Janus nanofiltration membrane as well as preparation method and application thereof

By performing free interface polymerization reaction on the surface of the nanofiltration membrane and spraying polyethyleneimine solution, a low-resistance ultra-short transmission channel is constructed to form a positive and negative-electric Janus nanofiltration membrane, which solves the lithium separation performance of the nanofiltration membrane in brine The problem of inefficiency and balance of selectivity and permeability has achieved efficient separation of magnesium lithium and improved permeability.

CN118976384AActive Publication Date: 2024-11-19WUYI UNIV
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411107362.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-13
Publication Date
2024-11-19
Estimated Expiration
2044-08-13

AI Technical Summary

Technical Problem

The existing nanofiltration membranes are not efficient in separating lithium extraction in brine, and the counterion selectivity to monovalent/divalent ions is low due to single charge, and there is a Trade- between selectivity and permeability flux. The off effect makes it difficult to find a balance between efficient separation of magnesium lithium and flux enhancement.

Method used

Using the preparation method of Janus nanofiltration membrane, the free interface polymerization reaction is carried out on the base film surface by aqueous monomer solution and oily monomer solution to form a composite film, and the polyethyleneimine solution is sprayed on the surface, heated and cured, and constructed. Low resistance ultra-short transmission channel forms positive and negative charge Janus nanofiltration membrane, optimizing the separation and permeability of magnesium lithium.

Benefits of technology

A rich low-resistance ultra-short transmission channel is achieved, which significantly improves the separation and permeability of magnesium lithium, weakens the Trade-off effect between separation and permeability, and improves the efficiency and flux of lithium extraction from salt lakes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118976384A_ABST
    Figure CN118976384A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of nanofiltration membranes, and discloses a Janus nanofiltration membrane as well as a preparation method and application thereof. The preparation method comprises the following steps: S1, carrying out free interfacial polymerization reaction on a water-phase monomer solution and an oil-phase monomer solution on the surface of a base membrane to form a composite membrane; s2, spraying a polyethyleneimine solution on the surface of the composite membrane, and heating and curing to obtain the Janus nanofiltration membrane, wherein the component of the water phase monomer solution comprises gamma-cyclodextrin subjected to amination modification; the component of the oil phase monomer solution comprises terephthaloyl chloride. The positive and negative electric Janus nanofiltration membrane prepared by the preparation method constructs abundant low-resistance ultrashort transmission channels, and shows excellent magnesium-lithium separation property and permeability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of nanofiltration membranes, and in particular to a Janus nanofiltration membrane and a preparation method and application thereof. Background Art

[0002] Nanofiltration is a membrane technology between ultrafiltration and reverse osmosis, and has a high retention rate for divalent ions and soluble organic molecules with a molecular weight of more than 200 Da. However, since the surface of the nanofiltration membrane is usually singly charged, it often leads to low selectivity for monovalent / divalent counterions. Therefore, the Janus nanofiltration membrane has emerged (Janus membrane is an emerging concept in the membrane field, referring to a separation membrane with an asymmetric structure or property), but it still faces the problem of large mass transfer resistance of the nanofiltration membrane, which makes the separation and extraction of lithium from brine inefficient. In addition, the "trade-off" effect between selectivity and permeation flux makes it difficult for nanofiltration membranes to make breakthroughs in the efficient separation of magnesium and lithium and flux improvement.

[0003] Therefore, in order to overcome the limitations of existing nanofiltration membranes and improve the efficiency and flux of lithium extraction from salt lakes, it is particularly urgent to develop a novel preparation method for Janus nanofiltration membranes. Summary of the invention

[0004] The present invention aims to solve at least one of the technical problems existing in the prior art. To this end, the first aspect of the present invention provides a method for preparing a Janus nanofiltration membrane, wherein the Janus nanofiltration membrane prepared by the method constructs a low-resistance ultra-short transmission channel, exhibits excellent magnesium-lithium separation and permeability, and weakens the trade-off effect between separation and permeability.

[0005] The second aspect of the present invention also provides a Janus nanofiltration membrane.

[0006] The third aspect of the present invention also provides an application of a Janus nanofiltration membrane.

