Magnetic composite

By forming a dense spinel-type ferrite layer on a non-metal inorganic substrate, the problem of poor magnetic properties and difficult film thickness of magnetic composite materials in the prior art is solved, and high-frequency magnetic loss reduction and electrical power are achieved Magnetic composites suitable for insulation.

CN118974853APending Publication Date: 2024-11-15POWDERTECH CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202380032092.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-31
Filing Date
2023-03-09
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

In the prior art, the magnetic composite material formed on the substrate of the ferrite layer has problems such as poor magnetic properties, difficulty in forming a film thickness, easy peeling, and not suitable for electrically insulating applications.

Method used

A magnetic composite of a non-metallic inorganic substrate and spinel-type ferrite layer is used to control the crystallization state, crystal crystal diameter and resistivity of the ferrite layer to form a dense and thick ferrite layer, combined with aerosol The film formation is carried out by the deposition method to ensure the adhesion and heat resistance of the magnetic composite.

Benefits of technology

It realizes the density, thickness uniformity and high-frequency magnetic loss reduction of the magnetic composite, and is suitable for electronic equipment with electromagnetic wave absorption, shielding and electrical insulation requirements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118974853A_ABST
    Figure CN118974853A_ABST
Patent Text Reader

Abstract

Provided is a magnetic composite which is provided with a ferrite layer that is compact, has a relatively thick film thickness, has an effect of reducing magnetic loss at high frequencies, has excellent adhesion, and has excellent heat resistance. The magnetic composite includes a non-metallic inorganic base material and a ferrite layer provided on a surface of the non-metallic inorganic base material. The non-metallic inorganic base material has a thickness (dM) of 2.0 [mu] m or more. Furthermore, the ferrite layer has a thickness (dF) of 2.0 [mu] m or more and 50.0 [mu] m or less, and contains spinel ferrite as a main component. In addition, the content of alpha-Fe2O3 in the ferrite layer is from 3.0% by mass to 25.0% by mass (inclusive).
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to magnetic composites. Background Art

[0002] With the rapid development of electronic information and communication technology in recent years, the use of electromagnetic waves has also increased rapidly, and the high-frequency and wide-bandwidth electromagnetic waves used have gradually developed. Specifically, in addition to systems in the quasi-microwave band represented by mobile phones (1.5, 2.0GHz) or wireless LAN (2.45GHz), the introduction of new systems that use radio waves in the millimeter wave band, such as high-speed wireless LAN (65GHz) or anti-collision radar (76.5GHz), is developing.

[0003] As the use of electromagnetic waves expands and high frequencies develop, electromagnetic interference issues such as erroneous operation of electronic devices or adverse effects on the human body caused by electromagnetic noise are becoming more and more concerned, and expectations for EMC countermeasures are increasing. As one method of EMC countermeasures, it is known to use electromagnetic wave absorbers (radio wave absorbers) to absorb unnecessary electromagnetic waves and prevent them from intruding.

[0004] For electromagnetic wave absorbers, materials that exhibit conductive loss, dielectric loss, and / or magnetic loss are used. As materials that exhibit magnetic loss, ferrites with high magnetic permeability and high electrical resistance are often used. Ferrites resonate at specific frequencies, absorb electromagnetic waves, convert the absorbed electromagnetic wave energy into heat energy, and radiate it to the outside. As electromagnetic wave absorbers using ferrites, a composite material or a ferrite film containing ferrite powder and a binder resin has been proposed. In addition, in uses other than electromagnetic wave absorbers, a technology for forming a ferrite film on a substrate is known.

[0005] For example, Patent Document 1 describes that a coating composition containing 20 to 80% by mass of ferrite powder such as Mn-Zn ferrite, 3 to 60% by mass of carbon black powder, and the remainder being a resin is applied to at least one side of a metal plate to produce a coated metal plate (claims 1 to 6 of Patent Document 1). In addition, Patent Document 1 describes that the coating composition has excellent heat dissipation and good electromagnetic wave absorption performance in a wide frequency band (patent document 1,

[0060] ).

[0006] Patent document 2 discloses an electromagnetic wave absorber characterized by being obtained by physically vapor-depositing a ferromagnetic substance on a substrate composed of an organic polymer, and describes that the electromagnetic wave absorber has good electromagnetic wave absorption characteristics, is small, lightweight, flexible, and strong (claims 1 and

[0008] of patent document 2). In addition, patent document 2 describes that oxide-based soft magnetism is mainly used as the ferromagnetic substance, and ferrite is preferably used as the oxide-based soft magnetism, and physical vapor deposition methods include EB vapor deposition, ion plating, magnetron sputtering, opposed target magnetron sputtering, etc. (patent document 2

[0009] ,

[0010] , and

[0017] ).

[0007] Patent Document 3 discloses a composite magnetic film having an electromagnetic wave absorption function, which is composed of a magnetic phase and a high resistance phase, wherein the magnetic phase is composed of a metal magnetic body, and the high resistance phase is a highly insulating ferrite dispersed in the magnetic phase in an island shape (claim 1 of Patent Document 3). In addition, Patent Document 3 also describes that the composite magnetic film is formed by aerosolizing a raw material fine particle powder and causing it to collide with a substrate as a film-forming body, and adopting an aerosol deposition (AD) method for forming a thick film, and by applying the AD method, a composite magnetic film of a desired film thickness can be quickly formed (Patent Document 3,

[0029] and

[0033] ).

[0008] Patent document 4 discloses an electromagnetic wave absorber characterized by a composite body formed by dispersing metal particles in a ceramic matrix such as ferrite (claims 1 and 8 of patent document 4). In addition, patent document 4 states that: the electromagnetic wave absorber is often formed on a substrate for use, but in this case, if the substrate is metal, reflection occurs at the interface between the electromagnetic wave absorber and the substrate, and absorption can be expected again in the electromagnetic wave absorber, and a gas deposition method or an aerosol deposition method is used when manufacturing the electromagnetic wave absorber (patent document 4

[0029] and

[0031] ).

[0009] Thus, in Patent Documents 1 to 4, a scheme is proposed to form a ferrite-containing layer on a substrate such as a metal plate to produce an electromagnetic wave absorber. On the other hand, a scheme of forming a ferrite-containing layer on a substrate is also proposed for uses other than electromagnetic wave absorbers. For example, Patent Document 5 discloses an inductor element having: a magnetic substrate; a coil formed on the surface of the magnetic substrate by a conductor; and a magnetic layer formed by an aerosol deposition method on the magnetic substrate in a manner such that the coil is embedded (Claim 1 of Patent Document 5).

[0010] Prior art literature

[0011] Patent Literature

[0012] Patent Document 1: Japanese Patent Application Publication No. 2004-027064

[0013] Patent Document 2: Japanese Patent Application Publication No. 2005-045193

[0014] Patent Document 3: Japanese Patent Application Publication No. 2007-088121

[0015] Patent Document 4: Japanese Patent Application Publication No. 2007-180289

[0016] Patent Document 5: Japanese Patent Application Publication No. 2007-250924 Summary of the invention

[0017] Technical problem to be solved by the invention

[0018] Although it is proposed to apply the composite body made by forming a ferrite-containing layer on a substrate to the use of electronic devices represented by electromagnetic wave absorbers or inductors, there is still room for improvement in the prior art. For example, the composite material containing ferrite powder proposed in Patent Document 1 has poor magnetic properties because it contains a large amount of resin as a non-magnetic body. Therefore, there are limitations in improving the electromagnetic wave absorption characteristics. The ferrite film proposed in Patent Document 2 is difficult to form a thicker film in manufacturing, and there are still limitations in improving the magnetic properties. In addition, even if it can be formed into a thicker film, there is still a problem that the film is easily peeled off from the substrate. The composite body proposed in Patent Document 3 or Patent Document 4 cannot be used in applications requiring electrical insulation because it contains a highly conductive metal magnetic body. In addition, the element proposed in Patent Document 5 is also limited in achieving improvements in electrical properties or adhesion.

[0019] The inventors of the present invention conducted in-depth research in view of such problems. As a result, they obtained the following insights: in a magnetic composite having a non-metallic inorganic substrate and a ferrite layer, the crystal state of the ferrite layer is important, and by controlling it, a magnetic composite having a dense and relatively thick film, an effect of reducing magnetic loss at high frequencies, an excellent adhesion, and excellent heat resistance can be obtained.

[0020] The present invention has been accomplished based on such findings, and an object of the present invention is to provide a magnetic composite having a dense and relatively thick ferrite layer that has an effect of reducing magnetic loss at high frequencies and excellent adhesion, and also has excellent heat resistance.

[0021] Technical means for solving technical problems

[0022] The present invention includes the following aspects (1) to (8). In addition, in this specification, the expression "to" includes both numerical values. That is, "X to Y" and "X or more and Y or less" have the same meaning.

[0023] (1) A magnetic composite comprising a non-metallic inorganic substrate and a ferrite layer provided on a surface of the non-metallic inorganic substrate,

[0024] The non-metallic inorganic substrate has a thickness (d M ) is 2.0 μm or more,

[0025] The ferrite layer has a thickness (d F ) is 2.0 μm or more and 50.0 μm or less, and has spinel ferrite as the main component,

[0026] The content of α-Fe 2 O 3 in the ferrite layer is 3.0 mass % or more and 25.0 mass % or less.

[0027] (2) The magnetic composite according to (1) above,

[0028] The ferrite layer has an integrated intensity (I 222 ) relative to the (311) surface (I 311 ) ratio (I 222 / I 311 ) is greater than or equal to 0.00 and less than or equal to 0.03.

