Developing composite material as well as preparation method and application thereof

CN118976149APending Publication Date: 2024-11-19UNITECH (CHONGQING) MEDICAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411078064.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-07
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

Traditional human implanted medical materials are difficult to detect under X-rays, and due to the instability of the developer and poor mechanical properties, it increases the difficulty of implantation and examination, and may trigger inflammation and coagulation reactions.

Method used

The matrix material is modified by double bond silane coupling agent, and the contrast agent is doped in the polymer material, and the contrast agent is fixed by chemical bonds, so as to control the weight ratio of the contrast agent to the polymer material is within the range of 0.25-0.85%, and the silane is combined with Modification of coupling agent and matrix material improves the development effect and mechanical properties of the developing composite material.

Benefits of technology

The development composite material has a clear development under X-ray, excellent mechanical properties and good biocompatibility, which ensures accurate implantation and positioning, while avoiding developer shedding and material deformation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention relates to the technical field of biomedical materials, and particularly discloses a developing composite material and a preparation method and application thereof. The developing composite material provided by the invention comprises a base material and a high polymer material wrapping the surface of the base material, the surface of the base material is modified by a silane coupling agent containing double bonds; the high polymer material is doped with a contrast agent; the contrast agent accounts for 0.25-0.85% of the total weight of the high polymer material; the invention further provides a preparation method of the developing composite material and application of the developing composite material in bone tissue and soft tissue repair. The developing composite material provided by the invention is high in developing capacity and excellent in mechanical property, can be degraded in vivo, and is a good medical implant material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of biomedical materials, and in particular to a developing composite material and a preparation method and application thereof. Background Art

[0002] With the development of medicine, modern medical treatment usually implants non-permanent medical materials into the body to repair human hard tissues. However, traditional medical materials used for human body implants are made of metal, which can be developed under X-rays, so the position of the implanted medical materials can be determined during use. However, since such materials cannot be degraded and will cause inflammation and coagulation reactions with human tissues, which will cause damage to the human body, there are certain defects in their use.

[0003] In recent years, most of the medical materials implanted in the human body are made of degradable high-resolution materials. This type of medical material has good biocompatibility and degradability. It can decompose in the body to generate small molecules that can be absorbed or excreted by the human body. However, most of the above materials only contain elements such as C, H, and O, which are difficult to be detected by X-rays. Therefore, during use, medical personnel cannot determine their specific shape and position in the body, making it difficult to achieve accurate implantation and inspection positioning, which greatly increases the difficulty of surgery and inspection. In view of the above defects, the commonly used method is to mix the developer into the medical material to achieve the development effect of the medical material. However, the developed medical material prepared by the above method is relatively unstable, the developer is easy to fall off, and the mechanical properties of the medical material are also poor.

[0004] Therefore, developing a degradable developing composite material with strong developing ability, excellent mechanical properties is currently a hot topic in biomedical materials. Summary of the invention

[0005] In order to improve the developing ability and mechanical properties of a developing composite material, the present application provides a developing composite material and a preparation method and application thereof.

[0006] In a first aspect, the present application provides a developing composite material, which adopts the following technical solution: A developing composite material comprises a base material and a polymer material wrapped on the surface of the base material; the surface of the base material is modified by a silane coupling agent containing double bonds; the polymer material is doped with a contrast agent; the contrast agent accounts for 0.25-0.85% of the total weight of the polymer material.

[0007] The present application provides a developing composite material, in which the polymer material is attached to the surface of the base material in the form of chemical bonds under the action of a silane coupling agent, which greatly increases the firmness between the base and the polymer material, and a contrast agent is doped in the polymer material, the contrast agent can be well fixed inside the polymer material, and the weight ratio of the contrast agent to the polymer material is further controlled within the above range, which can improve the mechanical properties of the developing composite material on the one hand, and ensure that the developer does not fall off on the other hand, thereby improving the developing effect of the developing composite material.

[0008] In some embodiments, the contrast agent may account for 0.25-0.45%, 0.25-0.6%, 0.25-0.75%, 0.45-0.6%, 0.45-0.75%, 0.45-0.85%, 0.6-0.75%, 0.6-0.85% or 0.75-0.85% of the total weight of the polymer material.

[0009] In a specific embodiment, the contrast agent may also account for 0.25%, 0.45%, 0.6%, 0.75% or 0.85% of the total weight of the polymer material.