[0007] A method for preparing a Janus nanofiltration membrane according to a first aspect of the present invention comprises the following steps:

[0008] S1, performing free interface polymerization reaction of the aqueous phase monomer solution and the oil phase monomer solution on the surface of the base film to form a composite film;

[0009] S2, spraying polyethyleneimine solution on the surface of the composite membrane, heating and curing to obtain a Janus nanofiltration membrane;

[0010] The components of the aqueous monomer solution include amino-modified γ-cyclodextrin; and the components of the oily monomer solution include terephthaloyl chloride.

[0011] The method for preparing the Janus nanofiltration membrane according to the embodiment of the present invention has at least the following beneficial effects:

[0012] The present invention uses amino-modified γ-cyclodextrin as a water phase monomer and terephthaloyl chloride as an oil phase monomer, performs free interfacial polymerization on the surface of a base film, and then sprays the surface of the composite film with a polyethyleneimine solution. The formed positive and negative charge Janus nanofiltration membrane constructs abundant low-resistance ultra-short transmission channels, exhibits excellent magnesium-lithium separation and permeability, and weakens the trade-off effect between separation and permeability.

[0013] Furthermore, this is because the amino-modified γ-cyclodextrin is more easily reacted with terephthaloyl chloride, causing most of the cyclodextrin cavities to be vertically arranged and distributed in the membrane, constructing abundant low-resistance ultra-short transmission channels and ultra-thin polyamide layers, and the cavity of γ-CDA also performs secondary separation of magnesium and lithium.

[0014] Furthermore, the polyethyleneimine solution reacts with unreacted terephthaloyl chloride to make the membrane surface positively charged, which is beneficial to the separation of magnesium and lithium due to the electrostatic repulsion effect.

[0015] According to some embodiments of the present invention, the concentration of the aqueous monomer solution is 0.2 wt.% to 0.5 wt.%. Thus, within the above range, magnesium-lithium separability and permeability are increased.

[0016] According to some embodiments of the present invention, in step S1, the free interface polymerization reaction time is 1 minute to 5 minutes.

[0017] According to some embodiments of the present invention, in step S1, the free interface polymerization reaction time is 1 minute to 2 minutes. Thus, good permeation flux and magnesium-lithium separation are achieved within the above range.

[0018] According to some embodiments of the present invention, the concentration of the oil phase monomer solution is 0.05 wt.% to 1 wt.%.

[0019] According to some embodiments of the present invention, the concentration of the oil phase monomer solution is 0.05 wt.% to 0.1 wt.%, thereby increasing the separation and permeability of the membrane.

[0020] According to some embodiments of the present invention, in step S2, the spraying time is 1 second to 5 seconds.

[0021] According to some embodiments of the present invention, the concentration of the polyethyleneimine solution is 0.05 wt.% to 0.25 wt.%.

[0022] According to some embodiments of the present invention, the temperature of the aqueous monomer solution is 10°C to 30°C.

[0023] According to some embodiments of the present invention, the temperature of the aqueous monomer solution is 10° C. to 20° C. As a result, the diffusion rate of the cyclodextrin monomer into the oil phase increases, the structure of the membrane gradually improves, and the permeation flux and separation factor of the membrane reach the highest.

[0024] Furthermore, when the temperature is higher than 20°C, the diffusion rate of cyclodextrin monomers continues to increase, and the hydroxyl groups on cyclodextrin may also react with TPC, resulting in a decrease in the arrangement regularity of cyclodextrin and an increase in film thickness.

[0025] According to some embodiments of the present invention, the temperature of the heating and curing is 50°C to 70°C.

[0026] According to some embodiments of the present invention, the amino-modified γ-cyclodextrin is prepared by the following method:

[0027] Mix γ-cyclodextrin, N,N'-carbonyldiimidazole and an organic solvent, then add ethylenediamine and continue mixing and reacting to obtain the product.

[0028] According to some embodiments of the present invention, the material of the base film is selected from at least one of polyethersulfone, sulfonated polysulfone, polyvinylidene fluoride or polyacrylonitrile.

[0029] A Janus nanofiltration membrane provided according to an embodiment of the second aspect of the present invention is prepared by the preparation method described in the first aspect of the present invention. Thus, the Janus nanofiltration membrane of the present invention constructs abundant low-resistance ultra-short transmission channels, exhibits excellent magnesium-lithium separation and permeability, and weakens the trade-off effect between separation and permeability.

