Catalyst for preparing methanol through carbon dioxide hydrogenation and preparation method thereof

By developing copper-zinc titanium catalysts, the problems of reducing selectivity of existing catalysts at high temperatures and difficulty in activation at low temperatures are solved, the CO2 conversion rate and methanol selectivity are improved, the stability and reaction activity of the catalyst are achieved, and it is suitable for carbon dioxide hydrogenation. Methanol reaction.

CN118976501APending Publication Date: 2024-11-19HUANENG CLEAN ENERGY RES INST +1
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411258390.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-09
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

The existing carbon dioxide hydrogenation catalysts are selectively reduced at high temperatures and are difficult to activate at low temperatures. Traditional copper-based catalysts have poor water resistance and poor stability, resulting in low CO2 conversion and methanol selectivity, making it difficult to maintain long-term stability. .

Method used

Develop a copper-zinc titanium-based catalyst with a chemical composition of CuaZnbTiOx, a Cu element content of 3 to 40 wt%, and an initial reduction temperature of no more than 135°C. The reaction activity and stability of the catalyst are improved by specific preparation methods, including the use of organic The aqueous solution of titanate, copper, zinc salt and complexing agent is reacted and the catalyst is formed by drying and calcining treatment.

Benefits of technology

It significantly improves CO2 conversion, methanol selectivity and methanol yield, reduces the incidence of side reactions, enhances the stability and reduction performance of the catalyst, and is suitable for the hydrogenation of carbon dioxide at low temperature conditions to methanol.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118976501A_ABST
    Figure CN118976501A_ABST
Patent Text Reader

Abstract

The invention provides a catalyst for preparing methanol by hydrogenation of carbon dioxide and a preparation method thereof, the catalyst has a chemical composition of CuaZnbTiOx, a is more than 0 and less than or equal to 2.1, b is more than 0 and less than or equal to 2.1, and x is equal to 2 + a + b; the content of the Cu element is 3-40 wt%, and in an H2-TPR test of the catalyst, the initial reduction temperature of the catalyst is not higher than 135 DEG C. When the catalyst is applied to a reaction for preparing methanol through carbon dioxide hydrogenation, the CO2 conversion rate, the methanol selectivity and the methanol yield can be obviously improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of catalysts and relates to a catalyst for preparing methanol by hydrogenating carbon dioxide, and in particular to a catalyst for preparing methanol by hydrogenating carbon dioxide and a preparation method thereof. Background Art

[0002] Due to the extensive use of fossil fuels such as coal and oil by humans, a large amount of CO2 is emitted, causing global environmental and energy problems. In this context, the reduction and utilization of CO2 has attracted much attention. Among the many CO2 conversion technologies, the hydrogenation of CO2 to methanol has great development potential. This is because CO2 hydrogenation to methanol not only directly converts CO2 into methanol, an important chemical intermediate, but also can use this technology to store hydrogen in methanol for energy storage. With the development of water electrolysis hydrogen production technology, the cost of hydrogen continues to decrease, and the economy and feasibility of CO2 hydrogenation to methanol have been greatly improved.

[0003] CO2 hydrogenation to methanol is an endothermic reaction. High temperature is not conducive to the reaction, but is conducive to the reverse water gas shift (RWGS) side reaction. Therefore, high temperature will reduce the selectivity of methanol. However, it is very difficult to activate CO2 at low temperature. Metal catalysts can activate CO2 at low temperature and react. The catalysts reported for low-temperature CO2 hydrogenation to methanol mainly include: copper-based catalysts, oxide catalysts, precious metal catalysts and new catalysts represented by molybdenum sulfide, such as CuO, ZnO, Al2O3, Cr2O3, or mixed oxides of Zn and Al. Among them, copper-based catalysts are widely used due to their high reaction activity and methanol space-time yield. However, traditional copper-based catalysts have poor water resistance and high Cu content, which easily lead to sintering of active sites, seriously affecting catalytic activity and stability. In addition, the current catalysts still have low CO2 conversion rate and are difficult to maintain long-term stability during continuous reaction.

[0004] Therefore, there is an urgent need to develop a catalyst with high catalytic activity and stability for the hydrogenation of carbon dioxide to methanol, so as to improve the CO2 conversion rate, methanol selectivity and methanol yield. Summary of the invention

[0005] In view of the above-mentioned defects, the present invention provides a catalyst for producing methanol by hydrogenating carbon dioxide. The content of Cu element in the catalyst is 3-40wt%, and the initial reduction temperature is not higher than 135°C. The catalyst has strong reducing ability, so the catalyst can significantly improve the CO2 conversion rate, methanol selectivity and methanol yield.

[0006] The present invention also provides a method for preparing the catalyst for producing methanol by hydrogenating carbon dioxide. The catalyst prepared by the preparation method can significantly improve the CO2 conversion rate, methanol selectivity and methanol yield.

[0007] The present invention also provides a method for producing methanol by hydrogenating carbon dioxide, by which the CO2 conversion rate, methanol selectivity and methanol yield can be effectively improved.