[0010] Preferably, the contrast agent accounts for 0.25-0.55% of the total weight of the polymer material.

[0011] When the amount of contrast agent added is too little, the development type of the development composite material will be poor; when the amount of contrast agent added is too much, the contrast agent is easy to fall off, resulting in reduced development effect, and too much contrast agent will affect the mechanical properties of the development composite material. Therefore, the present application has found through experimental research that by controlling the weight ratio of the contrast agent to the polymer material within the above range, the development performance of the obtained development composite material is good and the mechanical properties are excellent.

[0012] Preferably, the weight ratio of the matrix material to the polymer material is (12-23):1.

[0013] In the present application, the substrate material is first surface modified, and then the polymer material is coated on the surface of the polymer material in the form of chemical bonds. By adjusting the weight ratio of the substrate material to the polymer material within the above range, the mechanical properties of the obtained developing composite material are more excellent.

[0014] In some embodiments, the weight ratio of the matrix material to the polymer material may be (12-18):1 or (18-23):1.

[0015] In a specific embodiment, the weight ratio of the matrix material to the polymer material may also be 12:1, 18:1 or 23:1.

[0016] Preferably, the silane coupling agent is selected from γ-methacryloxypropyltrimethoxysilane, vinyltriethoxysilane, and vinyltri(β-methoxyethoxy)silane.

[0017] The present application uses the above-mentioned double-bonded silane coupling agent to modify the surface of the base material, which can make the base surface double-bonded, and then mix the modified base material with a polymer material. The polymer material will polymerize with the double bonds on the surface of the base material, thereby fixing the polymer material on the surface of the base material to obtain a developing composite material with excellent mechanical properties.

[0018] Preferably, the matrix material is selected from polyetheretherketone and hydroxyapatite; the polymer material contains at least one monomer selected from ethylene, styrene, and propylene; and one or more polymers selected from polylactic acid, polyglycolic acid, polyethylene glycol, polycaprolactone, polyanhydride, polyhydroxyalkanoate, polycarbonate, polyethylene glycol-polyglycolic acid copolymer, polystyrene olefin, and polylactic acid-polyglycolic acid copolymer.

[0019] In a specific embodiment, the matrix material is polyetheretherketone and hydroxyapatite in a weight ratio of 10:3.

[0020] In a specific embodiment, the polymer material is a mixture of styrene and polyethylene glycol.

[0021] In a specific embodiment, the polymer material is a mixture of propylene and polyethylene glycol-polyglycolic acid copolymer.

[0022] Preferably, the silane coupling agent accounts for 6-13% of the total weight of the base material.

[0023] In the present application, the amount of silane coupling agent added is controlled within the above range, so that the modification effect of the silane coupling agent on the surface of the base material can be better, the base material and the polymer material can be more closely connected, and the mechanical properties of the obtained developing composite material are better.

[0024] In some embodiments, the silane coupling agent may account for 6-10% or 10-13% of the total weight of the matrix material.

[0025] In a specific embodiment, the silane coupling agent may also account for 6%, 10% or 13% of the total weight of the base material.

[0026] Preferably, the contrast agent is a non-ionic contrast agent.

[0027] Non-ionic contrast agents have the advantages of small toxic side effects, low viscosity, fast absorption, good body tolerance, etc. Therefore, the composite imaging material provided in this application uses a non-ionic contrast agent, which will not cause adverse reactions in the human body, and on the other hand, is not affected by the blood-brain barrier and has a good imaging effect.

[0028] Further, the contrast agent is selected from iohexol, iomeprol, iosopeptidol, iovisol, iopromide, iopamidol, ioversol, iotrolan and iodixanol.

[0029] Preferably, the polymer material is also doped with growth factors; the growth factors are selected from epidermal growth factor, transforming growth factor, bone morphogenetic protein, nerve growth factor, vascular endothelial cell growth factor and fibroblast growth factor.

[0030] In the developing composite material provided in the present application, growth factors are doped into the polymer material, which can further improve the repair effect of the developing composite material in the body.

[0031] In a second aspect, the present application provides a method for preparing a developing composite material.