[0030] According to some embodiments of the present invention, the thickness of the Janus nanofiltration membrane is 20 nm to 50 nm.

[0031] A third aspect of the present invention provides the Janus nanofiltration membrane described above; or the use of the Janus nanofiltration membrane prepared by the preparation method described above in seawater desalination and lithium extraction from salt lakes.

[0032] Other features and advantages of the present invention will be set forth in the description which follows, and in part will be apparent from the description, or may be learned by practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] The above and / or additional aspects and advantages of the present invention will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:

[0034] Figure 1 These are scanning electron microscope (FESEM) and transmission electron microscope (TEM) images of the surface of the Janus nanofiltration membrane prepared in Example 1 of the present invention.

[0035] Figure 2 It is the pore size distribution diagram of the Janus nanofiltration membrane prepared in Example 1 of the present invention and the nanofiltration membrane prepared in Comparative Example 1.

[0036] Figure 3 It is the membrane surface potential diagram of the back and front sides of the Janus nanofiltration membrane prepared in Example 1 of the present invention. DETAILED DESCRIPTION

[0037] The following are specific embodiments of the present invention, and the technical solutions of the present invention are further described in conjunction with the embodiments, but the present invention is not limited to these embodiments.

[0038] Unless otherwise specified, the reagents, methods and equipment used in the present invention are conventional reagents, methods and equipment in the art.

[0039] Some of the raw materials in the embodiments of the present invention are as follows:

[0040] The amino-modified γ-cyclodextrin was prepared by the following method:

[0041] First, weigh 5.20g of γ-cyclodextrin (γ-CD) and 5.71g of N,N'-carbonyldiimidazole (CDI) and dissolve them in dimethyl sulfoxide (DMSO) solution. Stir at room temperature for 12h under argon protection, then add 53.6mL of ethylenediamine (EDA) and continue stirring for 12h. Then, use vacuum rotary evaporation to concentrate to 40-50mL, then add 500mL of acetone and stir and precipitate. Repeat three times to precipitate. Finally, add a small amount of deionized water and freeze-dry to obtain dry pure amino-modified γ-cyclodextrin (named: γ-CDA).

[0042] Terephthaloyl chloride, polyethyleneimine, and polyethersulfone-based membranes are all commercially available products.

[0043] Example 1

[0044] This example provides a Janus nanofiltration membrane, and the preparation method thereof is as follows:

[0045] Prepare an aqueous monomer solution: the mass concentration of γ-CDA is 0.25 wt.%, and the temperature of the γ-CDA aqueous monomer solution is controlled to be 15°C.

[0046] Prepare the oil phase monomer solution: dissolve terephthaloyl chloride in n-hexane, the concentration of terephthaloyl chloride is 0.1wt.%.

[0047] S1. Place the metal sieve with polysulfone (PES) base membrane in a flat-bottomed glass cylinder, add γ-CDA aqueous monomer solution, ensure that the liquid level is 0.5 cm above the PES base membrane plane, then add TPC oil-phase monomer solution drop by drop until it is 0.3 cm above the interface, perform free interface polymerization for 2 min, and then slowly take out the metal mesh at a certain tilt angle;

[0048] S2. Use an atomizer to spray a 0.1% wt% PEI aqueous solution on the membrane surface for 4 seconds, place the membrane in an oven and heat at 60° C. to cure, thereby obtaining a Janus nanofiltration membrane, which is then taken out and stored in deionized water for later use.

[0049] Example 2

[0050] This example provides a Janus nanofiltration membrane, and its preparation method and component dosage are basically the same as those in Example 1, except that: the aqueous phase monomer solution is prepared: the mass concentration of γ-CDA is 0.2 wt.%.

[0051] Example 3

[0052] This example provides a Janus nanofiltration membrane, and its preparation method and component dosage are basically the same as those in Example 1, except that: the aqueous phase monomer solution is prepared: the mass concentration of γ-CDA is 0.5 wt.%.

[0053] Example 4

[0054] This example provides a Janus nanofiltration membrane, and its preparation method and component dosage are basically the same as those in Example 1, except that: the aqueous phase monomer solution is prepared: the mass concentration of γ-CDA is 0.1 wt.%.

