[0129] (Easy Adhesion Layer)
[0130] The film may be provided with an easy-adhesion layer. The easy-adhesion layer can improve the adhesion with the functional layer described later, the adhesion with the adhesive when attached to the surface of the display device, etc., and can prevent the surface protection film itself and the functional layer from peeling off during long-term use. It should be noted that when referred to as a film in the present invention, the easy-adhesion layer is sometimes included, and when the easy-adhesion layer is not included, it is sometimes referred to as a film raw material.
[0131] The resin used in the easy bonding layer can use polyester resin, polyurethane resin, polycarbonate resin, acrylic resin, etc., preferably polyester resin, polyester polyurethane resin, polycarbonate polyurethane resin, acrylic resin. The easy bonding layer is preferably cross-linked. As a cross-linking agent, isocyanate compounds, melamine compounds, epoxy resins, oxazoline compounds, etc. can be listed.
[0132] The easy-adhesion layer can be provided by preparing a coating material to which these resins and, if necessary, a crosslinking agent, particles, etc. are added, applying the coating material to the surface protection film, and drying the coating material. Examples of the particles include those used for the above-mentioned substrates.
[0133] The lower limit of the thickness of the easy-adhesion layer is preferably 10 nm, more preferably 15 nm, and further preferably 20 nm. The upper limit of the thickness is preferably 500 nm, more preferably 300 nm, further preferably 200 nm, and particularly preferably 150 nm. It should be noted that the easy-adhesion layer can be managed by the coating amount.
[0134] When film has easy bonding layer, sometimes the reflected light caused by the interface of easy bonding layer and film original material and the reflected light of the interface (with the interface of functional layer, adhesive layer, adhesive layer) of the easy bonding layer on the opposite side of the film original material interfere, and the part with the uneven thickness of easy bonding layer produces interference color. This interference color is obvious when black display part, power off. In order to suppress this interference color, preferably reduce interference.
[0135] In order to reduce interference, it is preferred that the refractive index of the easy-adhesion layer be close to the refractive index of the film material. When the film material is a high-Re film, the refractive index of the film material in the fast axis direction is set to nf, and the refractive index in the slow axis direction is set to nl, and the refractive index n of the easy-adhesion layer is preferably nf-0.05≤n≤nl+0.05, more preferably nf-0.02≤n≤nl+0.02, and further preferably nf≤n≤nl.
[0136] For example, when the film material is polyethylene terephthalate, the refractive index in the fast axis direction is 1.6, and the refractive index in the slow axis direction is about 1.7, so the lower limit of the refractive index of the easy-adhesion layer is preferably 1.55, more preferably 1.57, more preferably 1.58, further preferably 1.59, and particularly preferably 1.60. The upper limit of the refractive index of the easy-adhesion layer is preferably 1.75, more preferably 1.73, more preferably 1.72, further preferably 1.71, and particularly preferably 1.70.
[0137] In the case of re-stretching after coating by online coating, the refractive index of easy bonding layer sometimes has birefringence. In this case, the refractive index of the above-mentioned easy bonding layer is the average refractive index of the fast axis direction and the slow axis direction. The refractive index of easy bonding layer can be measured by, for example, applying the coating liquid of easy bonding layer on a glass plate, drying it, and utilizing an ellipsometer, etc.
[0138] In order to set the refractive index in the above-mentioned range, a method of adjusting the refractive index of the resin used for the easily adhesive layer or a method of adding particles with a high refractive index is preferred.
[0139] If it is a resin, the refractive index can be increased by using aromatic components. Therefore, it is preferred to use a resin having a benzene ring or a naphthalene ring in the main chain or the side chain, and it is particularly preferred to use a resin having a naphthalene ring. Specifically, it is preferably a polyester copolymerized with naphthalene dicarboxylic acid. The polyester copolymerized with naphthalene dicarboxylic acid can be blended with other resins as needed as a polyester resin. In addition, it can also be used as a polyester polyol of polyester polyurethane. When the total acid component is set to 100 mol%, the naphthalene dicarboxylic acid component in the polyester is preferably 30 to 90 mol%, and more preferably 40 to 80 mol%.
[0140] The lower limit of the refractive index of the high refractive index particles is preferably 1.7, and more preferably 1.75. The upper limit of the refractive index of the high refractive index particles is preferably 3.0, more preferably 2.7, and further preferably 2.5.
[0141] As high refractive index particles, particles of metal oxides with high refractive index are preferably included. As such metal oxides, TiO2 (refractive index is 2.7), ZnO (refractive index is 2.0), Sb2O3 (refractive index is 1.9), SnO2 (refractive index is 2.1), ZrO2 (refractive index is 2.4), Nb2O5 (refractive index is 2.3), CeO2 (refractive index is 2.2), Ta2O5 (refractive index is 2.1), Y2O3 (refractive index is 1.8), La2O3 (refractive index is 1.9), In2O3 (refractive index is 2.0), Cr2O3 (refractive index is 2.5), etc., and composite oxides containing these metal atoms can be listed. Among them, SnO2 particles, TiO2 particles, ZrO2 particles, and TiO2-ZrO2 composite particles are preferred.
[0142] The lower limit of the average particle size of the high refractive index particles is preferably 5 nm, more preferably 10 nm, further preferably 15 nm, and particularly preferably 20 nm. By setting the above, the particles are less likely to aggregate.
[0143] The upper limit of the average particle size of the high refractive index particles is preferably 200 nm, more preferably 150 nm, further preferably 100 nm, and particularly preferably 60 nm. By setting as above, transparency becomes good.
[0144] The lower limit of the content of the high refractive index particles in the easy bonding layer is preferably 2% by mass, more preferably 3% by mass or more, further preferably 4% by mass or more, and particularly preferably 5% by mass or more. By setting as above, it is possible to ensure that the refractive index of the coating layer is high and low interference can be effectively obtained.
[0145] The upper limit of the content of the high refractive index particles in the easy-adhesion layer is preferably 50% by mass, more preferably 40% by mass or less, further preferably 30% by mass or less, and particularly preferably 20% by mass or less. By setting as above, film forming properties become good.
[0146] The easy-adhesion layer may contain lubricant particles in addition to the high-refractive index particles. Examples of the lubricant particles include the particles listed as lubricant particles that can be added to the film.
[0147] The easy-adhesive layer can be provided on the stretched film in an offline manner, but is preferably provided in an online manner in the film-making process. In the case of providing it online, it can be any one of before longitudinal stretching and before transverse stretching, preferably applied before transverse stretching, and dried and cross-linked in the preheating, heating, and heat treatment process based on the tenter. It should be noted that in the case of online coating before longitudinal stretching using a roller, it is preferably introduced into the stretching roller after being dried using a vertical dryer after coating.
[0148] The easy-adhesion layer is provided on at least one surface, and preferably on both surfaces.
[0149] 〔Functional layer〕
[0150] It is also a preferred method to provide a functional layer such as a hard coating, an anti-reflection layer, a low-reflection layer, an anti-glare layer, an antistatic layer, and a refractive index adjustment layer on at least one surface of the film. The anti-reflection layer, the low-reflection layer, and the anti-glare layer are collectively referred to as a reflection reduction layer. The reflection reduction layer can suppress the reflection of the interface, thereby reducing the rainbow spot, or make the total light transmittance higher than the total light transmittance of the film alone, so as to achieve a brighter and clearer captured image. When the film is used as a transparent electrode substrate for a touch panel, a refractive index adjustment layer is provided, so that the phenomenon of seeing the electrode can be suppressed. It should be noted that sometimes a film with a functional layer is referred to as a film laminate or a high-Re film laminate together with the functional layer.
[0151] Among these, when the film is used for a backplane, or for the outermost surface of a display screen such as a cover plate or a surface protection film, it is preferred that a reflection reducing layer be provided on the surface of the film on the opposite side of the image display unit. In particular, in order to achieve a clear captured image, an anti-reflection layer or a low-reflection layer called Clear AR (Clear AR) or Clear LR (Clear LR) which does not have an anti-glare function based on diffuse reflection is preferred.
[0152] The upper limit of the arithmetic mean roughness (Sa) of the surface of the antireflection layer and the low reflection layer is preferably 10 nm, more preferably 5 nm, further preferably 5 nm, particularly preferably 4 nm, and most preferably 2 nm. The lower limit is 0.1 nm.