[0029] (3) The magnetic composite according to (1) or (2) above,

[0030] The ferrite layer contains iron (Fe) and oxygen (O), and contains at least one element selected from the group consisting of lithium (Li), magnesium (Mg), aluminum (Al), titanium (Ti), manganese (Mn), zinc (Zn), nickel (Ni), copper (Cu), and cobalt (Co).

[0031] (4) The magnetic composite according to any one of (1) to (3) above,

[0032] The ferrite layer has a surface arithmetic mean roughness (Ra) relative to its thickness (d F ) ratio (Ra / d F ) is higher than 0.00 and lower than 0.20.

[0033] (5) The magnetic composite according to any one of (1) to (4) above,

[0034] The ferrite layer has a composition including a ferrite constituent component and the remainder being inevitable impurities.

[0035] (6) The magnetic composite according to any one of (1) to (5) above,

[0036] The non-metallic inorganic substrate is composed of oxide.

[0037] (7) The magnetic composite according to any one of (1) to (5) above,

[0038] The non-metallic inorganic substrate is composed of glass.

[0039] (8) An element or component having a coil and / or inductor function, an electronic device, a housing for storing electronic components, an electromagnetic wave absorber, an electromagnetic wave shield, or an element or component having an antenna function,

[0040] A magnetic composite comprising any one of (1) to (7) above.

[0041] Effects of the Invention

[0042] According to the present invention, there is provided a magnetic composite having a dense and relatively thick ferrite layer that has an effect of reducing magnetic loss at high frequencies and excellent adhesion, and has excellent heat resistance. BRIEF DESCRIPTION OF THE DRAWINGS

[0043] Figure 1 One embodiment of a magnetic composite is shown.

[0044] Figure 2 Another embodiment of the magnetic composite is shown.

[0045] Figure 3 Other schemes of magnetic composites are shown.

[0046] Figure 4 An example in which a magnetic composite is applied to an inductor is shown.

[0047] Figure 5 An example of applying the magnetic composite to an LC filter is shown.

[0048] Figure 6 Another example of applying the magnetic composite to an inductor is shown.

[0049] Figure 7 An example of applying the magnetic composite to a magnetic sensor is shown.

[0050] Figure 8 An example of applying the magnetic composite to an electromagnetic wave absorber is shown.

[0051] Fig. 9 An example in which a magnetic composite is applied to a housing for housing electronic components is shown.

[0052] Fig.10 An example of the configuration of an aerosol deposition film-forming apparatus is shown.

[0053] Fig.11 The cross-sectional element mapping image of the ferrite layer obtained in Example 1 is shown.

[0054] Fig.12 The cross-sectional element mapping image of the ferrite layer obtained in Example 4 is shown. DETAILED DESCRIPTION

[0055] A specific embodiment of the present invention (hereinafter referred to as "this embodiment") will be described. The present invention is not limited to the following embodiment, and various modifications can be made within the scope of the present invention.

[0056] <<1. Magnetic composite>>

[0057] The magnetic composite of this embodiment includes a non-metallic inorganic substrate and a ferrite layer provided on the surface of the non-metallic inorganic substrate. The non-metallic inorganic substrate has a thickness (d M ) is 2.0 μm or more. The ferrite layer has a thickness (d F ) is 2.0 μm or more and 50.0 μm or less, and has spinel ferrite as a main component. In addition, the α-Fe2O3 content of the ferrite layer is 3.0 mass % or more and 25.0 mass % or less. The magnetic composite will be described in detail below.

[0058] The non-metallic inorganic substrate (sometimes simply abbreviated as "substrate") is composed of an inorganic material other than a metal, and functions as a support for the magnetic composite. As long as it functions as a support, the shape of the substrate is not particularly limited. For example, it can be plate-shaped, foil-shaped, rod-shaped, box-shaped, filament-shaped, or ribbon-shaped. In addition, as long as the substrate is composed of an inorganic material other than a metal, the material is not particularly limited. The substrate can be composed of an oxide, or it can also be composed of glass. Alternatively, the substrate can also be composed of nitrides, carbides, and / or semiconductor materials. The material of the substrate can be any of single crystal, polycrystalline, or amorphous. In addition, the substrate can be a single layer, or it can also be a laminate.

[0059] When the substrate is composed of an oxide, the characteristics of the oxide can be reflected in the magnetic composite. For example, when a highly insulating material represented by aluminum oxide is used as a substrate, a magnetic composite having the characteristics of high insulation can be produced. When a highly thermally conductive material such as sapphire is used as a substrate, a magnetic composite having excellent thermal conductivity or heat dissipation can be produced. By using these materials, the insulation or thermal conductivity of the magnetic composite can be improved. The substrate is particularly preferably an aluminum oxide substrate.

[0060] In the case where the substrate is composed of an oxide, the substrate may contain iron (Fe) or may not contain it. As a material that does not contain iron (Fe), dielectric materials such as aluminum oxide (Al2O3), titanium oxide (TiO2), barium titanate (BaTiO3), or strontium titanate (SrTiO3), or materials with high volume resistivity such as zirconium oxide (ZrO2) and artificial sapphire are preferred. As a material containing iron (Fe), a magnetic material having characteristics in magnetic properties, optical magnetic properties, and / or electrical properties, such as various ferrites or iron oxides, is preferred.

[0061] When the substrate is made of a semiconductor material, a Si substrate, a GaN substrate, or a SiC substrate is preferred. When the substrate is made of glass, a substrate made of quartz glass, soda glass, or borosilicate glass is preferred.

[0062] The thickness of the non-metallic inorganic substrate (d M ) is limited to more than 2.0μm. If the substrate is too thin, it is difficult to give sufficient strength to the magnetic composite. In other words, in order for the magnetic composite to maintain its shape stably, it is expected to have a thickness equal to that of the ferrite layer formed on the substrate. Therefore, the thickness of the substrate is preferably more than 2.0μm, more preferably more than 10μm, more preferably more than 50μm, and particularly preferably more than 100μm. On the other hand, the upper limit of the thickness is not limited. However, by appropriately thinning the substrate, the magnetic composite can be miniaturized and lightweight. The thickness can be less than 5000μm, less than 1000μm, less than 500μm, less than 200μm, less than 100μm, or less than 50μm. In addition, the substrate can be filamentous, ribbon-shaped, plate-shaped, or sheet-shaped. However, it is preferably sheet-shaped. In addition, the surface shape of the substrate is not limited. It can be flat or curved.

[0063] The thermal diffusivity of the non-metallic inorganic substrate is preferably 5×10 -6 m 2 / s or more, preferably 10×10 -6 m 2 / s. The higher the upper limit of thermal diffusivity, the better. However, in the scheme of placing the magnetic composite material in contact with other components, if the thermal conductivity or thermal diffusivity of the other components is low, even if the thermal diffusivity of the non-metallic inorganic substrate is high, there is a situation where heat cannot be dissipated. Therefore, an excessively high thermal diffusivity is not required. The thermal diffusivity of the non-metallic inorganic substrate is preferably 15000×10 -6 m 2 / s or less, preferably 5000×10 -6 m 2 / or less, and most preferably 2000×10 -6 m 2 / s.

[0064] The ferrite layer of the present embodiment is a polycrystal with spinel ferrite as the main component. That is, it is an aggregate of crystal particles composed of spinel ferrite. Spinel ferrite is a composite oxide of iron (Fe) having a spinel crystal structure, most of which exhibit soft magnetism. By having a layer with spinel ferrite as the main component, the magnetic properties of the magnetic composite are excellent. The type of spinel ferrite is not particularly limited. For example, at least one selected from the group consisting of manganese (Mn) ferrite, zinc (Zn) ferrite, manganese zinc (MnZn) ferrite, magnesium (Mg) ferrite, magnesium zinc (MgZn) ferrite, nickel (Ni) ferrite, nickel copper (NiCu) ferrite, nickel copper zinc (NiCuZn) ferrite, cobalt (Co) ferrite, and cobalt zinc (CoZn) ferrite is cited. In addition, in this specification, the so-called main component refers to a component with a content of 50.0 mass% or more. In order to utilize the excellent magnetic properties of spinel ferrite, the content of spinel ferrite (ferrite phase) in the ferrite layer is preferably 60.0 mass% or more, more preferably 70.0 mass% or more, further preferably 80.0 mass% or more, and particularly preferably 90.0 mass% or more.

[0065] The thickness (d F ) is limited to be not less than 2.0μm and not more than 50.0μm. If the ferrite layer is too thin, the film thickness of the ferrite layer is uneven, and the magnetic properties and electrical properties (electrical insulation) may deteriorate. The thickness is preferably not less than 3.0μm, and more preferably not less than 4.0μm. However, it is difficult to form a ferrite layer that is too thick while maintaining density. In addition, if the ferrite layer is too thick, the internal stress of the ferrite layer becomes too large, which may cause the ferrite layer to peel off or the substrate to break. Moreover, in the case where the miniaturization and lightweight of the magnetic composite are the goals, it is expected that the ferrite layer is appropriately thin. The thickness is preferably not more than 50.0μm, more preferably not more than 30.0μm, further preferably not more than 20.0μm, and particularly preferably not more than 10.0μm. In addition, when ferrite layers are provided on both sides of the substrate, the thickness of the single-sided ferrite layer is equivalent to d F .