[0055] Example 5

[0056] This example provides a Janus nanofiltration membrane, and its preparation method and component dosage are basically the same as those in Example 1, except that: the aqueous phase monomer solution is prepared: the mass concentration of γ-CDA is 0.7 wt.%.

[0057] Example 6

[0058] This example provides a Janus nanofiltration membrane, the preparation method and component dosage of which are basically the same as those of Example 1, except that the temperature of the aqueous monomer solution is 10°C.

[0059] Example 7

[0060] This example provides a Janus nanofiltration membrane, the preparation method and component dosage of which are basically the same as those of Example 1, except that the temperature of the aqueous monomer solution is 20°C.

[0061] Example 8

[0062] This example provides a Janus nanofiltration membrane, the preparation method and component dosage of which are basically the same as those of Example 1, except that the temperature of the aqueous monomer solution is 30°C.

[0063] Comparative Example 1

[0064] This example provides a nanofiltration membrane, and its preparation method and component dosage are basically the same as those in Example 1, except that the step of spraying the polyethyleneimine solution is missing.

[0065] Comparative Example 2

[0066] This example provides a nanofiltration membrane, and its preparation method and component dosage are basically the same as those in Example 1, except that trimesoyl chloride is used to replace terephthaloyl chloride.

[0067] Performance Testing

[0068] The Janus nanofiltration membrane prepared in Example 1 of the present invention was subjected to FESEM detection, wherein Figure 1 a is the TEM image of Janus nanofiltration membrane surface; Figure 1 b is the SEM cross-sectional view of Janus nanofiltration membrane. Figure 1 It can be seen that uniform small protrusions appear on the surface of the Janus film of Example 1, and the thickness thereof is about 29 nm.

[0069] Furthermore, the nanofiltration membranes of Example 1 and Comparative Example 1 were tested for pore size, and the results are as follows: Figure 2 As shown, the pore size of the membrane in Comparative Example 1 is mainly concentrated at about 0.78 nm, and the distribution is relatively concentrated; while the pore size of the Janus nanofiltration membrane in Example 1 of the present application is mainly concentrated at about 0.72 nm, which is more conducive to the separation of magnesium and lithium.

[0070] Furthermore, the Janus nanofiltration membrane prepared in Example 1 of the present invention was subjected to a surface charge test (Sur-PASS solid surface Zeta potential instrument was used to measure the membrane surface charge). The results are as follows: Figure 3 As shown in the figure, in the raw material solution with pH = 6.35, the potential on the back side is -16.6 mV, while the potential on the front side is 4.5 mV, and the potential on the back / front membrane surface changes greatly, indicating that a Janus nanofiltration membrane with positive and negative charges is formed.

[0071] Furthermore, the permeate flux and separation factor S of the nanofiltration membranes prepared in the embodiments of the present invention and the comparative examples were tested. Li,Mg Analyzing the separation performance of nanofiltration membranes:

[0072] (1) The calculation formula of permeate flux is as follows

[0073]

[0074] Where F is the permeability of the membrane at a given pressure, L·m -2 ·h -1 bar -1 ; V is the volume of the permeate solution, A is the effective area of ​​the membrane, and p is the filtration pressure.

[0075] The equation for the solute rejection (R) (retention) of a solute is as follows:

[0076]

[0077] Among them, C p and C f represent the concentrations in the permeate solution and the feed solution, respectively.

[0078] Separation factor S, which indicates separation performance Li,Mg Calculated by the following formula:

[0079]

[0080] Among them, C Li,p and C Li,f are Li in the permeate and feed solution, respectively. + The concentration of C Mg,p and C Mg,f are the Mg in the permeate and feed solution, respectively. 2+ concentration.

[0081] The effective test area of ​​the membrane is 12.56 cm 2 , the test temperature is 25℃, the filtration pressure is 1.5 bar, and the membrane surface flow rate is 10L·h -1 In order to be closer to the application, the raw liquid simulated the magnesium-lithium mass ratio of salt lake brine to be 30, and the concentration was 2000 ppm. During the test, the nanofiltration membrane was first pre-pressed at 2 bar for 0.5 h. After the nanofiltration membrane reached a stable state, a sample was taken every 0.5 h and the permeate volume was recorded. To avoid errors, each sample was tested at least 3 times. The results are shown in Table 1.