[0153] (Hard Coating)
[0154] By providing a hard coating layer on the film, when the film is used as a backplane, damage caused by contact between an image display panel and a camera module, etc. can be reduced, and when used as a cover plate or a surface protection film, damage during use can be reduced. In addition, providing a hard coating layer as the lower layer of the reflection reduction layer is also a preferred form.
[0155] The pencil hardness of the hard coat layer is preferably H or higher, more preferably 2 H or higher. The hard coat layer can be provided by, for example, applying a composition solution of a thermosetting resin or a radiation-curable resin and curing the solution.
[0156] Examples of the thermosetting resin include acrylic resins, urethane resins, phenolic resins, urea-melamine resins, epoxy resins, unsaturated polyester resins, silicone resins, and combinations thereof. In addition to these curable resins, a curing agent is added to the thermosetting resin composition as needed.
[0157] The radiation curable resin is preferably a compound having a radiation curable functional group, and as the radiation curable functional group, ethylenically unsaturated bond groups such as (meth) acryloyl, vinyl, and allyl, epoxy, and oxetanyl groups can be listed. Among them, as the ionizing radiation curable compound, it is preferably a compound having an ethylenically unsaturated bond group, and more preferably a compound having two or more ethylenically unsaturated bond groups, and more preferably a multifunctional (meth) acrylate compound having two or more ethylenically unsaturated bond groups. As the multifunctional (meth) acrylate compound, it can be a monomer, an oligomer, or a polymer.
[0158] As specific examples thereof, those listed as the above-mentioned binder resins can be used.
[0159] In order to achieve the hardness of the hard coating layer, the monomers having two or more functions in the compound having radiation curable functional groups are preferably 50% by mass or more, and more preferably 70% by mass or more. Furthermore, the monomers having three or more functions in the compound having radiation curable functional groups are preferably 50% by mass or more, and more preferably 70% by mass or more.
[0160] The above-mentioned compound having a radiation-curable functional group may be used alone or in combination of two or more.
[0161] The refractive index of the hard coat layer is preferably 1.45 or more, more preferably 1.50 or more. The refractive index of the hard coat layer is preferably 1.70 or less, more preferably 1.60 or less.
[0162] It should be noted that the refractive index of the hard coat layer is a value measured under the condition of a wavelength of 589 nm.
[0163] Furthermore, the refractive index of the hard coat layer can be further reduced so as to also serve as a low refractive index layer described below.
[0164] In order to adjust the refractive index of the hard coat layer, there are mentioned a method of adjusting the refractive index of the resin and a method of adjusting the refractive index of the particles when adding the particles.
[0165] The lower limit of the total light transmittance of the film in a state where a hard coat layer is provided (a film laminate having a hard coat layer) is preferably 85%, more preferably 87%, further preferably 90%, particularly preferably 91%, and most preferably 92%. By setting the total light transmittance to the above range, a clear photographic image can be achieved.
[0166] The upper limit of the haze of the thin film laminate having a hard coat layer is preferably 5%, more preferably 4%, further preferably 3%, particularly preferably 2%, and most preferably 1.5%. The lower limit of the haze is preferably 0.1%. By setting the haze to the above range, a high-contrast image can be achieved.
[0167] The lower limit of the thickness of the hard coating is preferably 0.1 μm, more preferably 0.5 μm. The upper limit of the surface processing thickness is preferably 10 μm, more preferably 8 μm, further preferably 7 μm, particularly preferably 6 μm, and most preferably 5 μm. By setting it to the above range, it is possible to exert the function as a hard coating and cope with thinness, and in addition, it is possible to reduce warping caused by curing shrinkage.
[0168] (Reflection Reduction Layer)
[0169] The reflection reducing layer may be provided directly on the film or on the hard coat layer.
[0170] As the reflection reducing layer, there are various types such as low reflection layer, antireflection layer, antiglare layer, antiglare layer, etc. Among these, in order to achieve a clearer captured image, antireflection layer and low reflection layer which do not have an antiglare function based on diffuse reflection and are called clear AR and clear LR are preferred.
[0171] (Low reflection layer)
[0172] The low reflection layer is a layer having a function of reducing the refractive index difference with air and lowering the reflectivity by providing a layer with a low refractive index (low refractive index layer) on the surface of a base film.
[0173] (Anti-reflection layer)
[0174] The anti-reflection layer is a layer that controls the thickness of the low refractive index layer so that the reflected light of the upper interface of the low refractive index layer (the interface of the low refractive index layer-air) and the low refractive lower interface (for example, the interface of the substrate film-low refractive index layer) interfere to control the reflection. In this case, the thickness of the low refractive index layer is preferably about the wavelength of visible light (400 to 700 nm) / (refractive index of the low refractive index layer × 4).
[0175] It is also preferred to provide a high refractive index layer between the antireflection layer and the base film. Two or more low refractive index layers and high refractive index layers may be provided to further enhance the antireflection effect by multiple interference.
[0176] In addition, the antireflection layer may have a moth-eye structure.
[0177] The upper limit of the reflectivity of the thin film laminate having an antireflection layer or a reflection reducing layer is preferably 2%, and if further limited, preferably 1.5%, 1.2%, 1%, 0.9%, and 0.8%, respectively. The lower limit is actually 0.05%.
[0178] The upper limit of the total light transmittance of the film having the antireflection layer or the reflection reducing layer is preferably 88%, more preferably 90%, further preferably 92%, particularly preferably 93%, and most preferably 94%.
[0179] Preferred values of the haze of the thin film laminate having a hard coat layer and the haze of the film having an antireflection layer or a reflection reducing layer are the same as the preferred values shown in the high Re film.
[0180] (Low refractive index layer)
[0181] The upper limit of the refractive index of the low refractive index layer is preferably 1.45, and more preferably 1.42. In addition, the lower limit of the refractive index of the low refractive index layer is preferably 1.20, and more preferably 1.25 or more.
[0182] It should be noted that the refractive index of the low refractive index layer is a value measured at a wavelength of 589 nm.
[0183] The thickness of the low refractive index layer is not limited, but may be appropriately set within a range of about 30 nm to 1 μm.
[0184] In addition, if the purpose is to offset the reflection on the surface of the low refractive index layer and the interface reflection between the low refractive index layer and the layer inside it (base film, hard coat layer, etc.) to further reduce the reflectivity, the thickness of the low refractive index layer is preferably 70 to 120 nm, more preferably 75 to 110 nm.
[0185] As the low refractive index layer, preferably listed are (1) a layer formed from a resin composition containing a binder resin and low refractive index particles; (2) a layer formed from a fluorine-based resin as a low refractive index resin; (3) a layer formed from a fluorine-based resin composition containing silicon dioxide or magnesium fluoride; (4) a thin film of a low refractive index material such as silicon dioxide or magnesium fluoride, etc.
[0186] The binder resin contained in the resin composition of (1) may be polyester, polyurethane, polyamide, polycarbonate, acrylic, etc. without particular limitation. Among them, acrylic is preferred, and a photopolymerizable compound polymerized (crosslinked) by light irradiation is preferred.
[0187] As the photopolymerizable compound, photopolymerizable monomers, photopolymerizable oligomers, and photopolymerizable polymers can be listed, and they can be appropriately adjusted for use. As the photopolymerizable compound, a combination of a photopolymerizable monomer and a photopolymerizable oligomer or a photopolymerizable polymer is preferred. These photopolymerizable monomers, photopolymerizable oligomers, and photopolymerizable polymers are preferably multifunctional.
[0188] Examples of the polyfunctional monomer include pentaerythritol triacrylate (PETA), dipentaerythritol hexaacrylate (DPHA), pentaerythritol tetraacrylate (PETTA), dipentaerythritol pentaacrylate (DPPA), etc. In addition, a monofunctional monomer may be used in combination to adjust the coating viscosity and hardness.
[0189] Examples of the polyfunctional oligomer include polyester (meth)acrylate, urethane (meth)acrylate, polyester-urethane (meth)acrylate, polyether (meth)acrylate, polyol (meth)acrylate, melamine (meth)acrylate, isocyanurate (meth)acrylate, and epoxy (meth)acrylate.
