Catalyst and catalytic preparation method of 2, 5-furandicarboxylic acid

By directly adding the first oxidant and inorganic alkali to the divalent copper brine solution and filtering, a catalyst without drying, grinding, or calcining is obtained, which is used to catalyze the preparation of FDCA, and the problem of cumbersome preparation steps and low efficiency in the prior art is solved. , achieving efficient and safe catalyst preparation and FDCA production.

CN118976490APending Publication Date: 2024-11-19PUTIAN DAKAI NEW MATERIALS CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410972152.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

The existing FDCA catalyst preparation methods require drying, grinding and calcining steps, resulting in low production efficiency, high energy consumption and safety hazards.

Method used

The first oxidant and inorganic base are added dropwise to the divalent copper saline solution, and the catalyst is obtained directly after filtration, and applied to the reaction of 5-hydroxymethylfurfural, second oxidant and alkali metal base to adjust the pH Values ​​are catalyzed to prepare 2,5-furandicarboxylic acid, avoiding drying, grinding and calcining steps.

Benefits of technology

The catalyst preparation process is simplified, the production efficiency and safety are improved, the catalytic efficiency is high, the conversion rate of 5-HMF is high, the FDCA is good, the catalyst can be reused, reducing energy consumption and cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004953552870000061
    Figure BDA0004953552870000061
  • Figure BDA0004953552870000062
    Figure BDA0004953552870000062
  • Figure BDA0004953552870000071
    Figure BDA0004953552870000071
Patent Text Reader

Abstract

The invention provides a catalyst and a catalytic preparation method of 2, 5-furandicarboxylic acid, and relates to the technical field of organic synthesis. The catalyst is prepared according to the following method: mixing a first oxidant and an inorganic base, dropwise adding the mixture into a bivalent copper salt aqueous solution with the concentration of 1-30wt%, continuously reacting for 3 minutes to 2 hours after dropwise adding, and filtering to obtain the catalyst. The catalyst disclosed by the invention is simple in preparation process, high in efficiency, low in cost and small in potential safety hazard, is used for catalyzing 5-HMF to prepare FDCA, and is high in catalytic efficiency.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of organic synthesis and relates to a catalyst and a catalytic preparation method of 2,5-furandicarboxylic acid. Background Art

[0002] 2,5-Furandicarboxylic acid (FDCA) has a similar structure to terephthalic acid (PTA) and can replace PTA for the preparation of bio-based polyester materials. The existing preparation method of FDCA mainly adopts the catalytic method of 5-hydroxymethylfurfural (5-HMF). In this catalytic method, the catalyst plays a very important role. The most studied method is the catalyst (such as nano copper oxide) + sodium hypochlorite catalytic oxidation method. However, in the prior art, when preparing the catalyst, after completing the preparation reaction of the catalyst, the catalyst usually needs to be dried, ground and roasted to obtain a nano-scale catalyst with good dispersibility. This undoubtedly greatly increases the preparation steps of the catalyst, has low efficiency and high energy consumption, requires special grinding equipment and roasting equipment, and roasting needs to be carried out at high temperature, which poses a great safety hazard.

[0003] Therefore, further research is still needed on the catalytic preparation of FDCA. Summary of the invention

[0004] Surprisingly, the inventors have found a preparation method that does not require drying, grinding and calcination during the catalyst preparation process, and the synthesized catalyst can be directly used in the catalytic preparation of FDCA, and the catalyst has high catalytic activity. To this end, the present invention provides a catalyst and a catalytic preparation method of 2,5-furandicarboxylic acid.

[0005] The technical solution of the present invention is as follows:

[0006] A catalyst is prepared by the following method: a first oxidant and an inorganic base are mixed, and the mixture is added dropwise to a divalent copper salt aqueous solution with a concentration of 1-30 wt%, and the reaction is continued for 3 min-2 h after the addition, and the catalyst is obtained by filtering.

[0007] Preferably, the first oxidant is selected from one or a combination of two or more of a hydrogen peroxide solution, a hypochlorite solution, a perchlorate solution, a chlorite solution and a chlorine dioxide solution, and the concentration of the first oxidant is not less than 5wt%.

[0008] Preferably, the inorganic base is selected from one or a combination of two or more of sodium hydroxide, potassium hydroxide, calcium hydroxide, barium hydroxide, sodium carbonate, potassium carbonate and lithium hydroxide.

[0009] Preferably, the divalent copper salt is selected from one or a combination of copper chloride and its hydrate, copper sulfate and its hydrate, copper acetate and its hydrate, and copper nitrate and its hydrate.