[0032] A method for preparing a developing composite material comprises the following steps: (1) mixing the polymer material with the contrast agent and the growth factor, and stirring for 30-60 minutes to obtain a premix; (2) Mix deionized water, base material and silane coupling agent, place in an ultrasonic device, and stir at 35-45° C. for 3-4 hours; (3) Then, sodium dodecyl sulfate is added to the system of step (2), and the system temperature is raised to 70-90° C. The premix of step (1) is added under stirring, and the mixture is reacted at this temperature for 4-6 hours. Finally, the mixture is cooled to room temperature, and the developing composite material is obtained by demulsification and vacuum drying.

[0033] In a third aspect, the present application provides an application of the developing composite material in the repair of bone tissue and soft tissue.

[0034] The imaging composite material provided in the present application has excellent imaging properties, mechanical properties and degradability on the one hand, and excellent biocompatibility on the other hand. Therefore, when using the above imaging composite material for bone tissue and soft tissue repair, imaging will appear under X-rays during surgery and subsequent inspections, thereby enabling accurate implantation and positioning; and the above imaging composite material has good mechanical properties, so it will not deform during use, and therefore has good stability in use.

[0035] In summary, this application has the following beneficial effects: 1. The present application can obtain a degradable developing composite material with good developing effect, excellent mechanical properties and good biocompatibility by double-bonding the surface of the matrix and then blending it with a polymer material and a contrast agent. When the developing composite material is implanted into the body, it has clear development under X-rays, so it can be accurately implanted, and the above-mentioned developing composite material has good mechanical properties and will not deform during use.

[0036] 2. The present application controls the proportion of contrast agent in the polymer material to 0.25-0.85%, which can improve the mechanical properties of the developing composite material on the one hand, and ensure that the developer does not fall off on the other hand, thereby achieving an excellent developing effect.

[0037] 3. In the present application, the amount of silane coupling agent added is controlled to 6-13% of the total weight of the base material, which can make the modification effect of the silane coupling agent on the surface of the base material better, the base material and the polymer material can be connected more closely, and the mechanical properties of the obtained developing composite material are better. DETAILED DESCRIPTION

[0038] The present application provides a developing composite material, which includes 20-30 parts of a base material and 40-60 parts of a polymer material wrapped on the surface of the base material; the surface of the base material is modified by a silane coupling agent containing double bonds; a contrast agent and a growth factor are doped in the polymer material; the weight ratio of the contrast agent to the polymer material is (0.35-1.25):50; further, the weight ratio of the contrast agent to the polymer material is (0.5-1):50.

[0039] Among them, the silane coupling agent is selected from γ-methacryloxypropyltrimethoxysilane, vinyltriethoxysilane, and vinyltri(β-methoxyethoxy)silane. The matrix material is selected from polyetheretherketone and hydroxyapatite; the polymer material is selected from polylactic acid, polyglycolic acid, polyethylene glycol, polycaprolactone, polyanhydride, polyhydroxyalkanoate, polycarbonate, polyethylene glycol-polyglycolic acid copolymer, polyphenylene olefin and polylactic acid-polyglycolic acid copolymer. The contrast agent is a non-ionic developer. The contrast agent is selected from iohexol, iomeprol, ioisosopeptidol, iovisol, iopromide, iopamidol, ioforsol, iotrolan and iodixanol. The growth factor is selected from epidermal growth factor, transforming growth factor, bone morphogenetic protein, nerve growth factor, vascular endothelial growth factor and fibroblast growth factor.

[0040] The present application also provides a method for preparing the above-mentioned developing composite material, comprising the following steps: (1) mixing the polymer material with the contrast agent and the growth factor, and stirring for 30-60 minutes to obtain a premix; (2) Mix deionized water, base material and silane coupling agent, place in an ultrasonic device, and stir at 35-45° C. for 3-4 hours; (3) Then, sodium dodecyl sulfate is added to the system of step (2), and the system temperature is raised to 70-90° C. The premix of step (1) is added under stirring, and the mixture is reacted at this temperature for 4-6 hours. Finally, the mixture is cooled to room temperature, and the developing composite material is obtained by demulsification and vacuum drying.

[0041] In the present application, polyetheretherketone was purchased from Shanghai Huipu Industrial Chemicals Co., Ltd.; hydroxyapatite was purchased from Shanghai Aladdin Biochemical Technology Co., Ltd.; the CAS number of iotrolan is 79770-24-4; transforming growth factor (TGF-β) and fibroblast growth factor (FGF) were purchased from Saiye (Guangzhou) Biotechnology Co., Ltd.; the remaining raw materials, reagents, solvents, etc. can be obtained commercially.