[0066] The ferrite layer preferably has an integrated intensity (I 222 ) relative to the (311) surface (I 311 ) ratio (I 222 / I 311 ) is 0.00 or more and 0.03 or less (0.00≦I 222 / I 311≦0.03). That is, if the ferrite layer is analyzed by X-ray diffraction, the diffraction peak based on the (222) plane of the spinel phase is hardly observed in the X-ray diffraction distribution. This is because the crystal particles constituting the ferrite layer are composed of microcrystals. The crystal particles of the ferrite layer of this embodiment are subjected to plastic deformation when manufacturing the magnetic composite. Therefore, the crystallite diameter is small and the distribution of the lattice constant becomes wider. As a result, the XRD peak becomes wider and there is a tendency that the (222) diffraction peak is no longer observed. 222 / I 311 It is more preferably less than 0.02, and more preferably less than 0.01. In contrast, even in a polycrystalline state, the general spinel ferrite material has high crystallinity. Therefore, the (222) plane diffraction peak is observed to be relatively strong. Specifically, the XRD peak intensity ratio (I 222 / I 311 ) is about 0.04~0.05 (4~5%).

[0067] XRD peak intensity ratio (I 222 / I 311 ) The ferrite layer with a smaller diameter has the characteristic of being dense. The reason is that the crystal particles subjected to plastic deformation are easily filled finely. In addition, such a ferrite layer has the effect of excellent adhesion with the substrate. The reason is that the crystal particles are subjected to plastic deformation, thereby increasing the contact area with the substrate. In addition, it is also believed that the small crystallite diameter and the periodically disordered crystal structure lead to a stronger bond with the material constituting the substrate, which is also one of the reasons. In addition, such a ferrite layer has the characteristic of having a small magnetic loss (tanδ) in the high-frequency region above 500MHz. The small crystallite diameter leads to a shorter correlation length of the magnetic moment, and as a result, it is speculated that the magnetic domain wall movement in the high-frequency region proceeds smoothly. In contrast, in general spinel ferrite materials, the correlation length of the magnetic moment is considered to be longer. Therefore, in the low-frequency region, the magnetic domain wall movement caused by the external magnetic field can be carried out, but in the high-frequency region above 100MHz, the magnetic domain wall movement cannot follow the changes in the external magnetic field, and the magnetic loss becomes larger.

[0068] Preferably, the crystallite diameter of the ferrite layer is 1 nm or more and 10 nm or less. By reducing the crystallite diameter to less than 10 nm, the density and adhesion of the ferrite layer are higher, and the effect of suppressing the increase of magnetic loss is more significant. In addition, by setting the crystallite diameter to more than 1 nm, it is possible to prevent the ferrite layer from becoming amorphous and deteriorating the magnetic properties. The crystallite diameter is more preferably 1 nm or more and 5 nm or less, and more preferably 1 nm or more and 2 nm or less.

[0069] Preferably, the lattice constant of the spinel ferrite contained in the ferrite layer is above By setting the lattice constant to above The following results show that the magnetic properties of the raw material particles are improved. The lattice constant is preferably above The following are more preferably above the following.

[0070] Preferably, the thickness of the ferrite layer (d F ) relative to the thickness of the non-metallic inorganic substrate (d M ) ratio (d F / d M ) is 0.0004 or more and 1 or less (0.0004≦d F / d M ≦1). If the thickness ratio (d F / d M ) is too small, the film thickness of the ferrite layer is uneven, and the magnetic and electrical properties (electrical insulation) are reduced. F / d M ) is preferably 0.004 or more. On the other hand, if the thickness ratio (d F / d M ) is too large, the substrate cannot resist the internal stress of the ferrite layer, and the composite may bend or break. F / d M ) is more preferably 0.1 or less, more preferably 0.02 or less, and particularly preferably 0.01 or less.

[0071] When the substrate has irregularities, the arithmetic mean of the thinnest part and the thickest part of the substrate on which the ferrite layer is formed is taken as the thickness d of the substrate. M , the arithmetic mean of the thinnest and thickest parts of the composite and the thickness d of the substrate M The difference is the thickness of the ferrite layer d F . The thickness of the substrate d M If the thickness of the substrate exceeds 5000 μm, M Assuming it is 5000 μm, calculate the thickness ratio (d F / d M ).

[0072] The content of α-Fe2O3 (hematite) in the ferrite layer of the present embodiment is not less than 3.0 mass % and not more than 25.0 mass %. α-Fe2O3 is free iron oxide that has not become a spinel phase. Unlike the spinel phase of a ferromagnetic body, α-Fe2O3 is an antiferromagnetic body. Therefore, if there is too much α-Fe2O3, the magnetic properties of the ferrite layer may deteriorate. The amount of α-Fe2O3 is preferably less than 23.0 mass %, and more preferably less than 21.0 mass %. On the other hand, α-Fe2O3 is a stable compound with high resistance. By appropriately containing α-Fe2O3 in the ferrite layer, the conductive path in the ferrite layer can be cut off, and the resistance can be further increased. In particular, manganese (Mn) ferrites or manganese-zinc (MnZn) ferrites contain manganese (Mn) ions and iron (Fe) ions with unstable valence numbers, so the resistance tends to decrease. Therefore, by making these ferrites contain α-Fe2O3, the effect of improving resistance can be significantly exerted. In addition, by making it contain α-Fe2O3 appropriately, the densification of the ferrite layer and the improvement of the adhesion can be achieved. α-Fe2O3 is produced in the ferrite layer film forming process when manufacturing the magnetic composite. That is, during the film forming process, plastic deformation and reoxidation of the ferrite crystal particles are caused to generate α-Fe2O3. This plastic deformation and reoxidation play an important role in improving the densification and adhesion of the ferrite layer. Therefore, the density and adhesion of the ferrite layer that contains α-Fe2O3 appropriately are high. The amount of α-Fe2O3 is preferably 3.0 mass% or more, more preferably 5.0 mass% or more, further preferably 10.0 mass% or more, and especially preferably 15.0 mass% or more.

[0073] Preferably, the ferrite layer contains iron (Fe) and oxygen (O), and further contains at least one element selected from the group consisting of lithium (Li), magnesium (Mg), aluminum (Al), titanium (Ti), manganese (Mn), zinc (Zn), nickel (Ni), copper (Cu), and cobalt (Co). The elements contained in the ferrite layer can be confirmed using an analysis method or analysis device such as ICP, EDX, SIMS, and XRF.

[0074] Preferably, the ferrite layer has a surface arithmetic mean roughness (Ra) relative to the thickness (d F ) ratio (Ra / d F ) is higher than 0.00 and lower than 0.20 (0.00<Ra / d F ≦0.20). If the roughness ratio (Ra / d F ) is too large, the thickness of the ferrite layer tends to be uneven. Therefore, when a high voltage is applied, the electric field is locally concentrated, which may cause leakage current. F ) is more preferably higher than 0.00 and lower than 0.10, and further preferably higher than 0.00 and lower than 0.05.

[0075] The density of the ferrite layer of this embodiment is relatively high. This is because the ferrite crystal particles constituting the ferrite layer are repeatedly subjected to plastic deformation, resulting in the deposition of small crystal particles in a manner that forms a ferrite layer. The relative density of the ferrite layer is preferably greater than 0.60, more preferably greater than 0.70, even more preferably greater than 0.80, and particularly preferably greater than 0.90. By increasing the density, the effect of improving the magnetic properties, electrical properties, and adhesion of the ferrite layer is more significant.

[0076] The ferrite layer of this embodiment has a relatively high resistance. This is because the ferrite layer has a high density, so the adsorption of conductive components such as water, which is a factor that deteriorates the resistance, is small. In addition, it is also considered that the small crystallite diameter of the ferrite crystal particles constituting the ferrite layer also has an effect. In fact, the general MnZn ferrite material has a relatively low resistance, and its volume resistance is 10 4 ~10 5 Ω·cm. In contrast, the ferrite layer of this embodiment shows a higher resistance value than that, and the reason can be found in the size of the crystallite diameter. And by containing an appropriate amount of α-Fe2O3, the resistance of the ferrite layer can be further increased. The surface resistance of the ferrite layer is preferably 10 4 Ω or more, preferably 10 5 Ω or more, more preferably 10 7 By increasing the surface resistance, the insulation of the ferrite layer can be improved, and when the magnetic composite is applied to a device, problems such as the generation of eddy current can be suppressed.

[0077] The ferrite layer preferably has a composition containing ferrite constituents, and the remainder is an inevitable impurity. That is, it is preferred to contain organic components or inorganic components other than the ferrite constituents without exceeding the amount of inevitable impurities. The ferrite layer of the present embodiment can become sufficiently dense even without adding resin components such as binders or inorganic additives such as sintering aids. By suppressing the content of non-magnetic materials to a minimum, the excellent magnetic properties based on ferrite can be fully utilized. In addition, the so-called ferrite constituents are components that constitute spinel ferrite as a main component. For example, in the case where the ferrite layer is mainly composed of manganese-zinc (MnZn) ferrite, the ferrite constituents are iron (Fe), manganese (Mn), zinc (Zn) and oxygen (O). In the case where the ferrite layer is mainly composed of nickel-copper-zinc (NiCuZn) ferrite, the ferrite constituents are iron (Fe), nickel (Ni), copper (Cu), zinc (Zn) and oxygen (O). The unavoidable impurities are components that are inevitably mixed during production, and the content thereof is typically 1000 ppm or less. In particular, the ferrite layer preferably does not contain any metal component other than oxide.

[0078] The magnetic composite is preferably manufactured by the following method, comprising: a step of preparing a non-metallic inorganic substrate and a spinel ferrite powder having an average particle size (D50) of not less than 2.5 μm and not more than 10.0 μm (preparation step); and a step of forming a film of the ferrite powder on the surface of the non-metallic inorganic substrate by an aerosol deposition method (film forming step), wherein the ratio (LCf / LCp) of the lattice constant (LCf) of the spinel phase contained in the ferrite layer to the lattice constant (LCp) of the spinel phase contained in the spinel ferrite powder is not less than 0.95 and not more than 1.05 (0.95≦LCf / LCp≦1.05).

