Preparation method of gel ball for efficiently removing calcium and magnesium ions in seawater

Gel balls prepared by materials such as sodium alginate solve the problem of removing calcium and magnesium ions in seawater, achieving efficient, safe and low-cost calcium and magnesium ion adsorption effect, and are suitable for water treatment.

CN118976468APending Publication Date: 2024-11-19NINGBO UNIV
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411040112.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

The prior art is difficult to effectively remove calcium and magnesium ions in seawater, and common methods have problems such as complex preparation, pollution of the environment, and high cost. Biochar and zeolites perform poorly in adsorbing metal ions.

Method used

High-efficiency gel balls are prepared using materials such as sodium alginate, polyethylene glycol, polyvinyl alcohol and nano-calcium aluminate. The suspension is formed by magnetic stirring and dropper method, and then cured and elution in hydrochloric acid to form a stable Sodium alginate gel spheres use their polyanionic polyelectrolyte groups and hydroxyl and carboxyl groups to selective adsorption of calcium and magnesium ions.

Benefits of technology

The prepared gel balls are not easy to break, have high stability, strong selectivity and strong mechanical properties. They can efficiently and selectively remove calcium and magnesium ions in seawater. They are low-cost, safe and non-toxic, and are suitable for water treatment. Can be reused multiple times.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118976468A_ABST
    Figure CN118976468A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a gel ball for efficiently removing calcium and magnesium ions in seawater. The preparation method is characterized by comprising the following steps: mixing sodium alginate, polyethylene glycol, polyvinyl alcohol, nano calcium aluminate and deionized water according to a certain proportion to form turbid liquid; dripping the turbid liquid into a mixed solution containing calcium chloride and aluminum chloride, curing and settling to obtain coarse gel balls; finally, the coarse gel balls are soaked with a hydrochloric acid solution, calcium and aluminum ions in the coarse gel balls are removed, nano calcium aluminate in the coarse gel balls is dissolved, then the coarse gel balls are soaked with deionized water to be neutral, and the gel balls are obtained.The preparation method has the advantages that the preparation process is simple, conditions are easy to control, the cost is low, and the obtained gel balls are not prone to breakage and good in stability; the calcium and magnesium removal rate is high, the mass transfer property and the mechanical property are strong, and the characteristic of selectively adsorbing calcium and magnesium ions in seawater is realized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a calcium and magnesium ion remover in seawater, in particular to a preparation method of gel balls for efficiently removing calcium and magnesium ions in seawater. Background Art

[0002] Aquatic product processing is a high water consumption industry. Using purified seawater instead of drinking water to wash aquatic products not only solves the problem of water shortage, but also the seawater is rich in mineral elements such as potassium, selenium, zinc, vitamins, amino acids, humic acid, etc., which can not only improve the nutritional value of aquatic products, but also remove the fishy smell, increase the flavor, and reduce production costs. However, the content of calcium and magnesium ions in purified seawater is high, and it has a bitter taste, which is not suitable for the water requirements of the primary processing of aquatic products. When the concentration of calcium and magnesium ions is less than 450 mg / L, this purified seawater can be fully used for the water of the primary processing of aquatic products.

[0003] Commonly used methods for removing metal ions from water bodies include chemical precipitation, ion exchange, electrochemical method, membrane separation, etc. However, the above methods have problems such as complex preparation, environmental pollution, difficult regeneration, and inability to selectively remove. The adsorption method has attracted much attention due to its wide source of raw materials, simple operation method, low cost, safety and efficiency. It is one of the most commonly used water treatment methods.