[0008] The present invention provides a catalyst for preparing methanol by hydrogenating carbon dioxide, which has a chemical composition of formula 1, and a Cu content of 3 to 40 wt%.

[0009] Cu a Zn b TiO x Formula 1

[0010] In formula 1, 0<a≤2.1, 0<b≤2.1, x=2+a+b;

[0011] In the H2-TPR test of the catalyst, the initial reduction temperature of the catalyst is not higher than 135°C.

[0012] The present invention also provides a method for preparing the catalyst for producing methanol by hydrogenating carbon dioxide, comprising the following steps:

[0013] (1) adding an organic solvent solution including an organic titanate dropwise to an aqueous solution including a copper salt, a zinc salt, and a complexing agent to obtain a mixed solution, heating the mixed solution to 40 to 70° C. and stirring, reacting for 1 to 4 hours, then heating the mixed solution to 80 to 100° C. until the residual water content is less than 30%, stopping stirring, and maintaining the temperature for 1 to 4 hours for aging to obtain a first product;

[0014] In the mixed solution, the molar concentration of the organic titanate is 0.015-0.4 mol / L, the molar concentration of the copper salt is 0.02-0.4 mol / L, the molar concentration of the zinc salt is 0.03-0.75 mol / L, and the molar concentration of the complexing agent is 0.1-2.5 mol / L;

[0015] (2) Drying the first product to obtain a catalyst precursor, and calcining the catalyst precursor to obtain the catalyst.

[0016] Furthermore, in step (1), the dropping speed is 0.05 to 1 mL / s.

[0017] Furthermore, in step (1), the stirring speed is 60 to 400 r / min.

[0018] Furthermore, in step (2), the drying temperature is 105-150° C. and the drying time is 2-6 hours.

[0019] Furthermore, in step (2), the heating rate during the roasting process is 1.5-2°C / min, the roasting temperature is 350-550°C, and the holding time is 3-6h.

[0020] Further, the organic titanate includes at least one of tetrabutyl titanate and titanium isopropoxide;

[0021] And / or, the copper salt includes at least one of copper nitrate trihydrate and anhydrous copper acetate;

[0022] And / or, the zinc salt includes at least one of anhydrous zinc acetate and zinc nitrate;

[0023] And / or, the complexing agent includes at least one of chitosan, glucose, citric acid and fructose.

[0024] The present invention also provides a method for preparing methanol by hydrogenating carbon dioxide, wherein carbon dioxide is hydrogenated using any of the above catalysts or a catalyst prepared by any of the above methods for preparing a catalyst for hydrogenating carbon dioxide to prepare methanol to obtain methanol.

[0025] Further, the following steps are included:

[0026] The catalyst is placed in a reactor, a raw material mixed gas is introduced at a flow rate of 15 to 85 mL / min, and a carbon dioxide hydrogenation to methanol reaction is carried out at 230 to 310° C. and 1 to 5 MPa;

[0027] The raw mixed gas includes hydrogen, carbon dioxide and nitrogen;

[0028] The volume ratio of the hydrogen to the carbon dioxide is (3-5):1, and the volume percentage of the nitrogen is 4-10%.

[0029] The catalyst chemical composition of the present invention is Cu a Zn b TiO x The CuO, ZnO and TiO2 therein cooperate with each other and influence each other, which can effectively improve the reaction activity and stability of the catalyst; and the Cu element content in the catalyst is between 5 and 35wt%, which can not only effectively reduce the risk of sintering and reduce the loss of active sites, but also reduce the occurrence of side reactions in the carbon dioxide hydrogenation to methanol reaction and improve methanol selectivity; at the same time, in the H2-TPR test of the catalyst, the initial reduction temperature of the catalyst is low, not higher than 135°C, which shows that the catalyst has good reduction performance and reaction activity, which is conducive to the carbon dioxide hydrogenation to methanol reaction at low temperature, thereby further improving the carbon dioxide conversion rate, methanol selectivity and methanol yield of the reaction. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 H2-TPR test graphs of the catalysts prepared in Example 2 of the present invention and Comparative Example 10;

[0031] Figure 2 It is the CO2-TPD test graph of the catalyst prepared in Example 2 of the present invention and Comparative Example 10;

[0032] Figure 3 The stability test results of the catalyst prepared in Example 1 of the present invention are shown. DETAILED DESCRIPTION

[0033] In order to make the purpose, technical solutions and advantages of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0034] The first aspect of the present invention provides a catalyst for preparing methanol by hydrogenating carbon dioxide, which has a chemical composition of Formula 1 and a Cu content of 3 to 40 wt%.

[0035] Cu a Zn b TiO x Formula 1

[0036] In formula 1, 0<a≤2.1, 0<b≤2.1, x=2+a+b;

[0037] In the H2-TPR test of the catalyst, the initial reduction temperature of the catalyst is no higher than 135°C.

[0038] The content of the Cu element in the present invention can be calculated based on the chemical composition of the catalyst finally prepared.

[0039] The initial reduction temperature in the present invention refers to the temperature corresponding to when copper oxide in the catalyst is reduced by hydrogen and begins to produce water as the temperature rises in the H2-TPR test of the catalyst.