[0079] The form of the magnetic composite is not particularly limited. Figure 1 As shown in FIG. 1 , a ferrite layer (ferrite film) may be provided on the entire surface of a non-metallic inorganic substrate. Figure 2 As shown in FIG. 1 , it is also possible to provide the ferrite layer only on a portion of the surface of the substrate. It is also possible to provide the ferrite layer not only on one side of the substrate but also on both sides. Figure 3 As shown in FIG. 1 , a ferrite layer having a locally varying thickness may be provided on the surface of the substrate.

[0080] The magnetic composite can be used in various applications, such as components or parts having coil and / or inductor functions, electronic devices, electronic component storage housings, electromagnetic wave absorbers, electromagnetic wave shields, or components or parts having antenna functions.

[0081] exist Figure 4 An example of applying a magnetic composite to an inductor is shown in . The magnetic composite includes: a non-metallic inorganic substrate; a ferrite layer (ferrite film) disposed on the surface of the substrate; a coil layer disposed on the surface of the ferrite layer; a substrate-side electrode disposed on the back side of the substrate; and a through electrode connecting the coil layer and the substrate-side electrode. The substrate can be determined according to the application purpose. The coil layer is formed of a conductive material such as a metal and has a spiral circuit pattern. Therefore, the inductor function is exerted. The circuit pattern of the coil can be formed by electroless plating, screen printing using a paste containing metal colloidal particles, inkjet, sputtering, evaporation, etc. By forming a circuit pattern on the ferrite layer, a thin element having an inductor function can be obtained.

[0082] exist Figure 5An example of applying a magnetic composite to an LC filter is shown in . The magnetic composite includes: a non-metallic inorganic substrate; a ferrite layer (ferrite film) provided on a portion of the surface of the substrate; and a coil layer provided on the surface of the ferrite layer. On the other hand, a capacitor electrode is provided at a position on the surface of the substrate where the ferrite layer is not provided. In addition, a substrate-side electrode is provided on the back side of the substrate, and the substrate sandwiched by the capacitor electrode and the substrate-type electrode works as a dielectric. The portion where the ferrite layer is provided functions as an inductor element, and the substrate (dielectric) sandwiched by the capacitor electrode and the substrate-side electrode functions as a capacitor element. Moreover, they operate as an LC filter as a whole.

[0083] exist Figure 6 , another example of applying a magnetic composite to an inductor is shown in FIG. In this example, a ferrite layer (ferrite film) and a coil layer are provided on both sides of a non-metallic inorganic substrate. In addition, the coil layer on the surface side and the coil layer on the back side are electrically connected via through electrodes provided on the substrate and the ferrite layer. By giving the inductor function to both sides of the substrate, a miniaturized inductor can be produced.

[0084] exist Figure 7 An example of applying a magnetic composite to a magnetic sensor is shown in . In this example, an inductor element having a ferrite layer (ferrite film) and a coil layer is arranged in a matrix on both sides of a non-metallic inorganic substrate. When the magnetic sensor is in operation, under the condition of applying an external AC magnetic field, the voltage generated by each combination of the horizontal inductor electrodes A and B... (horizontally) arranged on the back side of the substrate and the vertical inductor electrodes a, b, c... arranged on the surface of the substrate is measured in sequence. In the absence of a magnetic body near the coil, the inductance shown by the inductor on the surface of the substrate and the inductor on the back side is the same, so no voltage is generated. In the presence of a magnetic body, the inductance of the inductor near the magnetic body changes, so a voltage is generated. According to the combination of inductors that generate voltage, the position of the magnetic body can be detected.

[0085] exist Figure 8 An example of applying a magnetic composite to an electromagnetic wave absorber is shown in FIG. The electromagnetic wave absorber (magnetic composite) has a structure in which a non-metallic inorganic substrate is saturated and a ferrite layer (ferrite film) is alternately stacked on the surface of the substrate. In addition, the bottom non-metallic inorganic substrate is composed of a substrate with excellent thermal conductivity.

[0086] exist Fig. 9An example of applying a magnetic composite to a housing for storing electronic components is shown in FIG. In this example, a ferrite layer (ferrite film) is provided on the surface of a non-metallic inorganic substrate, and electronic components are mounted thereon. In addition, a ferrite layer is also provided on the inner side of the substrate serving as a cover of the housing. By providing a ferrite layer having an electromagnetic wave shielding effect in the housing, it is possible to prevent the leakage of unnecessary electromagnetic waves radiated from the electronic components to the surrounding environment.

[0087] <<2. Method for producing magnetic composite>>

[0088] The manufacturing method of the magnetic composite of this embodiment is not limited as long as the above conditions are met. However, the preferred manufacturing method comprises the following steps: a step of preparing a non-metallic inorganic substrate and a spinel ferrite powder having an average particle size (D50) of 2.5 μm or more and 10.0 μm or less (preparation step); and a step of forming a film of the ferrite powder on the surface of the non-metallic inorganic substrate by aerosol deposition (film forming step).

[0089] In this way, by using ferrite powder with a specific particle size as a raw material and forming a film by an aerosol deposition method (AD method), a relatively thick ferrite layer can be produced at a higher film forming speed. The ferrite layer is dense, has excellent magnetic and electrical properties, and has excellent adhesion to the substrate. Therefore, it is preferred as a method for manufacturing a magnetic composite. Each process is described in detail below.

[0090] <Preparation process>

[0091] In the preparation process, a non-metallic inorganic substrate and spinel ferrite powder are prepared. The details of the substrate are as described above. On the other hand, as the spinel ferrite powder, a powder having an average particle size (D50) of 2.5 μm to 10.0 μm is prepared. The average particle size is preferably 2.5 μm to 9.0 μm, more preferably 2.5 μm to 7.0 μm. By adjusting the average particle size within the above range, a dense and highly adhesive ferrite layer can be obtained through a subsequent film-forming process.

[0092] The method for producing ferrite powder is not limited. However, preferably, the ferrite raw material mixture is formally fired in an atmosphere with an oxygen concentration lower than that of the atmosphere to produce a fired product, and the fired product is crushed to produce irregular particles of a specific particle size. In addition, before firing, the ferrite raw material mixture may also be subjected to pre-firing, crushing, and / or granulation. As the ferrite raw material, known ferrite raw materials such as oxides, carbonates, and hydroxides may be used.

[0093] The shape of the ferrite powder is preferably amorphous. Specifically, the average value of the shape factor (SF-2) of the ferrite powder is preferably 1.02 to 1.50, more preferably 1.02 to 1.35, and even more preferably 1.02 to 1.25. Here, SF-2 is an index indicating the degree of amorphousness of the particles, and the closer it is to 1, the more circular it is, and the larger it is, the more amorphous it is. If SF-2 is too small, the particles become too round. Therefore, the adhesion of the particles to the substrate becomes worse, and the film forming rate cannot be increased. On the other hand, if SF-2 is too large, the unevenness on the particle surface becomes too large. Therefore, although the film forming rate is increased, voids are likely to remain in the obtained ferrite layer due to the unevenness on the particle surface. If SF-2 is within the above range, a dense ferrite layer can be obtained at a high film forming rate. In addition, SF-2 is obtained according to the following formula (1).

[0094] [Formula 1]

[0095]

[0096] In addition, the average value of the aspect ratio of the ferrite powder is preferably greater than 1.00 and less than 2.00, more preferably greater than 1.20 and less than 1.85, and even more preferably greater than 1.40 and less than 1.70. If the aspect ratio is within the above range, the gas flow supplying the raw material during film formation is stable. On the other hand, if it is higher than the above range, the raw material is easily clogged in the piping from the raw material supply container to the nozzle. Therefore, as the film formation time passes, the film formation speed may become unstable. In addition, the aspect ratio is calculated according to the following formula (2).

[0097] [Formula 2]

[0098]

[0099] Furthermore, the CV value of the particle size of the ferrite powder is preferably not less than 0.5 and not more than 2.5. Here, the CV value indicates the degree of deviation of the particle size in the powder, and the more uniform the particle size, the smaller it is, and the more non-uniform it is, the larger it is. If a general pulverization method (bead mill, jet mill, etc.) is used to obtain amorphous particles, it is difficult to obtain a powder with a CV value lower than 0.5. On the other hand, a powder with a CV value higher than 2.5 tends to clog the piping from the raw material supply container to the nozzle. Therefore, as the film formation time passes, the film formation speed may become unstable. In addition, the CV value is obtained using the 10% cumulative diameter (D10), 50% cumulative diameter (D50; average particle size), and 90% cumulative diameter (D90) in the volume particle size distribution according to the following formula (3).

[0100] [Formula 3]

[0101]

[0102] When pre-firing is performed when ferrite powder is made, for example, pre-firing can be performed under the condition of 500-1100°C × 1-24 hours in an atmospheric atmosphere. The formal firing can be performed under the condition of 800-1350°C × 4-24 hours in an atmosphere such as an atmospheric atmosphere or a reducing atmosphere. In addition, the oxygen concentration during the formal firing is preferably low. As a result, lattice defects can be purposefully generated in the spinel crystals of the ferrite powder. When lattice defects are included in the crystal, when the raw material particles collide with the substrate in the subsequent film forming process, it is easy to cause plastic deformation starting from the lattice defects. Therefore, a dense and highly adhesive ferrite layer can be easily obtained. The oxygen concentration is preferably 0.001-10% by volume, more preferably 0.001-5% by volume, and even more preferably 0.001-2% by volume. When the ferrite contains copper (Cu), it is preferably fired in an atmosphere in which oxygen is present other than a reducing atmosphere. Even when firing is performed in an atmosphere other than a reducing atmosphere in which oxygen is present, copper (II) oxide (CuO) releases a portion of oxygen atoms due to the ionization tendency of copper, and changes into copper (I) oxide (Cu2O). At this time, lattice defects are easily generated. In addition, by making the ferrite powder a component rich in iron (Fe), it is also effective in obtaining a dense ferrite layer.