[0190] Examples of the polyfunctional polymer include urethane (meth)acrylate, isocyanurate (meth)acrylate, polyester-urethane (meth)acrylate, and epoxy (meth)acrylate.
[0191] The coating agent may contain, in addition to the above-mentioned components, a polymerization initiator, a catalyst for a cross-linking agent, a polymerization inhibitor, an antioxidant, an ultraviolet absorber, a leveling agent, a surfactant, and the like.
[0192] As the low refractive index particles contained in the resin composition of (1), silica particles (e.g., hollow silica particles), magnesium fluoride particles, etc. can be listed, among which hollow silica particles are preferred. Such hollow silica particles can be produced by the production method described in the examples of Japanese Patent Application Laid-Open No. 2005-099778, for example.
[0193] The average particle size of the primary particles of the low refractive index particles is preferably 5 to 200 nm, more preferably 5 to 100 nm, and further preferably 10 to 80 nm.
[0194] The low refractive index particles are more preferably surface-treated with a silane coupling agent, and particularly preferably surface-treated with a silane coupling agent having a (meth)acryloyl group.
[0195] The content of the low refractive index particles in the low refractive index layer is preferably 10 to 250 parts by mass, more preferably 50 to 200 parts by mass, and even more preferably 100 to 180 parts by mass, based on 100 parts by mass of the binder resin.
[0196] As the fluorine-based resin of (2), a polymerizable compound or a polymer thereof containing at least a fluorine atom in the molecule can be used. As the polymerizable compound, there is no particular limitation, and for example, it is preferred to have curing reactive groups such as a photopolymerizable functional group and a thermosetting polar group. In addition, it can also be a compound having these multiple curing reactive groups at the same time. In contrast to the polymerizable compound, the polymer does not have the above-mentioned curing reactive groups, etc.
[0197] As the compound having a photopolymerizable functional group, for example, a fluorine-containing monomer having an ethylenically unsaturated bond can be widely used.
[0198] In order to improve the anti-fingerprint property, it is also preferred to appropriately add a known silicone-based or fluorine-based antifouling agent to the low refractive index layer.
[0199] The thin film of (4) can be formed by a dry process such as evaporation, sputtering, CVD, etc. In addition, the sol-gel method is also a preferred method.
[0200] In order to exhibit anti-glare properties, the surface of the low refractive index layer may be a concave-convex surface, but is preferably a smooth surface.
[0201] When the surface of the low refractive index layer is a smooth surface, the upper limit of the arithmetic mean roughness SRa (JIS B0601: 1994) of the surface of the low refractive index layer is preferably 20nm, more preferably 15nm, further preferably 10nm, and particularly preferably 8nm. The lower limit is preferably 0.5nm, more preferably 1nm. In addition, the ten-point average roughness Rz (JIS B0601: 1994) of the surface of the low refractive index layer is preferably below 160nm, more preferably 50 to 155nm.
[0202] The refractive index of the high refractive index layer is preferably 1.55 to 1.85, more preferably 1.56 to 1.70.
[0203] It should be noted that the refractive index of the high refractive index layer is a value measured at a wavelength of 589 nm.
[0204] The thickness of the high refractive index layer is preferably 30 to 200 nm, more preferably 50 to 180 nm. The high refractive index layer may be a plurality of layers, preferably two or less layers, more preferably a single layer. In the case of a plurality of layers, the total thickness of the plurality of layers is preferably within the above range.
[0205] When two high refractive index layers are provided, the refractive index of the high refractive index layer on the low refractive index layer side is preferably increased. Specifically, the refractive index of the high refractive index layer on the low refractive index layer side is preferably 1.60 to 1.85, and the refractive index of the other high refractive index layer is preferably 1.55 to 1.70.
[0206] The high refractive index layer is preferably formed of a resin composition containing high refractive index particles and a resin.
[0207] Among them, the high refractive index particles are preferably antimony pentoxide particles, zinc oxide particles, titanium oxide particles, cerium oxide particles, tin-doped indium oxide particles, antimony-doped tin oxide particles, yttrium oxide particles, and zirconium oxide particles, etc. Among these, titanium oxide particles and zirconium oxide particles are suitable.
[0208] The high refractive index particles can be used in combination of two or more. In particular, in order to prevent aggregation, it is also preferred to add the first high refractive index particles and the second high refractive index particles having less surface charge than the first high refractive index particles. In addition, from the perspective of dispersibility, it is also preferred that the high refractive index particles are surface treated.
[0209] The preferred average particle size of primary particles of the high refractive index particles is the same as that of the low refractive index particles.
[0210] The content of the high refractive index particles is preferably 30 to 400 parts by mass, more preferably 50 to 200 parts by mass, and even more preferably 80 to 150 parts by mass, based on 100 parts by mass of the resin.
[0211] The resin used in the high refractive index layer is the same as the resin exemplified in the low refractive index layer except for the fluorine-based resin.
[0212] In order to flatten the low refractive index layer provided on the high refractive index layer, the surface of the high refractive index layer is also preferably flat. As a method for flattening the surface of the high refractive index layer, the method for flattening the low refractive index layer described above can be used.
[0213] The high refractive index layer and the low refractive index layer can be formed, for example, by coating a resin composition containing a photopolymerizable compound on a substrate film and drying it, and then irradiating the coated resin composition with light such as ultraviolet rays to polymerize (crosslink) the photopolymerizable compound.
[0214] In the resin combination of high refractive index layer and low refractive index layer, thermoplastic resin, thermosetting resin, solvent, polymerization initiator can be added as required. And then, dispersant, surfactant, antistatic agent, silane coupling agent, tackifier, anti-coloring agent, coloring agent (pigment, dye), defoamer, leveling agent, flame retardant, ultraviolet light absorber, adhesion imparting agent, inhibitor, antioxidant, surface modifier, easy lubricant etc. can be added.
[0215] The high refractive index layer can also be provided by a dry process using the high refractive metal oxide listed in the high refractive index particles.
[0216] In order to suppress the reflectance to be low in a wide wavelength range, the low refractive index layer and the high refractive index layer may be a plurality of layers. For example, the following configurations can be mentioned.
[0217] ·Base material / low refractive index layer / high refractive index layer / low refractive index layer
[0218] ·Base material / high refractive index layer / low refractive index layer / high refractive index layer / low refractive index layer
[0219] ·Base material / low refractive index layer / high refractive index layer / low refractive index layer / high refractive index layer / low refractive index layer
[0220] It should be noted that, here, the substrate may include a hard coat layer. In addition, the low refractive index layer and the high refractive index layer may be composed of two or three layers having different refractive indices.
[0221] For the low refractive index layer and the high refractive index layer, a dry process is preferred in order to be able to perform stable film thickness control, further reduce the wavelength dependence of the reflectivity, and achieve a lower reflectivity.
[0222] (Antistatic layer)
[0223] The upper limit of the surface resistance value of the antistatic layer is preferably e+12Ω / □ (1×10 12Ω / □), more preferably e+10Ω / □, further preferably e+9Ω / □, particularly preferably e+8Ω / □, and most preferably e+7Ω / □. In particular, when an antistatic layer is provided on the backplane, the surface resistance value is preferably less than e+8Ω / □, and more preferably less than e+7Ω / □. The lower limit of the surface resistance value is preferably e+3Ω / □, and more preferably e+4Ω / □.
[0224] Examples of the antistatic layer include an organic antistatic layer including an antistatic agent and a binder resin; and an inorganic antistatic layer including a metal or metal oxide layer.
[0225] Examples of the antistatic agent include lithium salts, surfactants, polymers containing polar groups, conductive polymers, metal fine particles, and metal oxide particles.
[0226] Examples of the lithium salt include lithium chloride, lithium fluoride, lithium bromide, lithium iodide, lithium perchlorate, lithium acetate, lithium fluorosulfonate, lithium methanesulfonate, lithium trifluoromethanesulfonate, and lithium pentafluoroethanesulfonate.
[0227] Surfactants include nonionic surfactants, anionic surfactants, cationic surfactants, and zwitterionic surfactants. Examples of nonionic surfactants include (N,N-bis(2-hydroxyethyl)alkylamines and fatty acid esters), examples of anionic surfactants include (alkyl sulfonates), examples of cationic surfactants include (alkyl ammonium salts), and examples of zwitterionic surfactants include (alkyl betaines and imidazoline-type amphoteric surfactants).