[0004] The existing raw materials used for adsorption mainly include biochar, zeolite, bioalgae, etc. Biochar has a wide range of sources, such as straw, peanut shells, rice husks and lignin. Biochar has a low cost, but it is difficult to prepare, including raw material processing, carbonization, activation and other links. Each link requires professional technology and equipment, and the adsorption effect of biochar is very unstable. Different batches of raw materials and different preparation conditions will bring huge differences. Therefore, biochar still has many shortcomings in the adsorption of metal ions. Zeolite is a general term for a class of aluminum silicate minerals, which has a certain adsorption capacity for heavy metals. Zeolite is low in cost, but it is not easy to separate after agglomeration, has low adsorption efficiency, and poor resistance to impurity interference, so it is not outstanding in the field of adsorption of metal ions. Sodium alginate is widely distributed in nature, low in price, green and environmentally friendly, has good biocompatibility, environmental friendliness, non-toxicity and other advantages, and is widely used in the field of removal of water pollutants. However, the sodium alginate adsorption method is commonly used to remove heavy metal ions in water bodies, and there are almost no reports on the removal of calcium and magnesium ions. Summary of the invention

[0005] The technical problem to be solved by the present invention is to provide a preparation method of gel balls which are not easy to break, have good stability, high removal rate, good selectivity and strong mechanical properties and can efficiently remove calcium and magnesium ions from seawater.

[0006] The technical solution adopted by the present invention to solve the above technical problems is: a method for preparing gel balls for efficiently removing calcium and magnesium ions from seawater, which comprises the following steps: (1) Sodium alginate, polyethylene glycol, polyvinyl alcohol, nano calcium aluminate and deionized water are mixed in a certain proportion, heated to 50-60° C., and magnetically stirred at 100-120 rpm for 20-40 min to form a suspension; (2) dropping the suspension obtained in step (1) into a mixed solution containing 0.01 to 0.05 g / mL calcium chloride solution and 0.01 to 0.05 g / mL aluminum chloride solution at 50 to 60° C. using a dropper with a diameter of 0.05 to 0.1 mm, and solidifying and settling for 30 to 40 minutes to obtain crude gel spheres; (3) The crude gel balls obtained in step (2) are washed with 0.2-2 mol / L hydrochloric acid solution until no calcium ions and aluminum ions are detected in the HCl eluent, and then the crude gel balls are repeatedly washed with deionized water until neutral, and dried at 50-70° C. for 12-24 hours to obtain gel balls that can efficiently remove calcium and magnesium ions from seawater. Calcium and aluminum ions in the crude gel balls are removed, and nano calcium aluminate in the crude gel balls is dissolved.

[0007] Furthermore, the solid-to-liquid ratio of the sodium alginate, polyethylene glycol, polyvinyl alcohol, nano-calcium aluminate and deionized water described in step (1) is 2-4 g: 0.5-2 g: 0.5-2 g: 1-4 g: 100 mL.

[0008] Furthermore, the average diameter of the nano calcium aluminate described in step (1) is 1 to 5 nm.

[0009] Preferably, the specific steps are as follows: (1) Weigh 3 g of sodium alginate, 1 g of polyethylene glycol, 1 g of polyvinyl alcohol and 3 g of nano-calcium aluminate, add them into 100 ml of deionized water, heat to 55° C., stir magnetically at 110 rpm for 30 min, and mix well to form a suspension; wherein the average diameter of the nano-calcium aluminate is 1 to 5 nm; (2) dropping the suspension obtained in step (1) into a mixed solution containing 0.03 g / mL calcium chloride solution and 0.03 g / mL aluminum chloride at 55° C. using a dropper with a diameter of 0.1 mm, and solidifying and settling for 35 minutes to obtain crude gel spheres; (3) The crude gel spheres were immersed in 0.5 mol / L HCl for three times until no calcium ions and aluminum ions were detected in the HCl eluate, and then the crude gel spheres were repeatedly washed with deionized water until neutral, and then placed in a 60°C electric blast drying oven for 18 h to obtain gel spheres that can efficiently remove calcium and magnesium ions from seawater.

[0010] The principle of the present invention is as follows: Sodium alginate contains abundant hydroxyl and carboxyl groups, and has multiple anionic polyelectrolyte groups, which react with divalent and higher metal ions (Al 3+ , Ca 2+ etc.) enter the sodium alginate molecular chain and react with the Na + Ion exchange is carried out, and the metal ions enter the interior of the molecular chain and chelate with the carboxyl and oxygen atoms on the polyguluronic acid block, strengthening the synergistic effect between the molecular chains, thereby forming an alginate hydrogel with a stable structure. 2+ 、Al 3+ The G block molecular chain begins to stack and fold due to the bonding with the G residue, making the molecular chain of sodium alginate orderly and not easy to bend, forming a hydrogel with a three-dimensional network structure of calcium alginate or aluminum alginate. 2+ 、Al 3+ ions, causing the gel balls to form pores, which in turn allow the target metal ions to adhere to the pore surface and remove the target metal ions.