[0103] The pulverization of the fired product is preferably carried out using a pulverizer such as a dry bead mill. Through dry pulverization, the fired product is subjected to mechanochemical treatment, the crystallite diameter becomes smaller, and the surface activity increases. The high surface activity of the pulverized powder combined with the appropriate particle size effect helps to densify the ferrite layer obtained in the subsequent film forming process. The crystallite diameter (CSp) of the ferrite powder is preferably above By using ferrite powder having a fine crystallite diameter, a dense ferrite layer can be obtained.

[0104] <Film forming process>

[0105] In the film forming process (deposition process), the ferrite powder is formed into a film on the surface of the non-metallic inorganic substrate by an aerosol deposition method. The aerosol deposition method (AD method) is a method of forming a film by spraying aerosolized raw material particles onto a substrate at high speed and utilizing the normal temperature impact curing phenomenon. Since the normal temperature impact curing phenomenon is utilized, it is possible to form a dense film with high adhesion. In addition, since the particles are used to supply the raw materials, a thick film can be obtained at a high film forming speed compared to thin film forming methods such as sputtering or evaporation methods that separate the raw materials to the atomic level. Furthermore, since normal temperature film formation can be performed, there is no need to complicate the structure of the device, and there is also an effect of reducing manufacturing costs.

[0106] exist Fig.10An example of the structure of an aerosol deposition film-forming device is shown in the figure. The aerosol deposition film-forming device (20) includes an aerosolization chamber (2), a film-forming chamber (4), a transmission gas source (6), and a vacuum exhaust system (8). The aerosolization chamber (2) includes a vibrator (10) and a raw material container (12) arranged thereon. A nozzle (14) and a stage (16) are provided inside the film-forming chamber (4). The stage (16) is configured to be movable vertically relative to the injection direction of the nozzle (14).

[0107] During film formation, a transport gas is introduced from a transport gas source (6) into a raw material container (12), and a vibrator (10) is activated. Raw material particles (ferrite powder) are placed in the raw material container (12). The raw material particles are mixed with the transport gas by vibration and aerosolized. In addition, the film forming chamber (4) is evacuated by a vacuum exhaust system (8), and the pressure in the chamber is reduced. The aerosolized raw material particles are transported to the inside of the film forming chamber (4) by a pressure difference and ejected from a nozzle (14). The ejected raw material particles collide with the surface of a substrate (base material) placed on a stage (16) and accumulate there. At this time, in the raw material particles accelerated by gas transport, when they collide with the substrate, kinetic energy is locally released, and bonding between substrate and particles and between particles and particles is achieved. Therefore, a dense film can be formed. During film formation, by moving the stage (16), a film that extends in the surface direction can be formed.

[0108] As a reason for obtaining a dense ferrite layer by the manufacturing method of this embodiment, it is speculated in the following manner. That is, ceramics are generally referred to as materials with high elastic boundaries and not easy to plastically deform. However, it is believed that when the film is formed by the aerosol deposition method, when the raw material particles collide with the substrate at high speed, the impact force is greater than the elastic boundary, so the particles will be plastically deformed. Specifically, defects such as crystal plane dislocation or dislocation movement are generated inside the particles. In order to compensate for the defects, plastic deformation occurs and the crystal structure becomes finer. In addition, a new surface is formed and material movement occurs. It is believed that they act in combination, and as a result, the bonding force between the substrate and the particles and between the particles increases, and a dense film is obtained. And it is believed that during plastic deformation, part of the ferrite is decomposed and reoxidized to generate α-Fe2O3 that contributes to high resistance. In addition, it is also speculated that the particles that collide with the substrate as the substrate at the initial stage of film formation may invade the substrate, and the intruding particles show an anchoring effect, thereby increasing the adhesion between the ferrite layer and the substrate.

[0109] In terms of obtaining a dense ferrite layer, the average particle size of the raw ferrite powder is very important. In the present embodiment, the average particle size (D50) of the ferrite powder is limited to 2.5 μm or more and 10.0 μm or less. When the average particle size is less than 2.5 μm, it is difficult to obtain a dense film. This is because the mass of the crystal grains constituting the powder with a small average particle size is small. The aerosolized raw material particles collide with the substrate at high speed together with the transport gas. The transport gas that collides with the substrate changes its direction and flows away as exhaust gas. Particles with small particle size and small mass are rushed into the exhaust flow of the transport gas, and the collision speed on the substrate surface and the impact force it brings are reduced. When the impact force is small, the plastic deformation of the particles becomes insufficient, and the crystallite diameter does not decrease. The film after film formation will not become dense, and it will become a compressed powder body in which only the powder is compressed. Such a compressed powder body contains multiple pores inside, and the magnetic and electrical properties are deteriorated. Moreover, the adhesion with the substrate is not high. On the other hand, when the average particle size is too large, exceeding 10.0 μm, although the impact force on one particle is large, the number of contact points between particles decreases, so plastic deformation and packaging become insufficient, and it becomes difficult to obtain a dense film.

[0110] The film forming conditions of the aerosol deposition method are not particularly limited as long as a dense and highly adhesive ferrite layer can be obtained. As a transport gas, air or an inert gas (nitrogen, argon, helium, etc.) can be used. However, an atmosphere that is easy to handle is preferred. The flow rate of the transport gas can be, for example, 1.0 to 20.0 L / min. In addition, the internal pressure of the film forming chamber is, for example, 10 to 50 Pa before film formation and 50 to 400 Pa during film formation. The scanning speed (moving speed) of the non-metallic inorganic substrate (stage) can be, for example, 1.0 to 10.0 mm / second. Coating (film formation) can be performed only once or multiple times. However, from the viewpoint of fully ensuring the film thickness of the obtained ferrite layer, it is preferably performed multiple times. The number of coatings is, for example, more than 5 times and less than 100 times.

[0111] The ratio (LCf / LCp) of the lattice constant (LCf) of the spinel phase contained in the ferrite layer to the lattice constant (LCp) of the spinel phase contained in the raw ferrite powder is preferably 0.95 or more and 1.05 or less (0.95≦LCf / LCp≦1.05). The spinel phase in the raw ferrite powder is a composition lacking oxygen and has lattice defects. Therefore, the lattice constant is large compared to a state in which there are no lattice defects. On the other hand, after the raw ferrite powder is subjected to aerosol deposition film forming treatment, plastic deformation starting from the lattice defects is caused. In addition, plastic deformation leads to the formation of active surfaces, and the active surfaces are oxidized. Due to the reconstruction of the crystal structure and the reoxidation of the active surfaces, the lattice constant changes. By controlling the lattice constant ratio (LCf / LCp) within the above range, the amount of α-Fe2O3 accompanying the reconstruction of the crystal structure and the reoxidation of the active surface can be adjusted within a desired range, and as a result, a ferrite layer can be formed that maintains excellent magnetic properties and has excellent electrical properties (electrical insulation). The lattice constant ratio (LCf / LCp) is preferably greater than 0.99 and less than 1.04.

[0112] The degree of change in lattice constant varies depending on the manufacturing conditions or composition of the raw material ferrite powder, and the material and type of the substrate. Specifically, when the ferrite component is a stoichiometric component or an iron (Fe)-rich component (M x Fe 3-x O4: 0<x≦1, M is a metal atom), although it also depends on the firing conditions, the amount of oxygen contained in the raw ferrite powder is likely to be substantially smaller than the stoichiometric ratio. Therefore, the lattice constant of the raw ferrite powder tends to become larger. On the other hand, in the ferrite layer formed by the AD method, the crystal structure is reconstructed by oxidation accompanied by plastic deformation of the raw material particles, so the lattice constant tends to be smaller than the raw ferrite powder. This tendency is particularly significant when using ferrite powder containing lithium (Li) or manganese (Mn) or firing ferrite powder at an oxygen concentration lower than that of the atmosphere. Therefore, at this time, LCf / LCp tends to be less than 1.00.

[0113] The stoichiometric ratio of Fe to ferrite (M x Fe 3-x O4:1<x, M is a metal atom), the amount of oxygen contained in the ferrite is the same as the stoichiometric ratio. In addition, in the ferrite layer formed by the AD method, the lattice defects caused by plastic deformation increase, so the lattice constant tends to become larger. In particular, when using ferrite powder containing Cu or ferrite powder fired in an atmospheric atmosphere, this tendency is more significant. Therefore, at this time, LCf / LCp tends to be higher than 1.00.

[0114] The lattice constant ratio (LCf / LCp) can also be adjusted by controlling the conditions of aerosol deposition film formation. That is, by increasing the collision speed of the raw material particles, the deformation and reoxidation can be promoted. The collision speed of the raw material particles can be changed by adjusting the pressure in the chamber, etc. In addition, by changing the film formation speed, excessive reoxidation can be prevented. Since reoxidation progresses from the surface of the raw material particles, if the film formation speed of the ferrite layer is increased and the exposure time of the raw material particles to the atmosphere is shortened, the progress of reoxidation is suppressed.