[0082] Table 1 Separation performance of nanofiltration membranes prepared in Examples and Comparative Examples

[0083]

[0084]

[0085] From the data in Table 1, it can be seen that the magnesium-lithium separation and permeation flux of the PES / γ-CDA-TPC / PEI nanofiltration membrane prepared by the embodiment of the present invention are the highest. Li,Mg The permeation fluxes reached 22.5 and 6.5 L·m -2 ·h -1bar -1 . The scheme of the present invention utilizes that amine groups react more easily with TPC than hydroxyl groups, and induces at low temperature to cause most of the cyclodextrin cavities to be arranged vertically and distributed in the membrane, thereby constructing abundant and precise screening channels, and allowing the cavity of γ-CDA to perform secondary separation of magnesium and lithium; at the same time, a nano-sprayed PEI aqueous solution is used on the membrane surface, and the membrane surface with a high positive potential is more conducive to the separation of magnesium and lithium due to electrostatic effects, thereby obtaining an ultra-thin functional layer, shortening the mass transfer path, and reducing the mass transfer resistance of water and ions. This shows that the nanofiltration membrane of the scheme of the present invention has broad application prospects in the fields of seawater desalination and lithium extraction from salt lakes.

[0086] Comparative Example 2 uses trimesoyl chloride to replace terephthaloyl chloride. However, trimesoyl chloride cannot react with amino-modified γ-cyclodextrin to make it oriented, resulting in the inability to accurately and effectively separate the cavity, large water channel resistance, and a long transmission path, resulting in low permeability and separation.

[0087] The above is a detailed description of the embodiments of the present invention, but the present invention is not limited to the above embodiments. Various changes can be made within the knowledge scope of ordinary technicians in the relevant technical field without departing from the purpose of the present invention.

Claims

1. A method for preparing a Janus nanofiltration membrane, It is characterized in that The steps include: S1, performing free interface polymerization reaction of the aqueous phase monomer solution and the oil phase monomer solution on the surface of the base film 2 to form a composite film; S2, spraying polyethyleneimine solution on the surface of the composite membrane, heating and curing to obtain a Janus nanofiltration membrane; The components of the aqueous monomer solution include amino-modified γ-cyclodextrin; and the components of the oily monomer solution include terephthaloyl chloride.

2. The method for preparing the Janus nanofiltration membrane according to claim 1, It is characterized in that The concentration of the aqueous monomer solution is 0.2 wt.% to 0.5 wt.%.

3. The method for preparing the Janus nanofiltration membrane according to claim 1, It is characterized in that In step S1, the free interface polymerization reaction time is 1 minute to 5 minutes.

4. The method for preparing the Janus nanofiltration membrane according to claim 1, It is characterized in that The concentration of the oil phase monomer solution is 0.05 wt.% to 1 wt.%.

5. The method for preparing the Janus nanofiltration membrane according to claim 1, It is characterized in that In step S2, the spraying time is 1 second to 5 seconds.

6. The method for preparing the Janus nanofiltration membrane according to claim 1, It is characterized in that The amino-modified γ-cyclodextrin is prepared by the following method: Mix γ-cyclodextrin, N,N'-carbonyldiimidazole and an organic solvent, then add ethylenediamine and continue mixing and reacting to obtain the product.

7. The method for preparing the Janus nanofiltration membrane according to claim 1, It is characterized in that The temperature of the aqueous monomer solution is 10°C to 30°C.

8. A Janus nanofiltration membrane, It is characterized in that The compound is prepared by the preparation method according to any one of claims 1 to 7.

9. The Janus nanofiltration membrane according to claim 8, It is characterized in that The thickness of the Janus nanofiltration membrane is 20nm to 50nm.

10. Use of the Janus nanofiltration membrane according to claim 8 or 9 in seawater desalination or lithium extraction from salt lakes.

Citation Information

Patent Citations

  • Composite membrane for water treatment, and preparation method thereof

    CN106345318A

  • Polyester polyamide amphoteric charge composite nanofiltration membrane and preparation method thereof

    CN108905624A

  • Preparation method of nanofiltration membrane adopting polyethyleneimine / gamma-cyclodextrin composite monomer

    CN115770476A