[0011] Polyethylene glycol is a water-soluble polymer with a wide molecular weight distribution. It is non-toxic, biocompatible, hydrophilic, highly ductile and tough. In aqueous solution, the ether bonds on the surface of its molecules carry a weak negative charge. 2+ With the participation of ions, alginate can be further converted into 2+ The bridges are connected to form a three-dimensional network structure of hydrogel, and then under the action of hydrochloric acid, the porosity of alginate is increased and its adsorption capacity is improved.

[0012] Nano calcium aluminate is a white cubic crystalline inorganic salt that is insoluble in water. After being mixed with sodium alginate, polyethylene glycol, and polyvinyl alcohol solutions, it is evenly distributed on the surface of sodium alginate hydrogel to form a suspension. At this time, the crude alginate gel balls prepared generate water-soluble aluminum chloride and calcium chloride when washed with hydrochloric acid, leaving more pores, thereby effectively increasing the binding sites of the gel balls to enhance their adsorption of calcium and magnesium ions.

[0013] Polyvinyl alcohol is a water-soluble polymer obtained by hydrolysis of polyvinyl acetate. It is cheap, non-toxic, and has good water solubility and biocompatibility. Polyvinyl alcohol contains many hydrophilic groups and is a flexible macromolecule. When preparing gel balls, the interchain hydroxyl hydrogen bond complexation can enhance the internal entanglement structure, improve the mechanical strength of the gel, and prevent the gel balls from cracking during the adsorption process.

[0014] When preparing alginate coarse gel spheres, Ca 2+ Contact with sodium alginate will quickly form a dense calcium alginate film layer on the surface of the droplet, affecting the sodium alginate inside the gel ball and preventing it from being absorbed by Ca 2+The replacement rate is low and the ball formation time is prolonged. 3+ The ball-forming speed is slow. Mixing calcium chloride and aluminum chloride can slow down the ball-forming speed, so that sodium alginate can combine with Ca 2+ 、Al 3+ Fully combined to effectively achieve internal reaction. And sodium alginate and Mg 2+ Unable to form gel balls, and Al 3+ With Mg 2+ The ionic radius is similar, so Al 3+ Replace Mg 2+ The prepared gel spheres can also enhance the Mg 2+ adsorption capacity.

[0015] In addition, the solution temperature is also an important factor in the preparation of crude gel spheres. 2+ 、Al 3+ The bonding rate with G residues is related to temperature. The hydrogel with three-dimensional network structure of calcium alginate or aluminum alginate formed at low temperature is too dense and has low bonding rate; while the hydrogel with three-dimensional network structure cannot be formed when the temperature is too high. The appropriate solution temperature is between 60 and 70°C. Since the reaction between calcium aluminate and hydrochloric acid is an exothermic reaction, the solution temperature can rise by 5 to 10°C. Therefore, the solution temperature should be controlled at 50 to 60°C before the reaction.

[0016] Compared with the prior art, the advantages of the present invention are: 1. Sodium alginate has a wide range of sources, is safe and non-toxic, low in price, and has a high raw material utilization rate; 2. The preparation process is simple, the removal process will not introduce new ions, will not pollute water bodies, and is green and environmentally friendly; 3. The prepared modified sodium alginate gel balls have good adsorption performance for calcium and magnesium ions, and can effectively and selectively remove calcium and magnesium ions without removing other ions except calcium and magnesium ions, and do not change other beneficial metal ions in seawater, which is conducive to the direct application of debittered seawater in the aquatic product processing industry; 4. The prepared modified sodium alginate gel spheres have high mechanical strength, are not easily damaged, are easy to separate from water, and can be reused many times after acid washing. After five repetitions, the adsorption capacity can still be maintained above 90%.