[0115] The ratio (CSf / CSp) of the crystallite diameter (CSf) of the spinel phase contained in the ferrite layer to the crystallite diameter (CSp) of the spinel phase contained in the raw ferrite powder is preferably 0.01 or more and 0.50 or less (0.01≦CSf / CSp≦0.50). After aerosol deposition film formation, the crystallite diameter of the ferrite will change. This is because deformation occurs when colliding with the substrate, and the active surface is reoxidized. Even if the film is formed under the condition that the crystallite diameter ratio (CSf / CSp) is excessively reduced, a dense and highly adhesive ferrite layer cannot be obtained. This is because the internal stress of the ferrite layer is too large. In addition, even if the film can be formed, the ferrite layer is easily peeled off due to the internal stress. Therefore, there is a lack of stability over time. The crystallite diameter ratio (CSf / CSp) is preferably 0.05 or more and 0.30 or less, and more preferably 0.10 or more and 0.20 or less.

[0116] In this way, the magnetic composite of the present embodiment can be obtained. In the obtained magnetic composite, the ferrite layer is dense, so the magnetic properties and electrical properties (electrical insulation) are excellent. And the adhesion with the substrate is high. In fact, the inventors of the present invention have succeeded in the production of a magnetic composite having a ferrite layer with a relative density of more than 0.89 and an adhesion of more than 10H in pencil hardness. In addition, the magnetic loss of the ferrite layer in the high-frequency region is relatively small. On this basis, although not limited, by using a thin-layered substrate, the miniaturization and lightweight of the magnetic composite can be achieved. The magnetic composite having such a ferrite layer can be used not only in electromagnetic wave absorbers, but also in electronic components such as transformers, inductors, and impedance devices, and is particularly preferably used in UHF tags, 5G filters, and high-frequency inductors.

[0117] The technology for making such a magnetic composite of the present embodiment has not been known in the past within the scope of the knowledge of the inventors of the present invention. For example, the composite material including ferrite powder proposed in Patent Document 1 has poor magnetic properties because it contains a large amount of resin as a non-magnetic body. In addition, the ferrite film proposed in Patent Document 2 is difficult to form a thicker film in manufacturing. Furthermore, the composite magnetic body proposed in Patent Document 3 cannot be used in applications requiring electrical insulation because it contains a highly conductive metal magnetic body. In the magnetic composite of the present embodiment, the ferrite layer does not contain resin or metal components, and can be fully used in applications requiring electrical insulation.

[0118] In addition, Patent Document 3 discloses that the content of iron powder (metallic magnetic body) is set to 0% to produce a composite magnetic film (Patent Document 3,

[0048] ). However, there is a peak of the (222) plane in the X-ray diffraction distribution (Patent Document 3,

[0049] ). Figure 3 ), the ferrite layer in the magnetic film is not in a microcrystalline state, and it is inferred that the density and adhesion are poor. In addition, in Patent Document 3, NiZn ferrite or MnZn ferrite, etc., and α-Fe2O3 are exemplified as ferrite raw materials (Patent Document 3

[0036] ). However, Patent Document 3 does not teach that a specified amount of α-Fe2O3 is contained in the ferrite layer, and that the resistance is increased by cutting off the conductive path in the ferrite layer. In fact, when α-Fe2O3 is used as a raw material, the ferrite layer will contain coarse α-Fe2O3, which hinders the movement of the magnetic domain wall of the ferrite component, and as a result, becomes a factor in the deterioration of magnetic properties.

[0119] Example

[0120] The present invention will be described in more detail using the following examples, but the present invention is not limited to the following examples.

[0121] (1) Preparation of magnetic composite

[0122] [Example 1]

[0123] In Example 1, ferrite powder containing MnZn ferrite as the main component was prepared, and the obtained ferrite powder was formed into films on the front and back of a glass substrate (non-metallic inorganic substrate) with a thickness of 1000 μm to prepare a magnetic composite. The preparation of ferrite powder and film formation were carried out in the following order.

[0124] <Production of ferrite powder>

[0125] As raw materials, iron oxide (Fe2O3), manganese tetraoxide (Mn3O4) and zinc oxide (ZnO) were weighed and mixed in a molar ratio of Fe2O3:Mn3O4:ZnO=53:12.3:10. The mixing was performed using a Henschel mixer. The obtained mixture was molded using a roller compactor to obtain a granulated product (pre-granulated product).

[0126] Next, the granulated raw material mixture (pre-granulated product) is pre-fired to produce a pre-fired product. The pre-fired product is pre-fired using a rotary kiln at 880° C. for 2 hours in an air atmosphere.

[0127] Thereafter, the obtained calcined product was crushed and granulated to produce a granulated product (formal granulated product). First, a dry bead mill (3 / 16 inch The pre-sintered product was coarsely pulverized, and then water was added and the product was milled using a wet bead mill ( The zirconia beads) were finely ground and slurried. The solid content concentration of the obtained slurry was 50% by mass, and the particle size of the crushed powder (slurry particle size) was 2.15 μm. In the obtained slurry, a polycarboxylic acid ammonium salt was added as a dispersant at a ratio of 50 cc relative to 25 kg of solid content in the slurry, and a 10% by mass aqueous solution of polyvinyl alcohol (PVA) was added as a binder at an addition amount of 500 cc. Thereafter, the slurry to which the dispersant and the binder were added was granulated using a spray dryer to obtain a formal granulated product.

[0128] Then, the obtained granulated product was fired at 1250°C for 4 hours in a non-oxidizing atmosphere using an electric furnace (main firing) to produce a fired product. Next, the fired product was crushed using a hammer crusher and further crushed using a dry bead mill (3 / 16 inch The raw material was passed through a bead mill twice at a blade circumferential speed of 6.5 m / sec and a raw material supply rate of 5.0 kg / h to produce a pulverized and fired product having a volume average particle size (D50) of 5.0 μm.

[0129] <Film Formation>

[0130] The obtained pulverized fired product is used to form a ferrite layer on the surface and back of a non-metallic inorganic substrate. As a substrate, a glass substrate with a thickness of 1000 μm is used. In addition, the film formation is carried out by an aerosol deposition (AD) method according to the following conditions. In addition, the film formation is carried out 12 times on the surface and back of the substrate, respectively, and the film is formed on the glass substrate under the same conditions in such a way that two types of ferrite layers (ferrite films) of annular and rectangular shapes are obtained.

[0131] -Carrier gas (transmission gas): air

[0132] -Gas flow rate: 2.5L / min

[0133] -Pressure in film forming chamber (before film forming): 30Pa

[0134] -Pressure in film forming chamber (during film forming): 100Pa

[0135] -Substrate scanning speed: 6mm / sec

[0136] -Number of applications: 12 times + 12 times

[0137] - Distance from substrate to nozzle: 20mm

[0138] -Nozzle shape: 10mm×0.4mm

[0139] -Membrane shape: ring, rectangle

[0140] [Example 2]

[0141] In Example 2, an alumina (Al2O3) substrate with a thickness of 635 μm was used as the inorganic substrate. In addition, a film was formed on the alumina substrate under the same conditions in such a manner that two types of ferrite layers (ferrite films) of annular and rectangular shapes were obtained. A magnetic composite was prepared in the same manner as in Example 1.

[0142] [Example 3]

[0143] In Example 3, a raw material powder (ferrite powder) containing NiCuZn-based ferrite as a main component was prepared, and then the obtained ferrite powder was formed into a film on the front and back surfaces of a glass substrate (non-metallic inorganic substrate) with a thickness of 1000 μm to produce a magnetic composite. The preparation of the ferrite powder and the film formation were carried out in the following order.

[0144] As raw materials, iron oxide (Fe2O3), zinc oxide (ZnO), nickel oxide (NiO) and copper oxide (CuO) were used, and the raw materials were weighed and mixed in a molar ratio of Fe2O3: ZnO: NiO: CuO = 48.5: 29.25: 16: 6.25. In addition, pre-firing was performed at 850°C × 2 hours in an air atmosphere, and formal firing was performed at 1100°C × 4 hours in an oxidizing atmosphere. In addition, the film formation was performed 36 times on the surface and back of the substrate. The magnetic composite was prepared in the same manner as in Example 1.

[0145] [Example 4]

[0146] In Example 4, an alumina (Al2O3) substrate with a thickness of 635 μm was used as the inorganic substrate. In addition, a film was formed on the alumina substrate under the same conditions so as to obtain two types of ferrite layers (ferrite films) of annular and rectangular shapes. A magnetic composite was prepared in the same manner as in Example 3 except for the above.

[0147] [Example 5 (Comparative Example)]

[0148] In Example 5, a ferrite layer (ferrite-containing resin sheet) is prepared by a coating method. Specifically, ferrite powder is prepared in the same manner as in Example 1, and 80 parts by mass of the obtained ferrite powder is dispersed and mixed with 20 parts by mass of a photocurable resin. Thereafter, the obtained mixture is coated on a PET film. The coating is performed using an applicator in such a manner as to obtain a coating film with a thickness of 50 μm. Next, the obtained coating film is cured by ultraviolet rays to prepare a magnetic sheet. In addition, the PET film is used to coat the ferrite-containing resin sheet (80 parts by mass of ferrite powder + 20 parts by mass of a photocurable resin). After the ferrite-containing resin sheet is formed, the PET film is removed, and only the ferrite-containing resin sheet (resin composition) is evaluated.