[0228] The polymer containing polar groups is obtained by incorporating the conductivity-imparting functional groups of the above-mentioned surfactants into the polymer units. In the nonionic system, polyethylene oxide, polyethylene oxide crosslinked bodies, polyethylene oxide copolymers, polyethylene glycol, polyethylene glycol copolymers, etc. can be listed. In the cationic system, quaternary ammonium salt systems are representative, and methacrylate copolymers containing quaternary ammonium salt groups, maleimide copolymers containing quaternary ammonium salt groups, methacrylic acid copolymers containing quaternary ammonium salt groups, etc. can be listed.
[0229] Among the anionic copolymers, sulfonic acid copolymers are representative, and examples thereof include polystyrene sulfonate, copolymers of styrene sulfonate, etc. Examples of monomers used in cationic and anionic copolymers include methyl methacrylate, styrene, ethylene, vinyl acetate, and the like.
[0230] Examples of the conductive polymer include polyacetylene, polyaniline, polythiophene, and polyethylene dioxythiophene / polystyrene sulfonic acid (PEDOT / PSS).
[0231] Examples of the metal fine particles include gold, silver, copper, aluminum, and nickel.
[0232] As metal oxide particles, for example, at least one oxide selected from indium, tin, antimony, lead and titanium is preferred, and specific examples include indium oxide (ITO), tin oxide (SnO2), antimony / tin oxide (ATO), antimony oxide (Sb2O5), lead / titanium oxide (PTO), etc.
[0233] The shape of the metal particles and metal oxide particles is not particularly limited, and may be any of spherical, needle-shaped, and flake-shaped. From the perspective of achieving both dispersibility and transparency, the particle size of the conductive metal oxide is preferably 0.001 to 0.2 μm, more preferably 0.01 to 0.1 μm.
[0234] The antistatic agent can be appropriately selected from the viewpoints of the desired antistatic property, color tone, transparency, etc. If the antistatic property is high, especially if the surface resistance is set to 10E+8Ω / □ or less, and further set to 10E+7Ω / □ or less, conductive polymers, metals, metal oxide fine particles, metals, and metal oxide films are preferred.
[0235] As the binder resin, various resins used in common coating agents can be used. For example, polyester resins, urethane resins, polyamide resins, acrylic resins, styrene resins, ethylene vinyl alcohol resins, etc. can be listed. In addition, the binder resin can be cross-linked using a curing agent, and as the curing agent, isocyanate compounds, melamine, benzoguanamine, epoxy compounds, multifunctional acrylic compounds, etc. can be listed. In addition, it can be a radiation-curable resin such as those listed in the hard coat layer.
[0236] The lower limit of the content of the antistatic agent in the components constituting the antistatic layer is preferably 0.1 mass %, more preferably 0.5 mass %, and further preferably 1 mass %. The upper limit is preferably 70 mass %, more preferably 60 mass %, and further preferably 50 mass %. It should be noted that, when a film is formed by coating the antistatic agent itself, such as in the case of cationic and anionic copolymers, the content may exceed 70 mass %, and a binder resin may not be used.
[0237] The antistatic layer containing the antistatic agent and the binder resin can be provided by applying a coating liquid containing them on a film, and drying and curing the liquid.
[0238] The lower limit of the thickness of the antistatic layer containing the antistatic agent and the binder resin is 0.01 μm, more preferably 0.05 μm, and further preferably 0.1 μm. The upper limit is preferably 20 μm, more preferably 10 μm, and further preferably 5 μm. From the viewpoints of the type of antistatic agent, the desired antistatic property, color tone, transparency, etc., the content of the antistatic agent and the thickness of the antistatic layer can be adjusted.
[0239] As the inorganic antistatic layer of the metal or metal oxide layer, the raw materials listed in the metal particles and metal oxide particles can be exemplified. The inorganic antistatic layer can be made using dry processes such as evaporation, sputtering, and CVD. The lower limit of the thickness of the inorganic antistatic layer is preferably 0.001 μm, more preferably 0.005 μm, and further preferably 0.01 μm. The upper limit is preferably 2 μm, more preferably 1 μm, and further preferably 0.5 μm.
[0240] The preferred values of haze and total light transmittance of the film having an antistatic layer are the same as those of the high Re film provided with a hard coat layer. By setting the values within this range, a clear image can be obtained.
[0241] About the film with antistatic layer, in the hue display based on Hunter Lab when measuring by transmission, the b value is preferably below 5 in absolute value, more preferably below 4, further preferably below 3.5, and particularly preferably below 3. The preferred value of the a value is also the same. By setting as above, there is no need to use the software of the camera, color matching filters etc. to perform excessive color matching, and the captured image of natural tone can be obtained.
[0242] The antistatic layer can be arranged at any position, such as between the film and the hard coating layer, between the hard coating layer and the anti-reflection layer, on the surface of the anti-reflection layer opposite to the film, on the surface of the film opposite to the hard coating layer or the anti-reflection layer, etc. The anti-reflection layer may not be present on the surface of the film opposite to the image display unit.
[0243] In addition, an antistatic agent may be added to the hard coat layer, antireflection layer, etc. so that the hard coat layer, antistatic layer, etc. themselves have an antistatic function, or an antistatic agent may be added to the adhesive or pressure-sensitive adhesive used when attaching the film so that they have an antistatic function.
[0244] If a hard coating layer, an anti-reflection layer, an adhesive layer, a bonding agent layer, etc. are provided on the antistatic layer so that the antistatic layer is not the outermost layer, the antistatic layer can be a conductive layer such as a mesh structure of a metal film, a metal, a printed material of a carbon paste, or a conductor with a conductivity lower than e+3Ω / □.
[0245] In addition, when the outermost layer is an antistatic layer, the preferred range of the surface roughness of the antistatic layer is the same as the above range.
[0246] When the antistatic layer has low transmittance or high haze, the portion of the antistatic layer where the camera receives light may have a mesh structure with multiple small holes, or the portion where the camera receives light may have no antistatic layer.
[0247] (Film Configuration)
[0248] In the UPC type image display device, thin films can be used in various parts as described above.
[0249] In order to suppress rainbow spots generated when using an oriented film, one of the preferred embodiments is to include a high Re film in the optical path of the camera. By using a high Re film, rainbow spots generated in a captured image can be effectively suppressed.
[0250] High Re films can be used for backplanes, electrode substrate films of image display units, electrode substrate films of touch panels, polarizer protective films, cover plates, surface protective films, etc. Among them, stretched oriented films such as polyester are often used for backplanes, electrode substrate films of touch panels, and surface protective films, and are preferably used as objects of high Re films. In particular, backplanes and surface protective films are suitable objects for high Re films.
[0251] A preferred configuration is that, in the optical path of the camera, as a component other than the high-Re film, there is no component whose in-plane phase difference is 300 nm or more. By making the component whose in-plane phase difference is 300 nm or more in the optical path of the camera of the image display device during shooting only the high-Re film, rainbow spots in the peripheral part of the captured image can be effectively suppressed.
[0252] On the other hand, even when there is a component having a retardation of 300 nm or more in addition to the high-Re film, the effect of the high-Re film, such as being able to reduce the rainbow spot in the peripheral portion of the captured image or being able to reduce the area of the rainbow spot, is fully exhibited. Therefore, in addition to the high-Re film, there may be a component having a retardation of 300 nm or more. In other words, when a component having a retardation of 300 nm or more is used in the optical path of the camera of the image display device, it is preferable to use a high-Re film at least at one location.
[0253] (Combination of multiple oriented films)
[0254] When the high-Re film and the medium-Re film are combined, it is preferred that the high-Re film also exists on the camera module side or the side opposite to the camera module where the medium-Re film exists, based on the polarizing plate. When the medium-Re film exists only on one side and the high-Re film exists only on the other side, the high-Re film may not be able to sufficiently suppress the rainbow spots generated by the medium-Re film.
[0255] When the high Re film and the medium Re film are combined, it is preferable to arrange the high Re film farther from the camera module than the medium Re film because the effect of suppressing rainbow spots becomes higher.