[0010] Preferably, the weight ratio of the first oxidant, the inorganic base and the divalent copper salt aqueous solution is 1-100:1:1-50.

[0011] A catalytic preparation method of 2,5-furandicarboxylic acid comprises the following steps: adding 5-hydroxymethylfurfural, a second oxidant and an alkali metal base into water and mixing them evenly; adding a catalyst in any of the above embodiments; reacting at 20-70° C. for 10-60 minutes; adjusting the pH to 1-3; and separating to obtain the 2,5-furandicarboxylic acid.

[0012] Preferably, the weight ratio of the 5-hydroxymethylfurfural, the second oxidant, the alkali metal base and the water is 1:1-300:0.7-3:1-500.

[0013] Preferably, the weight ratio of the 5-hydroxymethylfurfural to the catalyst is 1:0.5-20.

[0014] Preferably, the second oxidant is selected from one or a combination of two or more of a hydrogen peroxide solution, a hypochlorite solution, a perchlorate solution, a chlorite solution and a chlorine dioxide solution, and the concentration of the second oxidant is not less than 5wt%.

[0015] Preferably, the alkali metal base is selected from one or a combination of two or more of sodium hydroxide, potassium hydroxide, sodium carbonate and potassium carbonate.

[0016] The beneficial effects of the present invention are:

[0017] (1) The catalyst of the present invention does not require subsequent processing steps such as drying, grinding, and calcination during preparation, which greatly simplifies the production process and has the characteristics of high production efficiency and high safety. It does not require the use of special grinding equipment, calcination equipment, etc., and is conducive to industrial mass production.

[0018] (2) The catalyst of the present invention is used to catalyze the synthesis of 5-HMF to prepare FDCA, and has the characteristics of high catalytic efficiency, high conversion rate of 5-HMF, good selectivity of FDCA, and the catalyst can be reused multiple times after simple recovery treatment. DETAILED DESCRIPTION

[0019] The technical solution of the present invention is further illustrated and described below through specific implementation methods.

[0020] In order to solve the problems of the existing catalyst for catalyzing the synthesis of 5-HMF to prepare FDCA, such as the need for post-processing steps such as drying, grinding, and roasting, which lead to long process steps, low production efficiency, high energy consumption, and high safety hazards, the present invention provides a catalyst, which is prepared by the following method: a first oxidant and an inorganic base are mixed, and the mixture is added dropwise to a divalent copper salt aqueous solution with a concentration of 1-30wt%, and the reaction is continued for 3min-2h after the addition, and the catalyst is filtered to obtain a catalyst.

[0021] The catalyst preparation method of the present invention can be used directly after filtering after the synthesis reaction is completed, without the steps of drying, grinding, roasting, etc., and has a short process, high efficiency, low energy consumption, high safety, and is suitable for industrial mass production. Calculated based on the production of 100g of catalyst at a time, compared with the existing catalyst preparation method, the process time of the catalyst preparation method of the present invention can be shortened by more than 60%, and the energy consumption can be reduced by more than 80%.

[0022] In a preferred embodiment, the first oxidant is selected from one or a combination of two or more of hydrogen peroxide solution, hypochlorite solution, perchlorate solution, chlorite solution and chlorine dioxide solution, and the concentration of the first oxidant is not less than 5wt%. For example, the first oxidant can be a sodium hypochlorite aqueous solution, a sodium perchlorate aqueous solution, a hydrogen peroxide solution, etc., and the concentration of the first oxidant can be any value of 5wt%, 6wt%, 7wt%, 8wt%, 9wt%, 10wt%, 11wt%, 12wt%, etc., but is not limited to the above.

[0023] In a preferred embodiment, the inorganic base is selected from one or a combination of two or more of sodium hydroxide, potassium hydroxide, calcium hydroxide, barium hydroxide, sodium carbonate, potassium carbonate and lithium hydroxide. More preferably, the inorganic base can be sodium hydroxide, potassium hydroxide or sodium carbonate.

[0024] In a preferred embodiment, the divalent copper salt is selected from one or more combinations of copper chloride and its hydrate, copper sulfate and its hydrate, copper acetate and its hydrate, and copper nitrate and its hydrate. For example, the divalent copper salt can be copper sulfate, copper sulfate pentahydrate, copper chloride, and copper nitrate. Further preferably, the concentration of the divalent copper salt aqueous solution can be 5-20wt%, such as 5wt%, 6wt%, 7wt%, 8wt%, 9wt%, 10wt%, 11wt%, 12wt%, 13wt%, 14wt%, 15wt%, 16wt%, 17wt%, 18wt%, 19wt%, 20wt%, etc., but not limited to the above.