[0040] The H2-TPR test of the catalyst in the present invention comprises the following steps:

[0041] The above catalyst was ground and crushed, and a catalyst with a mesh size of 20 to 40 was sieved for testing; the catalyst with a mesh size of 20 to 40 was loaded into a quartz fixed bed reactor, and was first purged with Ar, and the temperature was raised to 350° C. to dehydrate the catalyst, and after it was cooled to room temperature, a mixed gas containing 10% H2 and 90% Ar was introduced, and the temperature was raised to 400° C. at 15° C. / min while the mixed gas was introduced, and during this process, a mass spectrometer was used to detect the fragment molecules of H2O and H2, and the response was observed to obtain a H2-TPR test curve.

[0042] The catalyst of the present invention is a copper-zinc-titanium catalyst, and its chemical composition is Cu a Zn b TiO x The Cu element can form a better crystal interface synergistic effect with ZnO and TiO2, increase the reaction active sites on the catalyst surface, and the three cooperate with each other and influence each other, thereby improving the reaction activity and stability of the catalyst; and the Cu element content in the catalyst is 3-40wt%. Within this range, the generation of effective side reactions can be reduced, the methanol selectivity can be improved, and the active site sintering phenomenon is not easy to occur, which can effectively avoid the loss of active sites caused by sintering, and ensure that the catalyst has high activity and stability; at the same time, in the H2-TPR test of the catalyst, the initial reduction temperature of the catalyst is low, not higher than 135°C, indicating that the catalyst has good reduction performance and reaction activity, and can undergo reduction reaction at a lower temperature, which is conducive to the smooth progress of the carbon dioxide hydrogenation to methanol reaction, thereby comprehensively improving the carbon dioxide conversion rate, methanol selectivity and methanol yield. When the Cu element content exceeds the range of 3 to 40wt%, due to the low Tammann temperature of Cu, sintering is likely to occur during the catalyst preparation process, resulting in loss of active sites and reduced CO2 conversion rate; at the same time, excessive Cu content will lead to increased CO generation in the carbon dioxide hydrogenation to methanol reaction, which in turn will lead to reduced methanol selectivity and thus reduced methanol yield.

[0043] The second aspect of the present invention provides a method for preparing the catalyst for producing methanol by hydrogenating carbon dioxide according to the first aspect, comprising the following steps:

[0044] (1) adding an organic solvent solution including an organic titanate dropwise to an aqueous solution including a copper salt, a zinc salt, and a complexing agent to obtain a mixed solution, heating the mixed solution to 40 to 70° C. and stirring, reacting for 1 to 4 hours, then heating the mixed solution to 80 to 100° C. until the residual water content is less than 30%, stopping stirring, and maintaining the temperature for 1 to 4 hours for aging to obtain a first product;

[0045] In the mixed solution, the molar concentration of the organic titanate is 0.015-0.4 mol / L, the molar concentration of the copper salt is 0.02-0.4 mol / L, the molar concentration of the zinc salt is 0.03-0.75 mol / L, and the molar concentration of the complexing agent is 0.1-2.5 mol / L;

[0046] (2) Drying the first product to obtain a catalyst precursor, and calcining the catalyst precursor to obtain a catalyst.

[0047] Specifically, in step (1), an organic solvent solution including an organic titanate is added dropwise to an aqueous solution including a copper salt, a zinc salt and a complexing agent to obtain a mixed solution; in the mixed solution, the molar concentration of the organic titanate is 0.015-0.4 mol / L, the molar concentration of the copper salt is 0.02-0.4 mol / L, the molar concentration of the zinc salt is 0.03-0.75 mol / L, and the molar concentration of the complexing agent is 0.1-2.5 mol / L; the reaction system is heated to 40-70°C and stirred, and after reacting for 1-4 hours, the temperature is further raised to 80-100°C to evaporate the water in the reaction system. When the residual water content in the reaction system is less than 30%, the reactants in the reaction system are in a gelatinous state, stirring is stopped, and the mixture is allowed to stand at a constant temperature for 1-4 hours for aging, and the first product is obtained after the aging is completed.

[0048] Preferably, stirring may be performed during the dropwise addition process to allow the organic solvent solution including the organic titanate to be better dispersed in the reaction system. Preferably, the stirring speed is 60 to 400 r / min.

[0049] The present invention does not specifically limit the dropping speed during the dropping process and the stirring speed during the stirring process after heating to 40 to 70° C.

[0050] The present invention does not specifically limit the types of the organic titanate, copper salt, zinc salt and complexing agent.

[0051] The present invention does not specifically limit the type of the organic solvent. For example, the organic solvent includes at least one of ethanol, methanol, and propanol.

[0052] The present invention does not limit the sources of the organic titanate, copper salt, zinc salt, and complexing agent, and they can be obtained, for example, through commercial sources or conventional preparation methods.

[0053] The present invention does not limit the manner of dripping and stirring. For example, dripping can be performed by a peristaltic pump; stirring can be performed by at least one of mechanical stirring and magnetic stirring.