[0017] In summary, the present invention provides a method for preparing gel balls for efficiently removing calcium and magnesium ions from seawater. The method utilizes the property that sodium alginate is easy to form a gel when combined with calcium ions, and prepares the gel balls made of the material of the present invention which is low-cost, safe and non-toxic, and has good adsorption performance and mechanical properties. The adsorption amount of the gel balls is increased by polyethylene glycol and nano-calcium aluminate modification and coordinated temperature control, and the mechanical strength of the gel balls is increased by modification of polyvinyl alcohol. The method has the advantages of simple preparation, low cost, and selective adsorption, and no new ions are introduced into the water body after adsorption, and the method can be safely applied to the field of water treatment. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 The adsorption amount of Ca2+ by the gel balls prepared in Examples 1, 2, 3 and Comparative Examples 1 and 2; Figure 2 The adsorption amount of Mg2+ by the gel balls prepared in Examples 1, 2, 3 and Comparative Examples 1 and 2; Figure 3 This is a performance analysis diagram of the regeneration and recycling of gel balls; Figure 4 This is the SEM-EDS image of the gel ball after adsorbing seawater in Example 1, the left side is the SEM scanning electron microscope image, and the right side is the EDS energy spectrum image. DETAILED DESCRIPTION

[0019] The present invention is further described in detail below with reference to the accompanying drawings.

[0020] 1. Embodiment 1 A method for preparing gel balls for efficiently removing calcium and magnesium ions from seawater, the preparation method steps are as follows: (1) Weigh 3 g of sodium alginate, 1 g of polyethylene glycol, 1 g of polyvinyl alcohol and 3 g of nano-calcium aluminate, add them into 100 ml of deionized water, heat to 55° C., stir magnetically at 110 rpm for 30 min, and mix well to form a suspension; wherein the average diameter of the nano-calcium aluminate is 1 to 5 nm; (2) dropping the suspension obtained in step (1) into a mixed solution containing 0.03 g / mL calcium chloride solution and 0.03 g / mL aluminum chloride at 55° C. using a dropper with a diameter of 0.1 mm, and solidifying and settling for 35 minutes to obtain crude gel spheres; (3) The crude gel balls were immersed in 0.5 mol / L HCl for 3 times until no calcium ions and aluminum ions were detected in the HCl eluent (to remove calcium and aluminum ions in the crude gel balls and dissolve the nano-calcium aluminate in the crude gel balls). The crude gel balls were then repeatedly washed with deionized water until neutral, and then placed in a 60°C electric blast drying oven for 18 hours to obtain gel balls that can efficiently remove calcium and magnesium ions from seawater.

[0021] 0.05 g of the gel spheres prepared in this example were placed in a series of solutions with a pH of 5.0 and a concentration of 10-1100 mg / L of Ca(NO3)2·4H2O and Mg(NO3)2·6H2O (Ca 2+ Mg 2+ In the case of an ion concentration ratio of 1:1), the gel spheres 2+ Mg 2+ The adsorption amount of Figure 1 As shown. Figure 1 It can be seen that when Ca 2+ Mg 2+ When the solution concentration reaches 1100 mg / L, the gel ball has a 2+ The adsorption capacity of Mg reached 76.39 mg / g. 2+ The adsorption capacity reached 38.88 mg / g.

[0022] Example 2 The same as the above-mentioned Example 1, except that: in step (1), the solid-liquid ratio of sodium alginate, polyethylene glycol, polyvinyl alcohol, nano-calcium aluminate and deionized water is 2g (Note: 1g of sodium alginate cannot be spherical): 0.5g: 0.5g: 1g: 100mL; the temperature is 50°C, the magnetic stirring speed is 100 rpm, and the time is 40min; Step (2) is to drip the suspension into a mixed solution containing 0.01 g / mL calcium chloride solution and 0.01 g / mL aluminum chloride at 50° C. using a dropper with a diameter of 0.05 mm, and solidify and settle for 30 minutes; In step (3), the hydrochloric acid solution is 0.2 mol / L; the drying temperature is 50° C. and the drying time is 24 h.