[0256] In order to achieve a higher rainbow spot suppression effect, the angle between the slow axis of the high Re film and the absorption axis of the polarizer of the polarizing plate is preferably set to 25 to 65 degrees, more preferably 30 to 60 degrees, further preferably 35 to 55 degrees, and particularly preferably 40 to 50 degrees.
[0257] When using multiple high Re films, it is preferred that the angle between the slow axes of the high Re film and the medium Re film when used in combination is set to 25 degrees or less. The aforementioned angle is more preferably less than 20 degrees, further preferably less than 15 degrees, and particularly preferably less than 10 degrees. By setting as above, the in-plane retardation of each other will not interfere with each other, and rainbow spots can be effectively suppressed. In particular, when the retardation of the two films is close, it is preferably set as above.
[0258] When a plurality of high Re films are used, the difference in in-plane retardation between the high Re film and the medium Re film when used in combination is preferably set to 2000 nm or more, more preferably 2500 nm or more, further preferably 3000 nm or more, particularly preferably 3500 nm or more, and most preferably 3800 nm or more. By setting the above values or more, rainbow spots can be effectively suppressed.
[0259] When multiple high-Re films are used, when a high-Re film and a medium-Re film are used in combination, it is preferred to make the slow axis of the film with higher retardation 90 degrees with the long side direction of the display screen from the perspective of eliminating rainbow spots. It should be noted that 90 degrees includes the same allowable range as above.
[0260] Even when the angle between their slow axes is close to 90 degrees, the above arrangement makes it possible to suppress the occurrence of rainbow spots because the retardation difference between the two films increases as the light tilts from the normal line toward the oblique direction.
[0261] The high Re film can be used on both sides of the camera module side or the opposite side of the camera module based on the polarizer, and is preferably used only on one side. When used on both sides, rainbow spots may also occur. In this case, the difference in in-plane retardation between each other is preferably the same as the range described above.
[0262] The objects of the medium Re film are the same as those of the high Re film, but among them, the electrode substrate of the image display unit, the electrode substrate of the touch panel, the surface protection film, the cover plate, and the back plate are preferred. The following combination is particularly preferred.
[0263] The backplane of the image display panel is set as a high-Re film, and the electrode substrate of the image display unit is set as a medium-Re film;
[0264] The backplane of the image display panel is set as a high-Re film, and the electrode substrate of the touch panel is set as a medium-Re film;
[0265] The surface protection film is set as a high-Re film, and the electrode substrate of the touch panel is set as a medium-Re film; The cover plate is set as a high-Re film, and the electrode substrate of the touch panel is set as a medium-Re film;
[0266] Set the surface protection film as a high-Re film and the cover plate as a medium-Re film;
[0267] The cover plate is set as a high-heat film, and the surface protection film is set as a medium-heat film.
[0268] When used in combination with a medium Re film, the slow axis of the high Re film is preferably at 45 degrees with respect to the absorption axis of the polarizer from the viewpoint of being able to more effectively suppress rainbow spots.
[0269] In order to suppress the rainbow spots generated when using the oriented film, another preferred embodiment is: at least one of the side of the backplane opposite to the image display unit and the side of the surface protection film of the image display device opposite to the image display unit has a reflection reduction layer. Furthermore, it is preferred that at least the side of the backplane opposite to the image display unit has a reflection reduction layer, and in particular, both of the above have an anti-reflection layer.
[0270] The reflection reduction layer can reduce the effect of the film as a polarizer caused by the interface reflection between the film and the air, and can suppress the occurrence of rainbow spots. By providing an anti-reflection layer, rainbow spots can be suppressed even when a medium-Re film is used for the back plate or the surface protection film. By also providing an anti-reflection layer for the high-Re film, the effect of further suppressing rainbow spots can be obtained. In addition, even if the back plate or the surface protection film is a zero-Re film, when there is a medium-Re film in the optical path of the camera, rainbow spots can be suppressed by providing a reflection reduction layer for the zero-Re film.
[0271] Example
[0272] Hereinafter, the present invention will be described in more detail with reference to the examples, but the present invention is not limited to the following examples, and can also be implemented by appropriately applying changes within the scope of the present invention, which are all included in the technical scope of the present invention. It should be noted that the physical property evaluation methods in the following examples are as follows.
[0273] (1) Refractive index of polyester film
[0274] A molecular orientation meter (MOA-6004 molecular orientation meter manufactured by Oji Scientific Instruments Co., Ltd.) was used to determine the slow axis direction of the film, and a 4 cm × 2 cm rectangle was cut out in a manner that the slow axis direction was parallel to the long side as a measurement sample. For this sample, an Abbe refractometer (NAR-4T manufactured by ATAGO CO., LTD., with a measurement wavelength of 589 nm) was used to determine the orthogonal biaxial refractive index (refractive index in the slow axis direction: ny, fast axis (refractive index in the direction orthogonal to the slow axis direction): nx) and the refractive index in the thickness direction (nz).
[0275] (2) In-plane retardation (Re)
[0276] In-plane retardation refers to a parameter defined by the product (△Nxy×d) of the orthogonal biaxial refractive index anisotropy (△Nxy=|nx-ny|) and the film thickness d (nm) on the film, which is a measure of optical isotropy and anisotropy. The biaxial refractive index anisotropy (△Nxy) is obtained using the method (1) above, and the absolute value of the biaxial refractive index difference (|nx-ny|) is calculated as the refractive index anisotropy (△Nxy). The thickness d (nm) of the film is measured using an electric micrometer (Millitron 1245D, manufactured by FILM LIWF), and the unit is converted into nm. The retardation (Re) is obtained from the product (△Nxy×d) of the refractive index anisotropy (△Nxy) and the film thickness d (nm).
[0277] (3) Thickness direction retardation (Rth)
[0278] The thickness direction retardation is a parameter that represents the average of the retardation obtained by multiplying the two birefringences △Nxz (=|nx-nz|) and △Nyz (=|ny-nz|) by the film thickness d when the film is observed in a cross section in the thickness direction. The thickness direction retardation (Rth) is obtained by calculating the average value of (△Nxz×d) and (△Nyz×d) obtained by the method (1) above and the film thickness d (nm).
[0279] (4) NZ coefficient
[0280] The coefficient Nz is obtained by substituting nx, ny, and nz obtained by the method (1) above into the equation represented by |ny-nz| / |ny-nx|.
[0281] (5) Planar orientation
[0282] The plane orientation degree is determined by substituting nx, ny, and nz obtained by the method of (1) above into the formula represented by |nx+ny| / 2-nz.
[0283] (6) Absorption axis of polarizer
[0284] A polarizing filter with a known absorption axis is overlapped with a polarizing plate, placed on a surface light source, and the polarizing filter is rotated, and the direction at 90 degrees to the absorption axis direction of the polarizing filter in the darkest state is set as the absorption axis direction of the polarizing plate. It should be noted that in the case of a long strip polarizing plate obtained by stretching PVA along the length direction, the length direction becomes the absorption axis direction, and therefore, the length direction can be regarded as the absorption axis direction.
[0285] (7) Reflectivity
[0286] The 5-degree reflectance at a wavelength of 550 nm was measured from the surface on the anti-reflection layer side (or low-reflection layer side) using a spectrophotometer (manufactured by Shimadzu Corporation, UV-3150). In addition, the surface of the polyester film opposite to the side on which the anti-reflection layer (or low-reflection layer) was coated with a black marker pen and then a black plastic tape (KYOWA LIMITED plastic tape HF-737, 50 mm wide) was attached for measurement.
[0287] (8) Transmittance
[0288] The determination was carried out in accordance with K 7375:2008.
[0289] (9) Haze
[0290] The haze of the film was measured using a turbidity meter (NHD2000, manufactured by NIPPON DENSHOKU INDUSTRIES Co., Ltd.) in accordance with JIS-K7136.
[0291] (10) Surface roughness
[0292] The parameters of each roughness were measured according to ISO 25178 using a non-contact surface profile measuring system (VertScan R550H-M100 manufactured by Ryoka Systems Co., Ltd.) under the following conditions.
[0293] (Measurement conditions)
[0294] Measurement mode: WAVE mode
[0295] Objective lens: 10 times
[0296] 0.5×Tube lens
[0297] Measurement area: 936μm×702μm
[0298] (Analysis conditions)
[0299] Surface correction: Four times correction
[0300] Interpolation processing: Full interpolation
[0301] ISO parameter processing: S-Filter 10μm specified
[0302] The measurement was performed at 5 locations, and the average value was calculated.