[0054] In step (2), the first product is dried to obtain a catalyst precursor, and the precursor is then calcined and ground to obtain a catalyst.

[0055] The present invention does not limit the method of drying and roasting. For example, drying can be carried out by any of normal pressure heating method, reduced pressure heating method, and freeze drying method, and it is only necessary to remove the residual moisture in the first product; roasting can be carried out by using any of muffle furnace and tubular furnace.

[0056] The present invention does not specifically limit the temperature and time in the drying process, the heating rate in the roasting process, the roasting temperature and the heat preservation time.

[0057] The method for preparing a catalyst for preparing methanol by hydrogenating carbon dioxide of the present invention comprises the following steps: adding an organic solvent solution including an organic titanate to an aqueous solution including a copper salt, a zinc salt and a complexing agent, and controlling the concentration of each component in the reaction system and the process parameters during the reaction, so that the finally prepared catalyst has a chemical composition of Formula 1, and the content of the Cu element in the catalyst is 5-35wt%, and in an H2-TPR test, the initial reduction temperature of the catalyst is not higher than 135°C; the method can effectively reduce the risk of sintering during the roasting process, reduce the occurrence of side reactions in the reaction of preparing methanol by hydrogenating carbon dioxide, improve the methanol selectivity, and enable the catalyst to undergo a reduction reaction at a relatively low temperature, thereby improving the reduction performance and reaction activity of the catalyst, facilitating the smooth progress of the reaction of preparing methanol by hydrogenating carbon dioxide, and comprehensively improving the carbon dioxide conversion rate, methanol selectivity and methanol yield of the reaction.

[0058] In a specific embodiment, in step (1), the dripping speed is 0.05-1 mL / s. Within this range, the organic titanate can be better dispersed in the mixed solution, and the hydrolysis of the organic titanate in water can be effectively alleviated.

[0059] In a specific embodiment, in step (1), the stirring speed is 60-400 r / min. Within this range, the organic titanate, copper salt and zinc salt in the mixed solution can react with the complexing agent better without destroying the formed colloid, so that the colloid can be better formed during the stirring process.

[0060] In a specific embodiment, in step (2), the drying temperature is 105-150° C. and the drying time is 2-6 hours. Within this range, it is not only helpful to form gaps between catalyst precursor particles, thereby increasing the specific surface area of ​​the catalyst, but also to prevent the metal elements therein from being carried away by the evaporated gas, resulting in the loss of active components.

[0061] In a specific embodiment, in step (2), the heating rate during the calcination process is 1.5-2°C / min, the calcination temperature is 350-550°C, and the holding time is 3-6h. When the heating rate, calcination temperature and holding time are within the above ranges, it is more conducive to the formation of crystal defects in the catalyst and improves the catalyst performance; and it will not cause the sintering of Cu in the catalyst precursor, thereby improving the stability of the catalyst.

[0062] In a specific embodiment, the organic titanate includes at least one of tetrabutyl titanate and titanium isopropoxide; and / or the copper salt includes at least one of copper nitrate trihydrate and anhydrous copper acetate; and / or the zinc salt includes at least one of anhydrous zinc acetate and zinc nitrate; and / or the complexing agent includes at least one of chitosan, glucose, citric acid, and fructose. When the aforementioned four compounds are mixtures of multiple specific compounds, the present invention does not impose too many restrictions on the ratios between the specific compounds.

[0063] The third aspect of the present invention provides a method for preparing methanol by hydrogenating carbon dioxide, wherein the catalyst of the first aspect or the catalyst prepared by the preparation method of the catalyst for preparing methanol by hydrogenating carbon dioxide of the second aspect is used to hydrogenate carbon dioxide to obtain methanol. Since the copper content in the catalyst of the first aspect and the catalyst prepared by the preparation method of the catalyst for preparing methanol by hydrogenating carbon dioxide of the second aspect is low, and in the H2-TPR test of the catalyst, the initial reduction temperature of the catalyst is not higher than 135°C, the application of the catalyst in the reaction of hydrogenating carbon dioxide to methanol can significantly improve the CO2 conversion rate, methanol selectivity and methanol yield in the reaction.

[0064] In a specific embodiment, the method comprises the following steps:

[0065] The catalyst is placed in a reactor, a raw material mixed gas is introduced at a flow rate of 15 to 85 mL / min, and a carbon dioxide hydrogenation to methanol reaction is carried out at 230 to 310° C. and 1 to 5 MPa;

[0066] The raw material mixed gas includes hydrogen, carbon dioxide and nitrogen;

[0067] The volume ratio of hydrogen to carbon dioxide is (3-5):1, and the volume percentage of nitrogen is 4-10%. When the above catalyst is used to carry out the carbon dioxide hydrogenation to methanol reaction under the above conditions, the CO2 conversion rate, methanol selectivity and methanol yield in the reaction process can be further improved.