[0042] The present application is further described in detail below in combination with embodiments, comparative examples and performance testing experiments. Example

[0043] Example 1 Embodiment 1 provides a developing composite material.

[0044] The method for preparing the above-mentioned developing composite material comprises the following steps: (1) 1 g of styrene, 9 g of polyethylene glycol, 0.025 g of iotrolan, and 0.005 g of growth factor (transforming growth factor and fibroblast growth factor in a mass ratio of 1:1) are mixed and stirred for 30 minutes to obtain a premix; wherein the contrast agent accounts for 0.25% of the total weight of the polymer material; and the growth factor accounts for 0.05% of the total weight of the polymer material.

[0045] (2) 180 g of the matrix material and 18 g of γ-methacryloxypropyltrimethoxysilane were added to 100 mL of deionized water, placed in an ultrasonic device, and stirred at 40° C. for 3 h; the matrix material was polyetheretherketone and hydroxyapatite in a mass ratio of 10:3.

[0046] (3) Then, 0.005 g of sodium dodecyl sulfate is added to the system of step (2), and the system temperature is raised to 85° C. The premix obtained in step (1) is added under stirring, and the mixture is reacted at this temperature for 5 h. Finally, the temperature is lowered to room temperature, and a developing composite material is obtained after demulsification and vacuum drying.

[0047] Embodiment 2-5 Examples 2-5 each provide a developing composite material.

[0048] The difference between the above embodiment and embodiment 1 is that the amount of contrast agent added to the developing composite material is specifically shown in Table 1.

[0049] Table 1 Addition amount of contrast agent in the developing composite material provided in Examples 2-5 Example 6 Example 6 provides a developing composite material.

[0050] The difference between the above embodiment and embodiment 3 is that the amount of the base material is 120 g, and the amount of γ-methacryloxypropyltrimethoxysilane is 12 g.

[0051] Example 7 Example 7 provides a developing composite material.

[0052] The difference between the above embodiment and embodiment 3 is that the amount of the base material is 230 g, and the amount of γ-methacryloxypropyltrimethoxysilane is 23 g.

[0053] Example 8 Example 8 provides a developing composite material.

[0054] The difference between the above embodiment and embodiment 3 is that the amount of the base material is 280 g, and the amount of γ-methacryloxypropyltrimethoxysilane is 28 g.

[0055] Example 9 Example 9 provides a developing composite material.

[0056] The difference between the above embodiment and embodiment 3 is that the silane coupling agent used in the preparation process of the developing composite material is vinyl triethoxy silane.

[0057] Example 10 Embodiment 10 provides a developing composite material.

[0058] The difference between the above embodiment and embodiment 3 is that in the preparation process of the developing composite material provided in embodiment 10, the added amount of γ-methacryloxypropyltrimethoxysilane is 7.2 g.

[0059] Embodiment 11 Example 11 provides a developing composite material.

[0060] The difference between the above embodiment and embodiment 3 is that in the preparation process of the developing composite material provided in embodiment 11, the added amount of γ-methacryloxypropyltrimethoxysilane is 10.8 g.

[0061] Example 12 Example 12 provides a developing composite material.

[0062] The difference between the above embodiment and embodiment 3 is that in the preparation process of the developing composite material provided in embodiment 10, the added amount of γ-methacryloxypropyltrimethoxysilane is 23.4 g.

[0063] Embodiment 13 Example 13 provides a developing composite material.

[0064] The difference between the above embodiment and embodiment 3 is that the polymer material is a mixture of 1 g of propylene and 9 g of polyethylene glycol-polyglycolic acid copolymer.

[0065] Comparative Example Comparative Example 1 Comparative Example 1 provides a developing composite material.

[0066] The difference between the above-mentioned developing composite material and Example 1 is that the added amount of the contrast agent in the developing composite material provided in Comparative Example 1 is 0.2 g.

[0067] Comparative Example 2 Comparative Example 2 provides a developing composite material.

[0068] The difference between the above-mentioned developing composite material and Example 1 is that the added amount of the contrast agent in the developing composite material provided in Comparative Example 2 is 1.5 g.

[0069] Comparative Example 3 Comparative Example 3 provides a developing composite material.