[0023] 0.05 g of the gel spheres prepared in this example were placed in a series of solutions with a pH of 5.0 and a concentration of 10-1100 mg / L of Ca(NO3)2·4H2O and Mg(NO3)2·6H2O (Ca 2+ Mg 2+ In the case of an ion concentration ratio of 1:1), the gel spheres 2+ Mg 2+ The adsorption amount of Figure 1 As shown. Figure 1 It can be seen that when Ca 2+ Mg 2+ When the solution concentration reaches 1100 mg / L, the gel ball has a 2+ The adsorption capacity of Mg2+ reached 72.39 mg / g, and the adsorption capacity of Mg2+ reached 31.12 mg / g.

[0024] Example 3 The same as the above-mentioned Example 1, except that: in step (1), the solid-liquid ratio of sodium alginate, polyethylene glycol, polyvinyl alcohol, nano-calcium aluminate and deionized water is 4g:2g:2g:4g:100mL; the temperature is 60°C, the magnetic stirring speed is 120 rpm, and the time is 40min; Step (2) is to drip the suspension into a mixed solution containing 0.05 g / mL calcium chloride solution and 0.05 g / mL aluminum chloride at 60° C. using a dropper with a diameter of 0.1 mm, and solidify and settle for 40 minutes; In step (3), the hydrochloric acid solution is 2 mol / L; the drying temperature is 70° C. and the drying time is 12 h.

[0025] 0.05 g of the gel spheres prepared in this example were placed in a series of solutions with a pH of 5.0 and a concentration of 10-1100 mg / L of Ca(NO3)2·4H2O and Mg(NO3)2·6H2O (Ca 2+ Mg 2+ In the case of an ion concentration ratio of 1:1), the gel spheres 2+ Mg 2+ The adsorption amount of Figure 1 As shown. Figure 1 It can be seen that when Ca 2+ Mg 2+ When the solution concentration reaches 1100 mg / L, the gel ball has a 2+ The adsorption capacity of Mg2+ reached 74.72 mg / g, and the adsorption capacity of Mg2+ reached 34.85 mg / g.

[0026] Comparative Example 1 A method for preparing gel balls for efficiently removing calcium and magnesium ions from seawater, the preparation method steps are as follows: (1) Weigh 3 g of sodium alginate, 1 g of polyethylene glycol, 1 g of polyvinyl alcohol, and 3 g of nano-calcium aluminate, add them to 100 ml of deionized water, heat to 55°C, stir magnetically at 110 rpm for 30 min, and mix well to form a suspension; (2) dropping the suspension obtained in step (1) into a 0.03 g / mL calcium chloride solution at 55° C. using a dropper with a diameter of 0.1 mm, and solidifying and settling for 35 minutes to obtain crude gel spheres; (3) The crude gel spheres were immersed in 0.5 mol / L HCl for three times until no calcium ions and aluminum ions were detected in the HCl eluate, and then the crude gel spheres were repeatedly washed with deionized water until neutral, and then placed in a 60°C electric blast drying oven for 18 h to obtain gel spheres that can efficiently remove calcium and magnesium ions from seawater.

[0027] 0.05 g of the prepared gel spheres were placed in a series of solutions with pH 5.0 and concentrations ranging from 10 to 1100 mg / L of Ca(NO3)2·4H2O and Mg(NO3)2·6H2O (Ca 2+ Mg 2+ In the case of an ion concentration ratio of 1:1), the gel spheres 2+ Mg 2+ The adsorption amount of Figure 2 As shown. Figure 2 It can be seen that when Ca 2+ Mg 2+ When the total concentration of the solution reached 1100 mg / L, the gel ball had a 2+ The adsorption capacity of Mg reached 64.05 mg / g. 2+ The adsorption amount reached 27.51 mg / g.