[0068] Specifically, the tail gas generated in the raw material mixer and the reaction process is collected during the reaction, and the raw material mixed gas, tail gas, N2, CO, CO2, and CH4 are tested by gas chromatography-mass spectrometry, and the peak area of ​​N2 in the raw material mixed gas can be obtained respectively. Peak area of ​​N2 in tail gas Peak area of ​​CO2 in raw mixed gas Peak area of ​​CO2 in tail gas Peak area of ​​CO in tail gas Peak area of ​​CH4 in tail gas Peak area of ​​pure N2 Peak area A of pure CO CO , the peak area of ​​pure CO2 Peak area of ​​pure CH4 The CO2 conversion rate in the present invention is Methanol Selectivity S MeOH , methanol yield Y MeOH It can be calculated by formula 2, formula 3, formula 4, formula 5 and formula 6 respectively.

[0069]

[0070]

[0071]

[0072]

[0073]

[0074] In formula 2, is the carbon dioxide conversion rate.

[0075] In formula 3, S CO is CO selectivity, f CO is the CO positive conversion factor, and A CO The ratio of The CO2 positive conversion factor is and ratio.

[0076] In formula 4, is CH4 selective, is the CH4 positive conversion factor, and ratio.

[0077] In formula 5, S MeOH It is selective for methanol.

[0078] In formula 6, Y MeOH is the methanol yield.

[0079] Hereinafter, the catalyst for producing methanol by hydrogenation of carbon dioxide of the present invention will be described in detail through specific examples.

[0080] Example 1

[0081] (1) 30 g of pure water was mixed with 2.64 g of Cu(NO3)2·3H2O and 8.00 g of anhydrous zinc acetate to obtain a mixed solution of copper salt and zinc salt; 15 g of pure water was mixed with 13.82 g of citric acid to obtain a complexing agent solution, and the complexing agent solution was mixed with the mixed solution of copper salt and zinc salt to obtain a first mixed solution; 7.43 g of tetrabutyl titanate was then dissolved in 15 g of anhydrous ethanol to obtain a second mixed solution; the second mixed solution was dropped into the first mixed solution at a dropping speed of 0.2 mL / s, and stirred during the dropping process at a stirring speed of 180 r / min; after the dropping was completed, the reaction system was placed in a constant temperature water bath at 60°C and stirred at a stirring speed of 180 r / min, and after reacting for 3 hours, the temperature was raised to 90°C and maintained for 1 hour to form a gel, and the stirring was stopped. At this time, the residual water content in the reaction system was 25%, and the reaction system was kept at a constant temperature for 3 hours for aging, and the first product was obtained after aging;

[0082] (2) The first product was placed in an oven at 140° C. and dried for 3 h to obtain a catalyst precursor, which was placed in a muffle furnace and heated to 450° C. at 2° C. / min for 4 h to obtain the catalyst of this embodiment, with a chemical composition of Cu 0.5 Zn2TiO 4.5 .

[0083] Example 2

[0084] (1) 20 g of pure water was mixed with 4.00 g of Cu(NO3)2·3H2O and 3.03 g of anhydrous zinc acetate to obtain a mixed solution of copper salt and zinc salt; 12 g of pure water was mixed with 9.33 g of citric acid to obtain a complexing agent solution, and the complexing agent solution was mixed with the mixed solution of copper salt and zinc salt to obtain a first mixed solution; 5.65 g of tetrabutyl titanate was then dissolved in 10 g of anhydrous ethanol to obtain a second mixed solution; the second mixed solution was dripped into the first mixed solution at a dripping speed of 0.2 mL / s, and stirred during the dripping process at a stirring speed of 180 r / min; after the dripping was completed, the reaction system was placed in a constant temperature water bath at 60°C and stirred at a stirring speed of 180 r / min, and after reacting for 3 hours, the temperature was raised to 90°C and maintained for 1 hour to form a gel, and the stirring was stopped. At this time, the residual water content in the reaction system was 25%, and the reaction system was kept at a constant temperature for 3 hours for aging, and the first product was obtained after aging;

[0085] (2) The first product was transferred into an oven at 140° C. and dried for 3 h to obtain a catalyst precursor, which was transferred into a muffle furnace and heated to 450° C. at 2° C. / min and calcined for 4 h to obtain the catalyst of this embodiment, whose chemical composition was CuZnTiO 4 .

[0086] Example 3

[0087] (1) 40 g of pure water is mixed with 0.96 g of Cu(NO3)2·3H2O and 0.72 g of anhydrous zinc acetate to obtain a mixed solution of copper salt and zinc salt; 40 g of pure water is mixed with 2.46 g of citric acid to obtain a complexing agent solution, and the complexing agent solution is mixed with the mixed solution of copper salt and zinc salt to obtain a first mixed solution; then 0.68 g of tetrabutyl titanate is dissolved in 20 g of anhydrous ethanol to obtain a second mixed solution; the second mixed solution is dropped into the first mixed solution at a dropping speed of 0.05 mL / s, and stirred during the dropping process at a stirring speed of 400 r / min; after the dropping is completed, the reaction system is placed in a constant temperature water bath at 40°C and stirred at a stirring speed of 400 r / min, and the temperature is raised to 80°C after the reaction for 4 hours, and the stirring is stopped after gelation, at which time the residual water content in the reaction system is 25%, and the reaction system is kept at a constant temperature for 4 hours for aging, and the first product is obtained after aging;

[0088] (2) The first product was transferred into an oven at 105°C and dried for 6 hours to obtain a catalyst precursor, which was then transferred into a muffle furnace and heated to 350°C at a rate of 1.5°C / min and calcined for 6 hours to obtain the catalyst of this embodiment, whose chemical composition is Cu2Zn2TiO6.