[0303] (11) Rainbow spot evaluation
[0304] A 5 cm×5 cm pseudo panel having the following laminated structure was prepared.
[0305] Film 3
[0306] Glass 3 (thickness 100 μm)
[0307] Film 2
[0308] Glass 2 (thickness 100 μm)
[0309] Polarizing plate (TAC / PVA polarizing plate / TAC structure, thickness about 140μm)
[0310] Glass 1 (thickness 100 μm)
[0311] Film 1
[0312] Here, film 1 corresponds to the backplane, glass 1 corresponds to the image display unit, film 2 corresponds to the touch panel base film or anti-scattering film, glass 3 corresponds to the cover glass plate, and film 3 corresponds to the surface protection film. This is because glass 2 is bonded to film 2 with water when evaluated as described below, so waterproofing is performed to prevent the TAC film from swelling.
[0313] As standard panels, films 1, 2, and 3 were all made of TAC films having a retardation of substantially zero and a thickness of 60 μm. The panels were bonded together using a commercially available substrate-free optical adhesive.
[0314] Next, as described in the examples, evaluation panels were prepared by replacing each film with a sample film. The evaluation panels were bonded with a commercially available substrate-free optical adhesive except for the replacement portion, and the portion to be replaced was bonded by dripping water so as not to form an air interface.
[0315] The upper surface cover of a commercially available smartphone with a built-in selfie camera was removed, and an evaluation panel or a standard panel was placed on it so that the film 1 was on the camera side. Five images were taken with the composition changed for a clear sky with about 50% white clouds. The five images taken using the evaluation panel were compared with the images taken using the standard panel, and the white cloud portion was scored according to the following criteria.
[0316] 1: Rainbow spots, coloring, or uneven brightness are observed in a wide area except the center of the image. 2: Rainbow spots, coloring, or uneven brightness are observed in part of the peripheral area of the image; or, although the area is large, the rainbow spots, coloring, or uneven brightness are slight.
[0317] 3: Rainbow spots, coloring, or uneven brightness are observed in a narrow portion of the image periphery; or, although the range is limited to a portion, the rainbow spots, coloring, or uneven brightness are slight.
[0318] 4: Slight rainbow spots, coloring, or uneven brightness are observed in extremely limited areas such as the four corners; or, although the range is a narrow area at the periphery, the rainbow spots, coloring, or uneven brightness are slight.
[0319] 5: No colorization of the image is observed.
[0320] (12) Surface resistance
[0321] The surface resistance was measured using a surface resistance measuring instrument (manufactured by Mitsubishi Petrochemical Corporation, Hiresta HT-210) under the conditions of applied voltage of 500 V, 25° C., and 15% RH. The unit of the surface specific resistance value is Ω / □ (also expressed as Ω / sq).
[0322] (13) Color a value, b value
[0323] The a value and the b value were measured based on transmission using a colorimeter (ZE2000 manufactured by NIPPON DENSHOKU INDUSTRIES Co., Ltd.) in accordance with JIS Z8722.
[0324] Preparation of sample films
[0325] (Polyester resin)
[0326] Polyester A (PET(A))
[0327] Polyethylene terephthalate with an intrinsic viscosity of 0.62 dl / g
[0328] Polyester B (PET(B))
[0329] A melt mixture of 10 parts by mass of an ultraviolet absorber (2,2'-(1,4-phenylene)bis(4H-3,1-benzoxazin-4-one) and 90 parts by mass of PET (A).
[0330] High refractive index adhesive modified coating liquid
[0331] Polymerization of copolyester resin
[0332] 381 parts by mass of dimethyl naphthalate, 58.3 parts by mass of dimethyl terephthalate, 41.5 parts by mass of dimethyl 5-sulfonate sodium isophthalate, 46.7 parts by mass of diethylene glycol, 245.8 parts by mass of ethylene glycol and 0.5 parts by mass of tetra-n-butyl titanate were added to a stainless steel autoclave equipped with a stirrer, a thermometer and a partial reflux condenser, and an ester exchange reaction was carried out from 160°C to 220°C over 4 hours. Then, the temperature was raised to 255°C, and after the reaction system was gradually depressurized, it was reacted under a reduced pressure of 30 Pa for 1 hour and 30 minutes to obtain a copolyester resin A. The obtained copolyester resin was light yellow and transparent. The composition measured by 1H-NMR was 2,6-naphthalene dicarboxylic acid / terephthalic acid / sodium 5-sulfonate sodium isophthalate / / ethylene glycol / diethylene glycol = 78 / 15 / 7 / / 90 / 10 (mol%).
[0333] Preparation of polyester aqueous dispersion
[0334] 20 parts by mass of the copolyester resin (A) and 15 parts by mass of ethylene glycol tert-butyl ether were added to a reactor equipped with a stirrer, a thermometer and a reflux device, and heated and stirred at 110°C to dissolve the resin. After the resin was completely dissolved, 65 parts by mass of water were slowly added to the polyester solution while stirring. After the addition, the liquid was cooled to room temperature while stirring to prepare a milky white polyester aqueous dispersion B with a solid content of 20% by mass.
[0335] Polymerization of blocked polyisocyanate crosslinkers
[0336] A four-necked flask equipped with a stirrer, a thermometer, a reflux condenser, a nitrogen blowing tube, and a dropping funnel was set to a nitrogen atmosphere, 600 parts of HMDI and 30 parts of a polycaprolactone polyester polyol (PLACCEL 303 manufactured by Daicel Corporation, molecular weight 300) as a triol were added, and the temperature in the reactor was maintained at 90° C. for 1 hour under stirring to carry out a urethanization reaction. Thereafter, the temperature in the reactor was maintained at 60° C., an isocyanuration catalyst tetramethylammonium decanoate was added, and phosphoric acid was added when the yield reached 48% to stop the reaction, thereby obtaining a polyisocyanate composition C.
[0337] Next, a four-necked flask equipped with a stirrer, a thermometer, a reflux condenser, a nitrogen blowing tube, and a dropping funnel was set to a nitrogen atmosphere, and 100 parts of polyisocyanate composition C, 19 parts of methoxy polyethylene glycol (UNIOX M400 manufactured by NOFCORPORATION) with a molecular weight of 400 (reacting with 10% of all isocyanate groups of the polyisocyanate), and 37 parts of propylene glycol monomethyl ether acetate were added, and kept at 80° C. for 7 hours. Thereafter, 38 parts of methyl ethyl ketoxime were added dropwise while keeping the temperature of the reaction liquid at 50° C. The infrared spectrum of the reaction liquid was measured, and the isocyanate group disappeared, thereby obtaining an aqueous blocked polyisocyanate resin D having a solid content concentration of 80% by mass.
[0338] Preparation of high refractive index adhesive modified coating liquid E
[0339] The following coating agents were mixed to prepare a high refractive index adhesive modified coating liquid E. Particle A was SnO2 having a refractive index of 2.1, and particle B was silica particles having an average primary particle size of about 500 nm.
[0340] Water: 43.26% by mass
[0341] Isopropyl alcohol: 30.00 mass%
[0342] Polyester aqueous dispersion B: 20.07 mass%
[0343] Water-based blocked polyisocyanate resin D: 0.74 mass%
[0344] Granule A: 5.58 mass%
[0345] (Cerameth S-8 manufactured by TAKI CHEMICAL CO., LTD., solid content concentration: 8% by mass)
[0346] Particle B: 0.30 mass%
[0347] (SEAHOSTAR KEW50 manufactured by Nippon Shokubai Co., Ltd., solid content concentration: 15% by mass)
[0348] Surfactant: 0.05 mass%
[0349] (DYNOL 604 manufactured by Nissin Chemical Industry Co., Ltd., solid content concentration: 100% by mass)
[0350] Preparation of coating liquid F for forming hard coat layer
[0351] The following coating materials were mixed to prepare a coating liquid F for forming a hard coat layer.
[0352] Methyl ethyl ketone: 65.00 mass%
[0353] Dipentaerythritol hexaacrylate: 27.20 mass%
[0354] (A-DPH manufactured by Shin-Nakamura Chemical Industry Co., Ltd.)