[0025] In a preferred embodiment, the weight ratio of the first oxidant, the inorganic base and the divalent copper salt aqueous solution is 1-100:1:1-50. For example, the weight ratio of the first oxidant, the inorganic base and the divalent copper salt aqueous solution can be any value in 1:1:1, 10:1:1, 10:1:20, 20:1:20, 20:1:30, 20:1:40, 30:1:1, 50:1:1, 100:1:1, 30:1:10, 30:1:30, 30:1:50, 50:1:5, 100:1:20, 50:1:20, etc., but is not limited to the above-listed values.

[0026] On the other hand, the present invention provides a catalytic preparation method of 2,5-furandicarboxylic acid, wherein the catalyst obtained above is directly used to catalyze 5-HMF to prepare FDCA. The specific method may be: 5-hydroxymethylfurfural, a second oxidant and an alkali metal base are added to water and mixed evenly, the catalyst in any of the above embodiments is added, reacted at 20-70° C. for 10-60 min, the pH is adjusted to 1-3, and separated to obtain 2,5-furandicarboxylic acid.

[0027] In a preferred embodiment, the weight ratio of 5-hydroxymethylfurfural, the second oxidant, the alkali metal base and water is 1:1-300:0.7-3:1-500. For example, the weight ratio of 5-hydroxymethylfurfural, the second oxidant, the alkali metal base and water can be any value in 1:1:0.7:1, 1:50:1:1, 1:50:1:100, 1:50:1:300, 1:100:1:250, 1:100:2:200, 1:100:2:500, 1:200:1:300, 1:200:2:300, 1:200:2:500, 1:200:3:300, 1:300:3:150, 1:300:3:300, 1:300:3:500, etc., but not limited to the above.

[0028] In a preferred embodiment, the weight ratio of 5-hydroxymethylfurfural and the catalyst is 1:0.5-20. For example, the weight ratio of 5-hydroxymethylfurfural and the catalyst can be any value of 1:0.5, 1:1, 1:2, 1:3, 1:4, 1:5, 1:6, 1:7, 1:8, 1:9, 1:10, 1:11, 1:12, 1:13, 1:14, 1:15, 1:16, 1:17, 1:18, 1:19, 1:20, etc., but not limited to the above. Further, the weight ratio of 5-hydroxymethylfurfural and the catalyst is 1:1-20, or further, the weight ratio is 1:1-10. A high amount of catalyst can still achieve a very high catalytic effect, but there is no obvious improvement in efficiency. Therefore, from the cost dimension, the amount of catalyst does not need to be very high.

[0029] In a preferred embodiment, the second oxidant is selected from one or a combination of two or more of hydrogen peroxide solution, hypochlorite solution, perchlorate solution, chlorite solution and chlorine dioxide solution, and the concentration of the second oxidant is not less than 5wt%. For example, the second oxidant can be a sodium hypochlorite aqueous solution, a sodium perchlorate aqueous solution, a hydrogen peroxide solution, etc., and the concentration of the second oxidant can be any value of 5wt%, 6wt%, 7wt%, 8wt%, 9wt%, 10wt%, 11wt%, 12wt%, etc., but is not limited to the above-listed values.

[0030] In a preferred embodiment, the alkali metal base is selected from one or a combination of two or more of sodium hydroxide, potassium hydroxide, sodium carbonate and potassium carbonate.

[0031] The technical solution of the present invention is further described and illustrated according to various embodiments below.

[0032] Example 1-6 Preparation of Catalyst

[0033] Example 1

[0034] 20 g of copper sulfate was added to 180 g of water, stirred to dissolve, and a mixed solution consisting of 10 g of sodium hydroxide and 100 g of 10 wt% sodium hypochlorite solution was added dropwise thereto. After the addition was complete, the mixture was stirred for 20 min and filtered. The solid product obtained was the catalyst.

[0035] Example 2

[0036] The difference between Example 2 and Example 1 is that in Example 1, copper sulfate is replaced by an equal weight of copper nitrate. The remaining steps remain unchanged.

[0037] Example 3

[0038] 20 g of copper sulfate was added to 280 g of water, stirred to dissolve, and a mixed solution consisting of 10 g of sodium hydroxide and 200 g of 6 wt% sodium hypochlorite solution was added dropwise thereto. After the addition was complete, the mixture was stirred for 50 min and filtered. The resulting solid product was the catalyst.

[0039] Example 4

[0040] The difference between Example 4 and Example 3 is that in Example 3, copper sulfate is replaced by an equal weight of copper acetate. The remaining steps remain unchanged.