[0089] Example 4

[0090] (1) 17 g of pure water was mixed with 6.04 g of Cu(NO3)2·3H2O and 4.59 g of anhydrous zinc acetate to obtain a mixed solution of copper salt and zinc salt; 12 g of pure water was mixed with 15.37 g of citric acid to obtain a complexing agent solution, and the complexing agent solution was mixed with the mixed solution of copper salt and zinc salt to obtain a first mixed solution; 4.25 g of tetrabutyl titanate was then dissolved in 5 g of anhydrous ethanol to obtain a second mixed solution; the second mixed solution was dropped into the first mixed solution at a dropping speed of 1 mL / s, and stirred during the dropping process at a stirring speed of 60 r / min; after the dropping was completed, the reaction system was placed in a constant temperature water bath at 70°C and stirred at a stirring speed of 60 r / min, and after reacting for 1 hour, the temperature was raised to 100°C, and stirring was stopped after gelation, at which time the residual water content in the reaction system was 25%, and the reaction system was kept at a constant temperature for 1 hour for aging, and a first product was obtained after aging;

[0091] (2) The first product was moved to an oven at 150°C and dried for 2 h to obtain a catalyst precursor, which was moved to a muffle furnace and heated to 550°C at 2°C / min for calcination for 3 h to obtain the catalyst of this embodiment, with a chemical composition of CuZnTi 0.48 O 2.96 .

[0092] Example 5

[0093] (1) 30 g of pure water was mixed with 0.37 g of Cu(NO3)2·3H2O and 8.00 g of anhydrous zinc acetate to obtain a mixed solution of copper salt and zinc salt; 15 g of pure water was mixed with 12.50 g of citric acid to obtain a complexing agent solution, and the complexing agent solution was mixed with the mixed solution of copper salt and zinc salt to obtain a first mixed solution; 7.43 g of tetrabutyl titanate was then dissolved in 15 g of anhydrous ethanol to obtain a second mixed solution; the second mixed solution was dropped into the first mixed solution at a dropping speed of 0.2 mL / s, and stirred during the dropping process at a stirring speed of 180 r / min; after the dropwise addition was completed, the reaction system was placed in a constant temperature water bath at 60°C and stirred at a stirring speed of 180 r / min, and after reacting for 3 hours, the temperature was raised to 90°C and maintained for 1 hour to form a gel, and the stirring was stopped. At this time, the residual water content in the reaction system was 25%, and the reaction system was kept at a constant temperature for 3 hours for aging, and the first product was obtained after aging;

[0094] (2) The first product was placed in an oven at 140° C. and dried for 3 h to obtain a catalyst precursor, which was placed in a muffle furnace and heated to 450° C. at 2° C. / min for 4 h to obtain the catalyst of this embodiment, with a chemical composition of Cu 0.07 Zn2TiO 4.07 .

[0095] Example 6

[0096] (1) 20 g of pure water was mixed with 4.00 g of Cu(NO3)2·3H2O and 3.03 g of anhydrous zinc acetate to obtain a mixed solution of copper salt and zinc salt; 12 g of pure water was mixed with 9.33 g of citric acid to obtain a complexing agent solution, and the complexing agent solution was mixed with the mixed solution of copper salt and zinc salt to obtain a first mixed solution; 5.65 g of tetrabutyl titanate was then dissolved in 10 g of anhydrous ethanol to obtain a second mixed solution; the second mixed solution was dropped into the first mixed solution at a dropping speed of 1.5 mL / s, and stirred during the dropping process at a stirring speed of 180 r / min; after the dropping was completed, the reaction system was placed in a constant temperature water bath at 60°C and stirred at a stirring speed of 180 r / min, and after reacting for 3 hours, the temperature was raised to 90°C and maintained for 1 hour to form a gel, and the stirring was stopped. At this time, the residual water content in the reaction system was 25%, and the reaction system was kept at a constant temperature for 3 hours for aging, and the first product was obtained after aging;

[0097] (2) The first product was transferred into an oven at 140° C. and dried for 3 h to obtain a catalyst precursor, which was transferred into a muffle furnace and heated to 450° C. at 2° C. / min and calcined for 4 h to obtain the catalyst of this embodiment, whose chemical composition was CuZnTiO 4 .