[0070] The difference between the comparative example and Example 3 is that the silane coupling agent used in the preparation process of the developing composite material provided in Comparative Example 4 is KH-560 (γ-glycidyloxypropyltrimethoxysilane) Comparative Example 4 Comparative Example 4 provides a developing composite material.

[0071] The preparation method of the above-mentioned developing composite material is as follows: (1) 1 g of styrene, 9 g of polyethylene glycol, 0.025 g of iotrolan, and 0.005 g of growth factor (transforming growth factor and fibroblast growth factor in a mass ratio of 1:1) are mixed and stirred for 30 minutes to obtain a premix; wherein the contrast agent accounts for 0.25% of the total weight of the polymer material; and the growth factor accounts for 0.05% of the total weight of the polymer material.

[0072] (2) 180 g of the matrix material and 0.005 g of sodium dodecyl sulfate were added to 100 mL of deionized water, and the system temperature was raised to 85° C. The premix obtained in step (1) was added under stirring, and the mixture was reacted at this temperature for 5 h. Finally, the mixture was cooled to room temperature, and the developing composite material was obtained by demulsification and vacuum drying.

[0073] Comparative Example 5 Comparative Example 5 provides a developing composite material.

[0074] The preparation method of the above-mentioned developing composite material is: mix 1g of styrene, 9g of polyethylene glycol, 0.025g of iotrolan, 0.005g of growth factor (transforming growth factor and fibroblast growth factor in a mass ratio of 1:1), 180g of matrix material, and 0.005g of sodium dodecyl sulfate, and melt blend them at 400°C to obtain the developing composite material.

[0075] Performance testing The developed composite materials obtained in Examples 1-13 and Comparative Examples 1-5 were melted and then molded using a flat-plate vulcanizer. The temperatures of the upper and lower templates were controlled at (170±2)°C and (160±2)°C, and the pressure was 14.5 MPa to obtain composite repair material plates, which were cut into 1 bone tissue repair material with a size of 0.5×0.5 cm and 2 sizes of 1×2 cm.

[0076] (I) Development performance test The developing performance of the bone tissue repair material with a size of 0.5×0.5 cm was tested using an X-ray developer to observe the developing effects of the bone tissue repair materials provided by each embodiment and comparative example. The results are shown in Table 2 below.

[0077] (II) Mechanical properties test The yield strength of the bone tissue repair material with a size of 1×2 cm was tested using an electronic tensile testing machine, and the test method was referred to GB / T 1040-2018. The notched impact strength of the bone tissue repair material with a size of 1×2 cm was tested using an impact testing machine, and the test method was referred to GB / T 1043-2018. The test results are shown in Table 2.

[0078] Table 2 Development effects of the development composite materials obtained in Examples 1-13 and Comparative Examples 1-5 According to the test results in Table 2, the developing composite materials obtained in Examples 1-13 have good developing effects, yield strength>26MPa, and impact resistance>15%; while the developing composite materials obtained in Comparative Examples 1-5 have average developing effects, yield strength<26MPa, and impact resistance≤15.0kJ / m 2 Therefore, it is explained that the present application uses a double-bonded silane coupling agent to modify the surface of the base material, dopes the contrast agent into the polymer material, and controls the doping amount of the contrast agent within the range of 0.25-0.85%, so as to obtain a developing composite material with good developing performance and excellent mechanical properties.

[0079] According to the test results of Examples 1-5 and Comparative Examples 1-2, the developing performance and mechanical properties of the developing composite material obtained in Examples 1-5 are better than those of the developing composite material obtained in Comparative Examples 1-2, indicating that the present application controls the doping amount of the contrast agent within the range of 0.25-0.85%, and can obtain a developing composite material with excellent performance; further comparison shows that the yield strength of the developing composite material obtained in Examples 2-4 is greater than 30MPa, the impact resistance is greater than 17%, and the developing effect is very clear and obvious, indicating that the present application further controls the doping amount of the contrast agent within the range of 0.45-0.75%, and the obtained developing composite material has better performance.

[0080] According to the test results of Example 3 and Examples 6-8, although the developing composite material obtained in Example 6 has a good developing effect, its mechanical properties are poor, its yield strength is only 26.5MPa, and its impact resistance is only 15.9kJ / m 2 The developing composite materials obtained in Example 3 and Examples 7-8 not only have good developing effects, but also have yield strength greater than 32MPa and impact resistance greater than 16%. Therefore, it is explained that the mechanical properties of the developing composite materials obtained by the present application are more excellent by controlling the weight ratio of the base material to the polymer material within the range of (12-23):1.