[0041] Example 5

[0042] 20 g of copper sulfate was added to 380 g of water, stirred to dissolve, and a mixed solution consisting of 10 g of sodium hydroxide and 200 g of 10 wt% sodium hypochlorite solution was added dropwise thereto. After the addition was complete, the mixture was stirred for 20 min and filtered. The solid product obtained was the catalyst.

[0043] Example 6

[0044] 20 g of copper chloride was added to 130 g of water, stirred to dissolve, and a mixed solution consisting of 10 g of sodium hydroxide and 100 g of 10 wt% hydrogen peroxide was added dropwise thereto. After the addition was complete, the mixture was stirred for 20 min and filtered. The solid product obtained was the catalyst.

[0045] Comparative Example 1

[0046] The catalyst of Comparative Example 1 was prepared as a nano-CuO catalyst according to the method of the journal article “Research on the Catalytic Synthesis of 2,5-Furandicarboxylic Acid by 5-Hydroxymethylfurfural” (Modern Chemical Industry, September 2019, Vol. 39, No. 9, 135-140).

[0047] Example 7

[0048] 2 g of the catalyst to be tested was added to a reaction container, and 1 g of 5-HMF, 250 g of water, 1 g of sodium hydroxide and 100 g of 10% sodium hypochlorite solution were added. The mixture was stirred at 25°C for 60 min. After the reaction was completed, a sample was taken, diluted to a fixed volume, and then tested by HPLC.

[0049] The results are shown in Table 1 below, where the blank refers to the case where no catalyst was added.

[0050] Assuming that the initial 5-HMF molar amount is W1, the remaining 5-HMF molar amount after the reaction is W2, and the FDCA molar amount in the reaction solution is W3,

[0051] 5-HMF conversion = (W1-W2) / W1 x 100%.

[0052] FDCA conversion rate = (W3-W2) / W1×100%.

[0053] Table 1

[0054]

[0055] From the results in Table 1 above, it can be seen that the catalyst of the present invention is used for catalytic preparation of FDCA from 5-HMF, the conversion rate of 5-HMF is complete, the yield of FDCA is very high, and the catalytic efficiency is basically the same as that of the nano copper oxide catalyst in the prior art. However, from the actual production dimension of the catalyst, the catalyst of the present invention does not require drying, grinding, roasting and other processes in preparation. According to the calculation of Example 1 and Comparative Example 1, compared with Comparative Example 1, the production time of Example 1 can be shortened by more than 80%, the energy consumption can be reduced by more than 90%, and there is no need for relatively expensive grinding equipment, roasting equipment and other investment, the cost is lower, and the safety is also higher.

[0056] Example 8

[0057] Different weights of the catalyst obtained in Example 1 were added to a reaction container, and 1 g of 5-HMF, 400 g of water, 2 g of sodium hydroxide and 200 g of 8% sodium hypochlorite solution were added, and the mixture was stirred at 25° C. for 60 min. After the reaction was completed, the mixture was sampled, diluted and fixed to volume for HPLC detection. The results are shown in Table 2 below, where Comparative Example 2 uses the nano CuO catalyst in Comparative Example 1 above, and the feed weight is 0.5 g.

[0058] Table 2

[0059]

[0060]

[0061] From the data results in Table 2 above, it can be seen that with the increase in the amount of catalyst used, the conversion rate of 5-HMF and the yield of FDCA are both improved within a certain range. When the weight ratio of the catalyst of the present invention to 5-HMF is 2:1 or above, a very high catalytic effect can be achieved, the conversion rate of 5-HMF is basically complete, and the yield of FDCA is about 99.8%. Moreover, when the weight ratio of the catalyst to 5-HMF is 1:2 using the existing nano CuO catalyst, the catalytic efficiency of the nano CuO catalyst is not high, and the catalytic effect is basically the same as that of the catalyst of the present invention.

[0062] Example 9

[0063] 2 g of the catalyst of Example 1 was added to a reaction container, and 1 g of 5-HMF, 200 g of water, 1.5 g of sodium hydroxide and 50 g of a 12% sodium hypochlorite solution were added, and stirred at different temperatures for different times. After the reaction was completed, the sample was diluted and fixed to volume for HPLC detection. The detection results are shown in Table 3.

[0064] Table 3

[0065] Temperature / ℃ Reaction time / min 5-HMF conversion rate / % FDCA yield / % 20 60 100 99.83 20 40 100 99.91 50 40 100 98.32 50 25 100 99.67 70 25 100 97.63 70 10 100 99.55

[0066] From the data in Table 3, it can be seen that the catalyst of the present invention has a good catalytic effect under the reaction conditions of different reaction temperatures and reaction times, and the conversion of 5-HMF is substantially complete. By adjusting the reaction time at different reaction temperatures, the yield of FDCA can reach more than 99.5%.