[0028] Comparative Example 2 A method for preparing gel balls for efficiently removing calcium and magnesium ions from seawater, the preparation method steps are as follows: (1) Weigh 3 g of sodium alginate, 1 g of polyethylene glycol and 1 g of polyvinyl alcohol, add them into 100 ml of deionized water, heat to 55°C, stir magnetically at 110 rpm for 30 min, and mix well to form a suspension; (2) dropping the suspension obtained in step (1) into a 0.03 g / mL calcium chloride solution at 55° C. using a dropper with a diameter of 0.1 mm, and solidifying and settling for 35 minutes to obtain crude gel spheres; (3) The crude gel spheres were immersed in 0.5 mol / L HCl for three times until no calcium ions and aluminum ions were detected in the HCl eluate, and then the crude gel spheres were repeatedly washed with deionized water until neutral, and then placed in a 60°C electric blast drying oven for 18 h to obtain gel spheres that can efficiently remove calcium and magnesium ions from seawater.

[0029] 0.05 g of the prepared gel spheres were placed in a series of solutions with pH 5.0 and concentrations ranging from 10 to 1100 mg / L of Ca(NO3)2·4H2O and Mg(NO3)2·6H2O (Ca 2+ Mg 2+ In the case of an ion concentration ratio of 1:1), the gel spheres 2+ Mg 2+ The adsorption amount of Figure 3 As shown. Figure 3 It can be seen that when Ca 2+ Mg 2+ When the total concentration of the solution reached 1100 mg / L, the gel ball had a 2+ The adsorption capacity of Mg reached 61.47 mg / g. 2+ The adsorption amount reached 25.12 mg / g.

[0030] In summary, the adsorption effect of Example 1 on calcium and magnesium ions is better than that of the other cases. The adsorption of the example is better than that of the comparative example because the addition of nano calcium aluminate increases the adsorption sites of the gel balls and Al 3+ With Mg 2+ The ionic radius size is similar, with Al 3+ Replace Mg 2+ The prepared gel spheres can also enhance the Mg 2+ Therefore, the present invention selects the preparation method in Example 1 for application research.

[0031] 2. Experimental Results Analysis 1. Gel ball regeneration performance Wash the adsorbed Ca in Example 1 with HCl 2+ or Mg 2+ Repeat several times, 30 minutes each time, until no Ca2+ can be detected in the washing solution. 2+ Mg 2+ Then rinse the surface of the gel ball with deionized water to remove the H + Then, it was dried in an electric blast drying oven at 50°C, and 0.05 g of gel balls were added to 100 mg / L Ca(NO3)2·4H2O and Mg(NO3)2·6H2O (Ca 2+ Mg 2+ The adsorption was carried out for 5 cycles. Figure 4 It can be seen that when the concentration of the ion solution is 100 mg / L, the gel ball has a 2+ The adsorption capacity of Mg is 43.23 mg / g. 2+ The adsorption capacity of Ca 2+ The adsorption of Mg decreased by only 6.66%. 2+ The adsorption amount of Ca decreased by only 10.44%, and the gel ball repeatedly adsorbed Ca for 5 times. 2+ Mg 2+ There was no damage after use, which shows that the gel balls are reusable and have high mechanical properties and practical application value.

[0032] 2. Selectivity of gel balls Example 1: Adsorption of Ca in natural seawater 2+ Mg 2+ The gel spheres were characterized by EDS structure. Figure 4 As shown. Figure 4 It can be seen that Ca and Mg peaks appeared in the EDS spectrum, indicating that the gel ball successfully adsorbed calcium and magnesium ions. +, so these three elements have a higher content in the EDS spectrum. Figure 4 It can also be seen from the figure that the gel balls, in addition to absorbing calcium and magnesium ions, do not absorb beneficial trace elements such as selenium and zinc. It can be seen that the gel balls prepared by the present invention can achieve the absorption of Ca without affecting the beneficial elements in seawater. 2+ Mg 2+ The selective adsorption of the gel spheres indicated that the gel spheres obtained in this study could be applied in practical production.

[0033] 3. Application Examples 10 g of the gel spheres prepared in Example 1 were placed in a chromatography tube with a diameter of 10 mm and natural seawater (Ca 2+ Mg 2+ The contents were: 1287.49 mg and 411.16 mg respectively) and flowed through the chromatography column at a flow rate of 1 mL / s for dynamic adsorption. 2+ Mg 2 + A total of 10L of natural seawater was tested and the results showed that Ca 2+ Ion content is 59.19mg / L, Mg 2+ The ion content is 210.36 mg / L, and the total amount is 269.55 mg / L, which is far lower than the standard of calcium and magnesium ion concentration below 450 mg / L required for cleaning water, indicating that this technology has application prospects. The gel ball prepared by the present invention will remove Ca 2+ Mg 2+ The subsequent application of seawater in the aquatic product processing industry can not only reduce the use of freshwater resources, but also help maintain the freshness and taste of aquatic products in actual processing, and maximize the advantages of seawater processing of aquatic products.