[0098] Example 7

[0099] (1) 20 g of pure water was mixed with 4.00 g of Cu(NO3)2·3H2O and 3.04 g of anhydrous zinc acetate to obtain a mixed solution of copper salt and zinc salt; 12 g of pure water was mixed with 9.33 g of citric acid to obtain a complexing agent solution, and the complexing agent solution was mixed with the mixed solution of copper salt and zinc salt to obtain a first mixed solution; 5.65 g of tetrabutyl titanate was then dissolved in 10 g of anhydrous ethanol to obtain a second mixed solution; the second mixed solution was dropped into the first mixed solution at a dropping speed of 0.2 mL / s, and stirred during the dropping process at a stirring speed of 180 r / min; after the dropwise addition was completed, the reaction system was placed in a constant temperature water bath at 60°C and stirred at a stirring speed of 500 r / min, and after reacting for 3 hours, the temperature was raised to 90°C and maintained for 1 hour to form a gel, and the stirring was stopped. At this time, the residual water content in the reaction system was 25%, and the system was kept at a constant temperature for 3 hours for aging, and the first product was obtained after aging;

[0100] (2) The first product was transferred into an oven at 140° C. and dried for 3 h to obtain a catalyst precursor, which was transferred into a muffle furnace and heated to 450° C. at 2° C. / min and calcined for 4 h to obtain the catalyst of this embodiment, whose chemical composition was CuZnTiO 4 .

[0101] Example 8

[0102] (1) 20 g of pure water was mixed with 4.00 g of Cu(NO3)2·3H2O and 3.04 g of anhydrous zinc acetate to obtain a mixed solution of copper salt and zinc salt; 12 g of pure water was mixed with 9.33 g of citric acid to obtain a complexing agent solution, and the complexing agent solution was mixed with the mixed solution of copper salt and zinc salt to obtain a first mixed solution; 5.65 g of tetrabutyl titanate was then dissolved in 10 g of anhydrous ethanol to obtain a second mixed solution; the second mixed solution was dropped into the first mixed solution at a dropping speed of 0.2 mL / s, and stirred during the dropping process at a stirring speed of 180 r / min; after the dropping was completed, the reaction system was placed in a constant temperature water bath at 60°C and stirred at a stirring speed of 180 r / min, and after reacting for 3 hours, the temperature was raised to 90°C and maintained for 1 hour to form a gel, and the stirring was stopped. At this time, the residual water content in the reaction system was 25%, and the reaction system was kept at a constant temperature for 3 hours for aging, and the first product was obtained after aging;

[0103] (2) The first product was transferred into an oven at 160° C. and dried for 1 h to obtain a catalyst precursor, which was transferred into a muffle furnace and heated to 450° C. at 2° C. / min and calcined for 4 h to obtain the catalyst of this embodiment, whose chemical composition is CuZnTiO4.

[0104] Example 9

[0105] (1) 20 g of pure water was mixed with 4.00 g of Cu(NO3)2·3H2O and 3.04 g of anhydrous zinc acetate to obtain a mixed solution of copper salt and zinc salt; 12 g of pure water was mixed with 9.33 g of citric acid to obtain a complexing agent solution, and the complexing agent solution was mixed with the mixed solution of copper salt and zinc salt to obtain a first mixed solution; 5.65 g of tetrabutyl titanate was then dissolved in 10 g of anhydrous ethanol to obtain a second mixed solution; the second mixed solution was dropped into the first mixed solution at a dropping speed of 0.2 mL / s, and stirred during the dropping process at a stirring speed of 180 r / min; after the dropping was completed, the reaction system was placed in a constant temperature water bath at 60°C and stirred at a stirring speed of 180 r / min, and after reacting for 3 hours, the temperature was raised to 90°C and maintained for 1 hour to form a gel, and the stirring was stopped. At this time, the residual water content in the reaction system was 25%, and the reaction system was kept at a constant temperature for 3 hours for aging, and the first product was obtained after aging;

[0106] (2) The first product was transferred into an oven at 140° C. and dried for 3 h to obtain a catalyst precursor, which was transferred into a muffle furnace and heated to 650° C. at a rate of 1.2° C. / min and calcined for 1 h to obtain the catalyst of this embodiment, whose chemical composition is CuZnTiO4.

[0107] Comparative Example 1

[0108] The catalyst preparation method of this comparative example is basically the same as that of Example 2, except that 0.18 g of tetrabutyl titanate is dissolved in 15 g of anhydrous ethanol to prepare the second mixed solution.

[0109] The chemical composition of the catalyst prepared in this comparative example is CuZnTi 0.03 O 2.06 .

[0110] Comparative Example 2

[0111] The catalyst preparation method of this comparative example is basically the same as that of Example 2, except that the amount of Cu(NO3)2·3H2O used is 0.2 g.

[0112] The chemical composition of the catalyst prepared in this comparative example is Cu 0.05 ZnTiO 3.05 .

[0113] Comparative Example 3

[0114] The catalyst preparation method of this comparative example is basically the same as that of Example 2, except that the amount of anhydrous zinc acetate used is 0.22 g.

[0115] The chemical composition of the catalyst prepared in this comparative example is CuZn 0.06 TiO 3.06 .

[0116] Comparative Example 4

[0117] The catalyst preparation method of this comparative example is basically the same as that of Example 2, except that the amount of citric acid used is 0.39 g.