[0149] [Example 6 (Comparative Example)]

[0150] In Example 6, a ferrite layer (ferrite-containing resin sheet) is prepared by a coating method. Specifically, ferrite powder is prepared in the same manner as in Example 3, and 80 parts by weight of the obtained ferrite powder is dispersed and mixed together with 20 parts by weight of a photocurable resin. Thereafter, the obtained mixture is coated on a PET film. The coating is performed using an applicator in such a manner as to obtain a coating film with a thickness of 50 μm. Next, the obtained coating film is cured by ultraviolet rays to prepare a magnetic sheet. In addition, the PET film is used to coat the ferrite-containing resin sheet (80 parts by weight of ferrite powder + 20 parts by weight of a photocurable resin). After the ferrite-containing resin sheet is formed, the PET film is removed, and only the ferrite-containing resin sheet (resin composition) is evaluated.

[0151] [Example 7 (Comparative Example)]

[0152] In Example 7, as in Example 1, a powder containing MnZn as the main component was used, and although the film was formed by the aerosol deposition method, when the fired product was decomposed and pulverized, it was passed through a bead mill 6 times under the conditions of a blade peripheral speed of 8.0 m / sec and a raw material supply amount of 3.5 kg / hour, and a pulverized fired product with a volume average particle size (D50) of 0.6 μm was produced. In addition, the film formation was performed 30 times on the surface and back of the substrate (glass substrate). Other than that, a magnetic composite was produced in the same manner as in Example 1.

[0153] [Example 8 (Comparative Example)]

[0154] When the fired product was decomposed and pulverized, it was passed through a bead mill once at a blade speed of 5.0 m / sec and a raw material supply rate of 6.0 kg / h to produce a pulverized fired product having a volume average particle size (D50) of 12.2 μm. A magnetic composite was produced in the same manner as in Example 7.

[0155] [Example 9 (Comparative Example)]

[0156] Instead of pulverizing the decomposed fired product, the particle size was adjusted by removing fine powder and coarse powder by air classification to produce a fired product having a volume average particle size (D50) of 9.8 μm. A magnetic composite was produced in the same manner as in Example 7 except for the above.

[0157] [Example 10 (Comparative Example)]

[0158] The film forming conditions of the ferrite layer were changed as shown in Table 2. Otherwise, a magnetic composite was produced in the same manner as in Example 1.

[0159] Regarding Examples 1 to 10, Tables 1 and 2 collectively show the production conditions of the ferrite powder and the magnetic composite.

[0160] [Table 1]

[0161]

[0162] [Table 2]

[0163] Table 2 Manufacturing conditions of magnetic composite

[0164]

[0165] Note 1) “*” indicates comparative example.

[0166] (2) Evaluation

[0167] In Examples 1 to 10, various properties of the ferrite powder, the non-metallic inorganic substrate, and the magnetic composite were evaluated as follows.

[0168] <Particle shape (raw material powder)>

[0169] The average value of SF-2 and the average value of aspect ratio of ferrite powder were obtained as follows. Ferrite powder was analyzed using a particle image analyzer (Morphologi G3, manufactured by Spectris Corporation) to obtain the projected circumference, projected area, major axis Fritt diameter, and minor axis Fritt diameter for 30,000 particles. The analysis was performed using an objective lens with a magnification of 20 times. Then, using the obtained data, SF-2 and aspect ratio were calculated for each particle according to the following formulas (1) and (2), and their average values ​​were obtained.

[0170] [Formula 4]

[0171]

[0172] [Formula 5]

[0173] <Particle size distribution (raw material powder)>

[0174] The particle size distribution of the ferrite powder was measured as follows. First, 0.1 g of the sample and 20 ml of water were placed in a 30 ml beaker, and two drops of sodium hexametaphosphate were added as a dispersant. Next, an ultrasonic homogenizer (SMT Co., Ltd., UH-150 model) was used for dispersion.

[0175] The output level of the sonic homogenizer was set to 4, and dispersion was performed for 20 seconds. Afterwards, the bubbles on the surface of the beaker were removed, and the mixture was introduced into a laser diffraction particle size distribution measuring device (SALD-7500nano, Shimadzu Corporation) for measurement. Through this measurement, the 10% cumulative diameter (D10), 50% cumulative diameter (D50; average particle diameter), and 90% cumulative diameter (D90) in the volume particle size distribution were obtained. The measurement conditions were set to a pump speed of 7, a built-in ultrasonic irradiation time of 30, and a refractive index of 1.70-050i. In addition, using D10, D50, and D90, the CV value was calculated according to the following formula (3).

[0176] [Formula 6]

[0177]

[0178] <XRD (raw material powder, ferrite layer)>

[0179] The ferrite powder and the ferrite layer of the magnetic composite were analyzed by X-ray diffraction (XRD) method. The analysis conditions are as follows.

[0180] -X-ray diffraction device: X'pertMPD manufactured by Panalytical (including high-speed detector)

[0181] -Line source: Co-Kα

[0182] -Tube voltage: 45kV

[0183] -Tube current: 40mA

[0184] -Scanning speed: 0.002° / sec (continuous scanning)

[0185] -Scanning range (2θ): 15~90°

[0186] In the obtained X-ray diffraction distribution, the integrated intensity (I 222 ) and the integrated intensity of the (311) surface diffraction peak (I 311 ), calculate the XRD peak intensity ratio (I 222 / I 311 ). In addition, the content ratios of the spinel phase and α-Fe2O3 were determined based on the X-ray diffraction distribution.

[0187] In addition, the X-ray diffraction distribution was subjected to Rietveld analysis to estimate the lattice constants (LCp, LCf) of the spinel phase, and the crystallite diameters (CSp, CSf) of the spinel phase were further obtained according to Scherrer's formula. Then, the lattice constant change rate (LCf / LCp) and crystallite diameter change rate (CSf / CSp) of the spinel phase before and after film formation were calculated.

[0188] <Magnetic properties (raw material powder, inorganic substrate, magnetic composite)>

[0189] The magnetic properties (saturation magnetization, residual magnetization and coercive force) of ferrite powder and inorganic substrate were measured as follows. First, the sample was filled in a cell with an inner diameter of 5 mm and a height of 2 mm and placed in a vibrating sample type magnetic measuring device (Toei Industry Co., Ltd., VSM-C7-10A). A magnetic field was applied and scanned to 5 kOe, then the applied magnetic field was reduced and a hysteresis curve was drawn. Based on the data of the obtained curve, the saturation magnetization (σs), residual magnetization (σr) and coercive force (Hc) of the sample were obtained.

[0190] For the magnetic composite with a glass substrate (Example 1 and Example 3), a sample in which a ferrite layer is formed on a glass substrate with a diameter of 5 mm and a thickness of 1 mm (1000 μm) is prepared. Then, the sample is filled into the sample unit, and the saturation magnetization (σs), residual magnetization (σr), and coercive force (Hc) of the sample are obtained in the same manner as the above method. For the magnetic composite with an alumina substrate (Example 2 and Example 4), a sample in which a ferrite layer is formed on an alumina substrate with a diameter of 5 mm and a thickness of 0.635 mm (635 μm) is prepared. Then, the sample is filled into the sample unit, and the saturation magnetization (σs), residual magnetization (σr), and coercive force (Hc) of the sample are obtained in the same manner as the above method.

[0191] <True specific gravity (raw material powder)>

[0192] The true specific gravity of the raw material powder was measured by the gas replacement method in accordance with JIS Z8837:2018.

[0193] <Thickness and element distribution (ferrite layer)>

[0194] The cross section of the ferrite layer was observed using a field emission scanning electron microscope (FE-SEM) to determine the thickness, and an element mapping analysis was performed on the cross section using an energy dispersive X-ray analyzer (EDX) attached to the microscope to obtain a mapping image.

[0195] <Density (Ferrite layer)>

[0196] The density of the ferrite layer is measured as follows. First, the mass of the substrate alone before the ferrite layer is formed is measured. Next, the mass of the substrate after the ferrite layer is formed is measured, and the difference between the mass of the substrate alone and the mass of the ferrite layer is calculated to obtain the mass of the ferrite layer. In addition, the film-forming area and film thickness of the ferrite layer are measured. The film thickness is obtained by observing the cross section of the ferrite layer using a scanning electron microscope (SEM). Then, the density of the ferrite layer is calculated according to the following formula (4).

[0197] [Formula 7]

[0198]

[0199] <Surface roughness (ferrite layer)>

[0200] The arithmetic mean roughness (Ra) and maximum height (Rz) of the ferrite layer surface were evaluated using a laser microscope (lasertec Co., Ltd., OPTELICS HYBRID). For each sample, 10 points were measured and the average value was obtained. The measurement was performed in accordance with JIS B 0601-2001. In addition, the arithmetic mean roughness (Ra) and the thickness (d F ), calculate the roughness ratio (Ra / d F ).

[0201] <Surface resistance (ferrite layer)>

[0202] The surface resistance of the ferrite layer was measured using a resistivity meter (Mitsubishi Chemical Corporation, LorestaHP MCP-T410).

[0203] <Magnetic Permeability (Magnetic Composite)>

[0204] The magnetic permeability of the magnetic composite was measured by the microstrip line complex permeability measurement method using a vector network analyzer (Keysight, PNA N5222B, 10MHz~26.5GHz) and a permeability measurement fixture (KEYCOM Corporation). Specifically, the magnetic composite was cut and placed in the permeability measurement fixture as a measurement sample. At this time, a sheet sample was cut into a length of 16mm and a width of 5mm for use. In addition, a ring-shaped sample was prepared by preparing a substrate with an outer diameter of 6.75mm and an inner diameter of 3.05mm, and forming a ferrite layer thereon. Next, the measurement frequency was scanned in the range of 100MHz to 10GHz on a logarithmic scale. The real part μ' and the imaginary part μ" of the complex permeability at a frequency of 1GHz were obtained, and the loss coefficient (tanδ) was calculated according to the following formula (5).