[0355] Polyethylene glycol diacrylate: 6.80 mass%
[0356] (A-400 manufactured by Shin-Nakamura Chemical Industry Co., Ltd.)
[0357] Photopolymerization initiator: 1.00 mass%
[0358] (Irgacure 184 manufactured by Ciba Specialty Chemicals)
[0359] Preparation of coating liquid G for forming high refractive index layer
[0360] 80 parts of methyl methacrylate, 20 parts of methacrylic acid, 1 part of azoisobutyronitrile, and 200 parts of isopropyl alcohol were placed in a reaction container and reacted at 80° C. for 7 hours under a nitrogen atmosphere to obtain an isopropyl alcohol solution of a polymer having a weight average molecular weight of 30,000. The obtained polymer solution was further diluted with isopropyl alcohol to a solid content of 5% to obtain an acrylic resin solution B. Next, the obtained acrylic resin solution was mixed with the following components to obtain a coating solution G for forming a high refractive index layer.
[0361] Acrylic resin solution: 5 parts by mass
[0362] Bisphenol A diglycidyl ether: 0.25 parts by mass
[0363] Titanium oxide particles with an average particle size of 20 nm: 0.5 parts by mass
[0364] Triphenylphosphine: 0.05 parts by mass
[0365] Isopropyl alcohol: 14.25 parts by mass
[0366] Preparation of coating liquid H for forming low refractive index layer
[0367] 2,2,2-Trifluoroethyl acrylate (45 parts by mass), perfluorooctylethyl acrylate (45 parts by mass), acrylic acid (10 parts by mass), azoisobutyronitrile (1.5 parts by mass), and methyl ethyl ketone (200 parts by mass) were placed in a reaction container and reacted at 80° C. for 7 hours under a nitrogen atmosphere to obtain a methyl ethyl ketone solution of a polymer having a weight average molecular weight of 20,000. The obtained polymer solution was diluted with methyl ethyl ketone to a solid content concentration of 5% by mass to obtain a fluoropolymer solution C.
[0368] The obtained fluoropolymer solution C was mixed as follows to obtain a coating solution H for forming a low refractive index layer.
[0369] Fluoropolymer solution C: 44 parts by mass
[0370] · 1,10-bis(2,3-epoxypropoxy)-2,2,3,3,4,4,5,5,6,6,7,7,8,8,9,9-hexafluorodecane (Fluorite FE-16 manufactured by KYOEISHA CHEMICAL Co., LTD.): 1 part by mass
[0371] Triphenylphosphine: 0.1 parts by mass
[0372] Methyl ethyl ketone: 19 parts by mass
[0373] Production of polyester film as base material
[0374] (Film A)
[0375] As the raw material for the intermediate layer of the substrate film, 90 parts by mass of PET (A) resin pellets without particles and 10 parts by mass of PET (B) resin pellets containing ultraviolet absorbers were dried under reduced pressure (1 Torr) at 135°C for 6 hours and then supplied to extruder 2 (for intermediate layer II). In addition, PET (A) was dried by a conventional method and supplied to extruder 1 (for outer layer I and outer layer III) respectively, and dissolved at 285°C. The two polymers were filtered using a filter material of a stainless steel sintered body (95% of particles with a nominal filtration accuracy of 10 μm were cut off), stacked using two kinds of three-layer confluence blocks, extruded from a tube head into a sheet, and then wound onto a casting drum with a surface temperature of 30°C using an electrostatic casting method, cooled and solidified to produce an unstretched film. At this time, the discharge amount of each extruder was adjusted so that the thickness ratio of layer I, layer II, and layer III became 10:80:10.
[0376] Then, the coating amount after drying was 0.08 g / m 2 After the adhesive modified coating liquid (E) is applied to both sides of the unstretched PET film, it is dried at 80°C for 20 seconds. During the coating, a cartridge filter with a 95% separation particle size of 2 μm is set in the line for delivering the coating liquid to the coating die to remove the aggregates of particles.
[0377] The unstretched film with the coating layer formed thereon was introduced into a tenter stretching machine, and while the ends of the film were grasped by a clamp, it was introduced into the tenter at 110°C and stretched to 4.0 times in the width direction. Then, while maintaining the width stretched in the width direction, it was treated in a heat fixing zone at a temperature of 190°C for 10 seconds, and further relaxed by 3.0% in the width direction to obtain a stretched PET film. The reflectivity of the PET film A was 5.2%.
[0378] (Film B~H)
[0379] Films as described in the table were obtained in the same manner as in Film A except that the thickness of the unstretched film was adjusted.
[0380] (Film I)
[0381] The unstretched PET film obtained by the same operation as film A except for adjusting the thickness was heated to 110°C and stretched 1.5 times between rolls with different peripheral speeds to a coating weight of 0.08 g / m after drying. 2 The adhesive modified coating liquid was applied to both sides in a manner and dried in the same manner as above. The film formed with the obtained coating layer was introduced into a tenter stretching machine, and while the ends of the film were grasped by a clamp, it was introduced into a tenter at 110°C and stretched to 4.0 times in the width direction. Then, while maintaining the width stretched in the width direction, it was treated in a heat fixing zone at a temperature of 190°C for 10 seconds, and further relaxed by 2.0% in the width direction to obtain a stretched PET film.
[0382] (Film J)
[0383] The same operation as for Film I was carried out except that the thickness was adjusted and the stretching between the rolls was set to 2.0 times to obtain a stretched PET film.
[0384] (Polarizer protective film K)
[0385] The same operation as for Film I was carried out except that the thickness was adjusted and the stretching between the rolls was set to 2.5 times to obtain a stretched PET film.
[0386] (Polarizer protective film L, M, N)
[0387] A stretched PET film was obtained in the same manner as in Film I except that the thickness was adjusted, the stretching between the rolls was set to 3.6 times, and the temperature of the tenter was set to 125°C.
[0388] Table 1 shows the properties of these films.
[0389] [Table 1]
[0390]
[0391] (Production of surface treatment films)
[0392] Anti-reflection layer 1
[0393] The coating liquid F for forming a hard coat layer was applied to one side of the polyester film A and dried at 70° C. for 1 minute to remove the solvent. Then, the film coated with the hard coat layer was irradiated with ultraviolet rays using a high pressure mercury lamp to form a hard coat layer with a thickness of 5 μm.
[0394] Furthermore, the coating liquid G for forming a high refractive index layer obtained by the above method was applied to the hard coat layer, and dried at 150° C. for 2 minutes to form a high refractive index layer with a film thickness of 0.1 μm. The coating liquid H for forming a low refractive index layer obtained by the above method was applied to the high refractive index layer, and dried at 150° C. for 2 minutes to form a low refractive index layer with a film thickness of 0.1 μm, thereby obtaining a surface-processed film A-ar1 laminated with an antireflection layer 1. Similarly, each surface-processed film laminated with an antireflection layer 1 shown in Table 2 was obtained.
[0395] Anti-reflection layer 2
[0396] On the hard coating layer surface of the polyester film A laminated with a hard coating layer obtained above, silicon dioxide as a low refractive index layer and titanium oxide as a high refractive index layer were provided by a sputtering method to obtain a surface processed film A-ar2 laminated with an antireflection layer 2 showing a structure of hard coating layer side / low refractive index layer / high refractive index layer / low refractive index layer / high refractive index layer / low refractive index layer. Similarly, each surface processed film laminated with an antireflection layer 2 shown in Table 2 was obtained.
[0397] Low reflective layer
[0398] The hard coating layer of the polyester film L laminated with a hard coating layer obtained above was coated with the coating liquid H for forming a low refractive index layer obtained by the above method, and dried at 150°C for 2 minutes to form a low refractive index layer with a thickness of 2 μm, thereby obtaining a surface-processed film L-lr1 laminated with an anti-reflection layer. The same operation was performed to obtain each surface-processed film laminated with a low reflection layer shown in Table 2.
[0399] The surface roughness (Sa) of the antireflection layer and the low reflection layer of the surface processed film is 2 nm or less.