[0067] Example 10

[0068] 2 g of the catalyst of Example 1 was added to a reaction container, and 1 g of 5-HMF, 150 g of water, 1 g of sodium hydroxide and 200 g of a 5% sodium hypochlorite solution were added. After stirring at 25° C. for 40 min, a sample was taken, diluted to a fixed volume, and then tested by HPLC.

[0069] After the reaction was completed, the catalyst was filtered out, washed twice with 300 g of water, and then ground for 0.5 h. The test was repeated according to the above reaction conditions. The results are shown in Table 4 below.

[0070] Table 4

[0071]

[0072] It can be seen from the results in Table 4 that the catalyst of the present invention can be reused for 5 times and still achieve a good catalytic effect, and the method of reuse is relatively simple.

[0073] As described above, the basic principles, main features and advantages of the present invention are shown and described. Those skilled in the art should understand that the present invention is not limited by the above embodiments, which are only preferred embodiments of the present invention and cannot be used to limit the scope of the present invention. That is, equivalent changes and modifications made according to the scope of the present invention and the content of the specification should still be within the scope of the present invention. The scope of protection required by the present invention is defined by the attached claims and their equivalents.

Claims

1. A catalyst, characterized in that The preparation method is as follows: the first oxidant and the inorganic base are mixed, and the mixture is added dropwise to a divalent copper salt aqueous solution with a concentration of 1-30 wt %, and the reaction is continued for 3 min-2 h after the addition, and the catalyst is obtained by filtering.

2. The catalyst according to claim 1, characterized in that The first oxidant is selected from one or a combination of two or more of a hydrogen peroxide solution, a hypochlorite solution, a perchlorate solution, a chlorite solution and a chlorine dioxide solution, and the concentration of the first oxidant is not less than 5 wt %.

3. The catalyst according to claim 1, characterized in that The inorganic base is selected from one or a combination of two or more of sodium hydroxide, potassium hydroxide, calcium hydroxide, barium hydroxide, sodium carbonate, potassium carbonate and lithium hydroxide.

4. The catalyst according to claim 1, characterized in that The divalent copper salt is selected from one or a combination of copper chloride and its hydrate, copper sulfate and its hydrate, copper acetate and its hydrate, and copper nitrate and its hydrate.

5. The catalyst according to claim 1, characterized in that The weight ratio of the first oxidant, the inorganic base and the divalent copper salt aqueous solution is 1-100:1:1-50.

6. A catalytic preparation method of 2,5-furandicarboxylic acid, characterized in that: 5-Hydroxymethylfurfural, a second oxidant and an alkali metal base are added to water and mixed evenly, and the catalyst according to any one of claims 1 to 5 is added, reacted at 20 to 70° C. for 10 to 60 minutes, the pH is adjusted to 1 to 3, and separated to obtain the 2,5-furandicarboxylic acid.

7. The catalytic preparation method of 2,5-furandicarboxylic acid according to claim 6, characterized in that: The weight ratio of the 5-hydroxymethylfurfural, the second oxidant, the alkali metal base and the water is 1:1-300:0.7-3:1-500.

8. The catalytic preparation method of 2,5-furandicarboxylic acid according to claim 6, characterized in that: The weight ratio of the 5-hydroxymethylfurfural to the catalyst is 1:0.5-20.

9. The catalytic preparation method of 2,5-furandicarboxylic acid according to claim 6, characterized in that: The second oxidant is selected from one or a combination of two or more of a hydrogen peroxide solution, a hypochlorite solution, a perchlorate solution, a chlorite solution and a chlorine dioxide solution, and the concentration of the second oxidant is not less than 5 wt %.

10. The catalytic preparation method of 2,5-furandicarboxylic acid according to claim 6, characterized in that: The alkali metal base is selected from one or a combination of two or more of sodium hydroxide, potassium hydroxide, sodium carbonate and potassium carbonate.

Citation Information

Patent Citations

  • Method for synthesizing 2, 5-furandicarboxylic acid

    CN109678823A

  • Preparation method of 2,5-furandicarboxylic acid under mild condition

    CN112830916A

  • Catalyst, preparation method thereof and method for preparing 2, 5-furandicarboxylic acid through catalysis of catalyst

    CN116408081A

  • Preparation method of FDCA and FDCA product

    CN116675660A

  • Preparation method of 2, 5-furandimethanol

    CN117229238A