[0034] The above description is not intended to limit the present invention, and the present invention is not limited to the above examples. Any changes, modifications, additions or substitutions made by a person skilled in the art within the spirit and scope of the present invention shall also fall within the protection scope of the present invention.

Claims

1. A method for preparing gel balls for efficiently removing calcium and magnesium ions from seawater, characterized in that The following steps are involved: (1) Sodium alginate, polyethylene glycol, polyvinyl alcohol, nano calcium aluminate and deionized water are mixed in a certain proportion, heated to 50-60° C., and magnetically stirred at 100-120 rpm for 20-40 min to form a suspension; (2) dropping the suspension obtained in step (1) into a mixed solution containing 0.01 to 0.05 g / mL calcium chloride solution and 0.01 to 0.05 g / mL aluminum chloride at 50 to 60° C. using a dropper with a diameter of 0.05 to 0.1 mm, and solidifying and settling for 30 to 40 minutes to obtain crude gel spheres; (3) The crude gel spheres obtained in step (2) are rinsed with a 0.2-2 mol / L hydrochloric acid solution until no calcium ions and aluminum ions are detected in the HCl eluate, and then the crude gel spheres are repeatedly rinsed with deionized water until neutral, and dried at 50-70° C. for 12-24 h to obtain gel spheres that can efficiently remove calcium and magnesium ions from seawater.

2. The method for preparing gel balls for efficiently removing calcium and magnesium ions from seawater according to claim 1, characterized in that: The solid-to-liquid ratio of the sodium alginate, polyethylene glycol, polyvinyl alcohol, nano-calcium aluminate and deionized water described in step (1) is 2-4 g: 0.5-2 g: 0.5-2 g: 1-4 g: 100 mL.

3. The method for preparing gel balls for efficiently removing calcium and magnesium ions from seawater according to claim 2, characterized in that: The average diameter of the nano calcium aluminate described in step (1) is 1 to 5 nm.

4. The method for preparing a gel ball for efficiently removing calcium and magnesium ions from seawater according to claim 2, characterized in that The specific steps are as follows: (1) Weigh 3 g of sodium alginate, 1 g of polyethylene glycol, 1 g of polyvinyl alcohol and 3 g of nano-calcium aluminate, add them into 100 ml of deionized water, heat to 55° C., stir magnetically at 110 rpm for 30 min, and mix well to form a suspension; wherein the average diameter of the nano-calcium aluminate is 1 to 5 nm; (2) dropping the suspension obtained in step (1) into a mixed solution containing 0.03 g / mL calcium chloride solution and 0.03 g / mL aluminum chloride at 55° C. using a dropper with a diameter of 0.1 mm, and solidifying and settling for 35 minutes to obtain crude gel spheres; (3) The crude gel spheres were immersed in 0.5 mol / L HCl for three times until no calcium ions and aluminum ions were detected in the HCl eluate, and then the crude gel spheres were repeatedly washed with deionized water until neutral, and then placed in a 60°C electric blast drying oven for 18 h to obtain gel spheres that can efficiently remove calcium and magnesium ions from seawater.

Citation Information

Patent Citations

  • Composite adsorption material for removing heavy metal ions and preparation method and application of composite adsorption material

    CN103752286A

  • Preparation method of sodium alginate / polyvinyl alcohol@polyacrylamide core-shell structure gel sphere and application of preparation method

    CN108187641A

  • Preparation method of sodium alginate gelatin ball

    CN109464989A

  • Preparation method of three-dimensional carrageenan / sodium alginate double network structure gel spheres

    CN109651653A

  • Treatment method of high-calcium wastewater and heavy metal ion industrial wastewater

    CN114031164A