[0400] [Table 2]
[0401]
[0402] Examples 1 to 21, Comparative Examples 1 to 3, Reference Examples
[0403] The evaluation panel obtained by changing the film 3 to the surface processed film shown in Table 3 was used to perform photography and evaluate the rainbow spots. The angle between the slow axis of the film and the absorption axis of the polarizer at the position of the film 3 was set to 45 degrees in Examples 1 to 12, 0 degrees in Example 11, and 90 degrees in Example 12. In addition, the angle between the long side of the screen and the slow axis of the film was changed to 0 degrees, 45 degrees, and 90 degrees for evaluation.
[0404] [Table 3]
[0405]
[0406] As in Comparative Example 1, rainbow spots were observed in the film A without a functional layer, but when an anti-reflection layer was provided as in Example 1, the extent of the rainbow spots became a practical level. Furthermore, when the reflectivity was reduced as in Example 17, the rainbow spots were more effectively suppressed. The same was true for Comparative Example 2, Example 14, and Example 18 obtained using the film L. In addition, in Example 19, which had a higher reflectivity than Example 14, the effect of suppressing rainbow spots became weaker. The same was also true in the comparison of Comparative Example 3, Example 15, and Example 20, and in the comparison of the reference example, Example 16, and Example 21. Based on these results, it can be seen that the higher the reflectivity, the better the effect of suppressing rainbow spots.
[0407] In addition, as can be seen from Examples 2, 9, 16, and 18 to 21: when the slow axis of the film of the back panel is parallel to the long side direction of the screen, the area where rainbow spots are prone to appear becomes outside the shooting frame, and in the resulting captured image, the area where rainbow spots occur becomes smaller.
[0408] Embodiments 22-23
[0409] Films 1 and 3 were replaced with the films shown in Table 4 to obtain an evaluation panel, and the same evaluation was performed. The slow axes of the two films were set to be parallel, and the angle formed with the absorption axis of the polarizer was set to 45 degrees. The angle formed between the long side of the screen and the slow axis of the film was set to 0 degrees.
[0410] [Table 4]
[0411]
[0412] As is clear from Examples 22 to 24, even when a film having retardation as a base film is used as a surface protection film for a back sheet or a screen, rainbow spots can be suppressed if an antireflection layer or a low reflection layer is provided on the film.
[0413] Embodiment 25
[0414] 100 parts by mass of a toluene dispersion of ATO, which is a tin oxide-based compound and is an antistatic agent [manufactured by ISHIHARA SANGYOKAISHA, LTD., trade name "SN-100P", solid content concentration of 30% by mass] and 30 parts by mass of a copolyester resin [manufactured by TOYOBO CO., LTD., trade name "VYLON 20SS", solid content concentration of 30% by mass] are added to a mixed solvent of cyclohexanone and toluene in a mass ratio of 1 / 1 to prepare an antistatic coating agent 1 with a solid content concentration of 5% by mass.
[0415] The antistatic coating agent 1 was applied to the surface of Far1 opposite to the antireflection layer and dried at 120° C. for 3 minutes to form an antistatic layer with a thickness of 0.25 μm, thereby obtaining an antireflection film Far1-as1 having an antistatic layer.
[0416] The rainbow spot evaluation was performed in the same manner as in Example 6 except that Far1-as1 was used.
[0417] Embodiment 26
[0418] As the antistatic coating agent 2, an antireflection film Far1-as2 having an antistatic layer with a thickness of about 0.12 μm was obtained by using an antistatic coating agent containing PEDOT as a conductive polymer (ARACOAT AS601D / CL910 (mass ratio) = 10 / 1, manufactured by Arakawa Chemical Industries, Ltd., solid content concentration of 3.0%) in the same manner as in Example 25. The rainbow spot evaluation was performed in the same manner.
[0419] Embodiment 27
[0420] The same operation as above was performed to set a hard coating layer on the film F, and the same operation as Example 25 was performed to set an antistatic layer on the hard coating layer, and further, an antireflection layer 1 was set on the antistatic layer in the same manner as above to obtain an antireflection film Far1-as3 having an antistatic layer. The rainbow spot evaluation was performed in the same manner.
[0421] Embodiment 28
[0422] An ITO antistatic layer of 0.01 μm was formed by sputtering on one surface of the film F. Furthermore, an antireflection layer 1 was provided on the antistatic layer to obtain antireflection films Far1-as4 having an antistatic layer. The rainbow spot evaluation was performed in the same manner.
[0423] Embodiment 29
[0424] After coating the hard coating layer forming coating liquid F on one side of the polyester film F, it was dried at 80°C and further cured by ultraviolet irradiation to form a hard coating layer with a thickness of 5 μm. The high refractive index layer forming coating liquid obtained by the above method was further coated on the hard coating layer, and dried at 150°C for 2 minutes to form a high refractive index layer with a film thickness of 0.1 μm. The low refractive index layer forming coating liquid obtained by the following method was coated on the high refractive index layer and dried, and then cured by ultraviolet irradiation to form a low refractive index layer, thereby obtaining an anti-reflection film Faras having an antistatic layer. The rainbow spot evaluation was performed in the same manner.
[0425] Coating liquid for forming low refractive index layer having antistatic property
[0426] 2.2 wt% of dimethylaminoethyl methacrylate quaternary ammonium salt (manufactured by KYOEISHA CHEMICAL Co., LTD., trade name: LIGHTESTER DQ100), 2 wt% of EO-modified dipentaerythritol hexaacrylate (trade name: DPEA-12, manufactured by Nippon Kayaku Co., Ltd.), 15.0 wt% of a dispersion of porous silica particles (average particle size: 50 nm, solid content: 20%, solvent: methyl isobutyl ketone), and 0.07 wt% of a photopolymerization initiator (manufactured by CIBA JAPAN, trade name: Irgacure 184) were diluted with 82 wt% of methyl isobutyl ketone as a solvent.
[0427] Table 5 shows the properties and evaluation results of the films having each antistatic layer.
[0428] It should be noted that the surface resistance value is the value of the antistatic layer surface, and the value in parentheses is the value of the antireflection layer surface.
[0429] [Table 5]
[0430]
[0431] Industrial Applicability
[0432] The present invention can provide an image display device that can suppress color spots and rainbow spots in the peripheral area of an image captured through the display panel even when the camera disposed below the display panel is used, thereby enabling high-quality capture of natural colors.
Claims
1. An image display device, wherein: In an image display device including a housing, an image display panel and a camera module, The camera module is disposed in a space formed by the housing and the image display panel in such a manner that a light receiving side of the camera module faces the image display panel. The image display panel has a back plate on the camera module side. The back plate has an anti-reflection layer or a low-reflection layer on the camera module side.
2. The image display device according to claim 1, wherein: The backplane has a substrate film and an anti-reflection layer or a low-reflection layer, and the in-plane retardation of the substrate film is 300 to 30000 nm.
3. The image display device according to claim 1 or 2, wherein: The back sheet has a reflectivity of 2% or less as measured from the anti-reflection layer or the low-reflection layer side.
4. The image display device according to any one of claims 1 to 3, wherein: The haze of the back sheet is less than 5%.
5. The image display device according to any one of claims 1 to 4, wherein: The back plate has an antistatic layer.
6. The image display device according to any one of claims 2 to 5, wherein: The angle formed by the slow axis direction of the substrate film of the backplane and the long side direction of the display screen of the image display device is 80 to 90 degrees on the acute angle side.
7. The image display device according to any one of claims 2 to 6, wherein: The in-plane retardation of the substrate film of the backplane is 2500 to 30000 nm, and the ratio (Re / Rth) of the in-plane retardation to the retardation in the thickness direction (Rth) is 0.3 to 1.
2.
8. The image display device according to any one of claims 2 to 7, wherein: The in-plane retardation of the substrate film of the backplane is 2500 to 30000 nm, and the NZ coefficient is 1.2 to 4.
0.
9. The image display device according to any one of claims 2 to 6, wherein: The in-plane retardation of the substrate film of the backplane is 300 to 9000 nm, and the ratio (Re / Rth) of the in-plane retardation to the retardation in the thickness direction (Rth) is less than 0.
5.
10. The image display device according to any one of claims 2 to 6 or claim 9, wherein: The in-plane retardation of the substrate film of the backplane is 300 to 9000 nm, and the NZ coefficient is greater than 2.
5.
11. The image display device according to any one of claims 1 to 10, wherein: When viewed from the camera module of the camera module, a polarizing plate is provided further away from the back plate.