[0205] [Formula 8]

[0206]

[0207] <Adhesion (magnetic composite)>

[0208] The adhesion between the ferrite layer and the inorganic substrate is evaluated by a pencil hardness test (pencil scratch test). The measurement is based on the old JIS K5400. In each test, a pencil with the same concentration mark is repeatedly scratched five times. At this time, the front end of the pencil core is ground every time it is scratched. In addition, the pencil hardness increases in the order of 3B, 2B, B, HB, F, H, 2H, 3H, 4H, 5H, 6H, 7H, 8H, 9H, and 10H. The higher the hardness, the better the adhesion.

[0209] <Curie point (magnetic complex)>

[0210] The Curie point (Tc) of the magnetic composite is measured using a vibrating sample type magnetic measuring device (VSM). At this time, for the sheet-like sample, the magnetic composite cut into a fixed size (length 8mm, width 6mm) is placed in a measuring unit and set in a vibrating sample type magnetic measuring device (Toei Industry Co., Ltd., VSM-5 model). The sample is heated from room temperature to 500°C at a rate of 0.3°C / second under an applied magnetic field of 10kOe, and the saturation magnetization during heating is measured. The Curie point is calculated based on the temperature dependence of the obtained saturation magnetization. For the magnetic composite with a glass substrate (Examples 1 and 3), a sample with a ferrite layer formed on a glass substrate with a diameter of 5mm and a thickness of 1mm (1000μm) is prepared. And, the sample is filled in the sample unit, and the Curie point of the sample is calculated in the same way as the above method. For the magnetic composites with an alumina substrate (Examples 2 and 4), a sample with a ferrite layer formed on an alumina substrate with a diameter of 5 mm and a thickness of 0.635 mm (635 μm) was prepared. The sample was then filled into a sample cell and the Curie point of the sample was calculated in the same manner as above.

[0211] (3) Evaluation results

[0212] The properties of the ferrite powder and the properties of the substrate are shown in Tables 3 and 4, respectively, for Examples 1 to 10. In addition, the properties of the magnetic composite are shown in Tables 5 and 6.

[0213] As shown in Table 3, the ferrite powders used for film formation in Examples 1 to 10 all contained a spinel phase in an amount of 95% by mass or more, and the synthesis of spinel ferrite was fully performed. 222 / I 311 ) is 1.98 to 8.13%, which is comparable to that of general spinel ferrite. In addition, the average particle size (D50) is 0.6 to 12.2 μm, and the crystallite diameter is 8.621 to 32.331 nm.

[0214] As shown in Table 4, the non-metallic inorganic substrates used in Examples 1 to 4 and Examples 7 to 10 have a saturation magnetization (σs) of zero.

[0215] As shown in Tables 5 and 6, the magnetic composites of Examples 1 to 4 have a ferrite layer thickness (dF) of 2.3 μm or more, which is relatively large, and an XRD peak intensity ratio (I 222 / I 311 ) is approximately zero (0). In addition, the amount of α-Fe2O3 is 18.6~20.6% by mass, and the crystallite diameter is as small as less than 1.92nm. Therefore, the relative density, adhesion, and surface resistance of these samples are high. Specifically, the relative density of Examples 1 to 4 is as high as 0.89~0.92. In addition, the pencil hardness is as high as 10H or more, and the results of the adhesion test are good. In addition, an excellent composite with small imaginary part of magnetic permeability (μ") and loss coefficient (tanδ) and small loss is obtained. In addition, since it does not contain resin components (organic components), it has magnetic properties that can be measured even at high temperatures reaching the Curie point.

[0216] On the other hand, in Examples 5 and 6 prepared by the coating method, the imaginary part of the magnetic permeability (μ") and the loss coefficient (tanδ) were large, and the loss was large at 500 MHz and 1 GHz. In addition, in Examples 5 and 6, a binder resin was used when forming the magnetic composite, so the resin decomposed when the Curie point was measured while the temperature was increased. Therefore, the morphology of the magnetic composite could not be maintained.

[0217] In Example 7, in which a ferrite powder with a small particle size was used for aerosol deposition film formation, although a ferrite layer was slightly formed on the surface of the substrate, the raw material during film formation was a compressed powder. Therefore, the film properties of the resulting ferrite layer were the same as those of the raw material during film formation. On the other hand, in Examples 8 and 9, in which ferrite powder with a large particle size was used, the surface of the substrate was etched, but a ferrite layer was not formed. The thickness of the ferrite layer in Example 10 was the largest. However, after film formation (after the production of the magnetic composite), each substrate cracked due to internal stress. Therefore, as a magnetic composite, it lacks stability over time.

[0218] Regarding the ferrite layer of the magnetic composite obtained in Example 1, Fig.11 (a) to (f) show cross-sectional element mapping images. Fig.11 (a) to (f) are respectively an electron beam image (a), a carbon (C) mapping image (b), a silicon (Si) mapping image (c), an iron (Fe) mapping image (d), a manganese (Mn) mapping image (e), and an oxygen (O) mapping image (f). In addition, Fig.11 (a) to (f) show a non-metallic inorganic base material (glass substrate) on the upper side and a ferrite layer (MnZn-based ferrite layer) on the lower side.

[0219] The component elements of the non-metallic inorganic substrate (glass substrate) and the ferrite layer (MnZn-based ferrite layer) are clearly separated. That is, silicon (Si) exists on the substrate side, and manganese (Mn), iron (Fe) and oxygen (O) exist only on the ferrite layer side. It can be seen that there is no element diffusion caused by reaction between the substrate and the ferrite layer. In addition, no carbon (C) was confirmed in either the substrate or the ferrite layer.

[0220] For the ferrite layer of the magnetic composite obtained in Example 4, Fig.12 (a) to (g) show cross-sectional element mapping images. Fig.12 (a) to (g) are respectively electron beam image (a), carbon (C) mapping image (b), aluminum (Al) mapping image (c), iron (Fe) mapping image (d), zinc (Zn) mapping image (e), nickel (Ni) mapping image (f), and oxygen (O) mapping image (g). In addition, Fig.12 (a) to (g) show a non-metallic inorganic substrate (alumina substrate) on the upper side and a ferrite layer (NiCuZn-based ferrite layer) on the lower side.

[0221] The component elements of the non-metallic inorganic substrate (alumina substrate) and the ferrite layer (NiCuZn-based ferrite layer) are clearly separated. That is, aluminum (Al) exists on the substrate side, and nickel (Ni), copper (Cu), iron (Fe), zinc (Zn) and oxygen (O) exist only on the ferrite layer side. It can be seen that there is no diffusion of elements caused by reaction between the substrate and the ferrite layer. In addition, carbon (C) is confirmed in either the substrate or the ferrite layer.

[0222] [Table 3]

[0223]

[0224] [Table 4]

[0225] Table 4 Characteristics of non-metallic inorganic substrates

[0226]

[0227] Note 1) “*” indicates comparative example.

[0228] Note 2) The PET film used for coating the ferrite layer (ferrite powder 80 wt% + photocurable resin 20 wt%) was removed after the ferrite layer was formed, and the evaluation was performed only on the ferrite layer.

[0229] [Table 5]

[0230]

[0231] [Table 6]

[0232]

Claims

1. A magnetic composite comprising a non-metallic inorganic substrate and a ferrite layer provided on a surface of the non-metallic inorganic substrate, The non-metallic inorganic substrate has a thickness d M 2.0μm or more, The ferrite layer has a thickness d F The diameter is between 2.0 μm and 50.0 μm, and the main component is spinel ferrite. The α-Fe 2 O 3 The content of is 3.0 mass % or more and 25.0 mass % or less.

2. The magnetic composite according to claim 1, The ferrite layer, the integrated intensity I of the (222) plane in the X-ray diffraction analysis 222 The integrated intensity I relative to the (311) surface 311 Ratio I 222 / I 311 It is not less than 0.00 and not more than 0.

03.

3. The magnetic composite according to claim 1 or 2, The ferrite layer includes iron (Fe) and oxygen (O), and further includes at least one element selected from the group consisting of lithium (Li), magnesium (Mg), aluminum (Al), titanium (Ti), manganese (Mn), zinc (Zn), nickel (Ni), copper (Cu), and cobalt (Co).

4. The magnetic composite according to any one of claims 1 to 3, In the ferrite layer, the surface arithmetic mean roughness Ra is relative to its thickness d F Ratio Ra / d F It is higher than 0.00 and lower than 0.

20.

5. The magnetic composite according to any one of claims 1 to 4, The ferrite layer has a composition including a ferrite constituent component and the remainder being inevitable impurities.

6. The magnetic composite according to any one of claims 1 to 5, The non-metallic inorganic substrate is composed of oxide.

7. The magnetic composite according to any one of claims 1 to 5, The non-metallic inorganic substrate is composed of glass.

8. An element or component having coil and / or inductor functions, an electronic device, a housing for electronic components, an electromagnetic wave absorber, an electromagnetic wave shield, or an element or component having antenna functions, A magnetic composite according to any one of claims 1 to 7.

Citation Information

Patent Citations

  • Coating material excellent in heat radiation and electromagnetic wave absorbability and coated metal plate

    JP2004027064A

  • Electromagnetic wave absorber and electromagnetic noise control electronic apparatus

    JP2005045193A

  • Composite magnetic film and its manufacturing method

    JP2007088121A

  • Electromagnetic wave absorber

    JP2007180289A

  • Inductor element and its manufacturing method, and semiconductor module using inductor element

    JP2007250924A