[0081] According to the test results of Example 3 and Example 9, the double-bonded silane coupling agent used in the present application can achieve surface modification of the base material, and the modified base material and the polymer material will be more firmly connected, and the obtained developing composite material has better mechanical properties.

[0082] According to the test results of Example 3 and Examples 10-12, the yield strength of the developing composite materials obtained in Examples 3 and Examples 11-12 is greater than 30 MPa, and the impact resistance is greater than 17%; while the yield strength of the developing composite material obtained in Example 10 is only 28.4 MPa, and the impact resistance is 16.6 kJ / m 2Therefore, it is explained that the application controls the addition amount of the silane coupling agent within the range of 6-13%, the silane coupling agent has a better modification effect on the surface of the base material, the base material and the polymer material are more closely connected, and the mechanical properties of the obtained developing composite material are better.

[0083] According to the test results of Example 13, the yield strength of the developed composite material obtained in Example 13 is 33.4 MPa, and the impact resistance is greater than 17.8 kJ / m 2 , indicating that the developing composite material prepared by the mixture of propylene and polyethylene glycol-polyglycolic acid copolymer in the present application can also obtain excellent developing effect and mechanical properties.

[0084] Although the present invention has been described in detail above with general descriptions and specific embodiments, it is obvious to those skilled in the art that some modifications or improvements may be made thereto based on the present invention. Therefore, these modifications or improvements made without departing from the spirit of the present invention all fall within the scope of protection claimed by the present invention.

Claims

1. A developing composite material, characterized in that: It comprises a base material and a polymer material wrapped on the surface of the base material; the surface of the base material is modified by a silane coupling agent containing double bonds; the polymer material is doped with a contrast agent; and the contrast agent accounts for 0.25-0.85% of the total weight of the polymer material.

2. The developing composite material according to claim 1, characterized in that: The contrast agent accounts for 0.45-0.75% of the total weight of the polymer material.

3. The developing composite material according to claim 1, characterized in that: The weight ratio of the matrix material to the polymer material is (12-23):

1.

4. The developing composite material according to claim 1, characterized in that: The silane coupling agent is selected from γ-methacryloxypropyltrimethoxysilane, vinyltriethoxysilane, and vinyltri(β-methoxyethoxy)silane.

5. The developing composite material according to claim 1, characterized in that: The silane coupling agent accounts for 6-13% of the total weight of the base material.

6. The developing composite material according to claim 1, characterized in that: The matrix material is selected from polyetheretherketone and hydroxyapatite; The polymer material comprises at least one monomer selected from ethylene, styrene and propylene; and one or more polymers selected from polylactic acid, polyglycolic acid, polyethylene glycol, polycaprolactone, polyanhydride, polyhydroxyalkanoate, polycarbonate, polyethylene glycol-polyglycolic acid copolymer, polystyrene olefin and polylactic acid-polyglycolic acid copolymer.

7. The developing composite material according to claim 1, characterized in that: The contrast agent is a non-ionic developer.

8. The developing composite material according to any one of claims 1 to 7, characterized in that: The polymer material is also doped with growth factors; the growth factors are selected from epidermal growth factor, transforming growth factor, bone morphogenetic protein, nerve growth factor, vascular endothelial cell growth factor and fibroblast growth factor.

9. The method for preparing the developing composite material according to any one of claims 1 to 7, characterized in that: The following steps are involved: (1) Mixing the polymer material with the contrast agent and the growth factor and stirring for 30-60 minutes to obtain a premix; (2) Add the matrix material and silane coupling agent into deionized water, place in an ultrasonic device, and stir at 35-45°C for 3-4 hours; (3) Then, sodium dodecyl sulfate is added to the system of step (2), and the system temperature is raised to 70-90°C. The premix of step (1) is added under stirring, and the mixture is reacted at this temperature for 4-6 hours. Finally, the mixture is cooled to room temperature, and the developing composite material is obtained by demulsification and vacuum drying.

10. Use of the developing composite material according to any one of claims 1 to 7 in repairing bone tissue or soft tissue.