[0118] The chemical composition of the catalyst prepared in this comparative example is CuZnTiO4.

[0119] Comparative Example 5

[0120] The catalyst preparation method of this comparative example is basically the same as that of Example 2, except that the temperature of the constant temperature water bath is 30°C.

[0121] The chemical composition of the catalyst prepared in this comparative example is CuZnTiO4.

[0122] Comparative Example 6

[0123] The catalyst preparation method of this comparative example is basically the same as that of Example 2, except that the reaction is carried out in a constant temperature water bath for 30 minutes.

[0124] The chemical composition of the catalyst prepared in this comparative example is CuZnTiO4.

[0125] Comparative Example 7

[0126] The catalyst preparation method of this comparative example is basically the same as that of Example 2, except that the temperature is raised to 75° C. after reacting in a water bath for 3 hours.

[0127] The chemical composition of the catalyst prepared in this comparative example is CuZnTiO4.

[0128] Comparative Example 8

[0129] The catalyst preparation method of this comparative example is basically the same as that of Example 2, except that the aging time at 90° C. is 30 minutes.

[0130] The chemical composition of the catalyst prepared in this comparative example is CuZnTiO4.

[0131] Comparative Example 9

[0132] The preparation method of the catalyst of this comparative example is basically the same as that of Example 1, except that 30 g of pure water and 8.0 g of anhydrous zinc acetate are mixed to obtain a zinc salt aqueous solution; 15 g of pure water and 12.29 g of citric acid are mixed to obtain a complexing agent solution, and the complexing agent solution is mixed with the zinc salt aqueous solution to obtain a first mixed solution; then 7.46 g of tetrabutyl titanate is dissolved in 15 g of anhydrous ethanol to prepare a second mixed solution.

[0133] The chemical composition of the catalyst prepared in this comparative example is Zn2TiO4.

[0134] Comparative Example 10

[0135] Mix 2 g of pure water with 2.33 g of Cu(NO3)2·3H2O to obtain a copper salt aqueous solution; at room temperature, the catalyst particles prepared in Comparative Example 9 were immersed in the copper salt aqueous solution and ultrasonicated for 1 hour, then moved into a 120°C oven and dried for 2 hours, placed in a muffle furnace and heated to 450°C at a heating rate of 2°C / min and calcined for 4 hours to obtain the catalyst of this comparative example.

[0136] The chemical composition of the catalyst prepared in this comparative example is Cu 0.45 Zn2TiO 4.45 .

[0137] Test example

[0138] 1. The catalysts prepared in the above embodiments and comparative examples were subjected to H2-TPR test and CO2-TPD test, comprising the following steps:

[0139] (1) H2-TPR test

[0140] The catalysts prepared in the above embodiments and comparative examples were ground and crushed, and 20-40 mesh catalysts were screened for testing; the 20-40 mesh catalysts were loaded into a quartz fixed bed reactor, first purged with Ar, and the catalyst was dehydrated by heating to 350°C. After cooling to room temperature, a mixed gas containing 10% H2 and 90% Ar was introduced. While the mixed gas was introduced, the temperature was raised to 400°C at 15°C / min. During this process, a mass spectrometer was used to detect the fragment molecules of H2O and H2, and the response was observed. The test results are shown in Tables 1 and Figure 1 .

[0141] Figure 1 The H2-TPR test diagram of the catalyst prepared in Example 2 and Comparative Example 10 is shown in FIG. Figure 1 It can be seen from the H2O signal curves of the two catalysts in the analysis figure that as the temperature rises, the copper oxide in the catalyst is reduced by hydrogen and generates water. The temperature corresponding to the beginning of water generation in the figure represents the starting reduction temperature. At this time, the CuO in the catalyst begins to be reduced. Figure 1 It can be seen that the starting reduction temperatures of Example 2 and Comparative Example 10 are not the same, wherein the starting reduction temperature of Example 2 is 112.4°C, and the starting reduction temperature of Comparative Example 10 is 167.8°C, indicating that the reducing ability of the catalyst in Example 2 is stronger than that in Comparative Example 10, and has better reducing performance, and can better reduce CO2 into methanol.

[0142] (2) CO2-TPD test

[0143] The catalysts prepared in the above examples and comparative examples were ground and crushed, and catalysts with a size of 20 to 40 mesh were screened for testing; the catalysts with a size of 20 to 40 mesh were loaded into a quartz fixed bed reactor, CO2 was first adsorbed for 30 min at room temperature, and then Ar was introduced for purging for 30 min, and the temperature was raised to 350°C at 20°C / min under Ar. During this process, a mass spectrometer was used to detect CO2 fragment molecules and observe the peaks. The test results are shown in Tables 1 and Figure 2 .

[0144] Figure 2 The CO2-TPD test diagram of the catalyst prepared in Example 2 and Comparative Example 10 is shown in FIG. Figure 2 It can be seen that the catalyst in Comparative Example 10 has a short peak near 180°C, indicating that the catalyst in Comparative Example 10 has fewer medium alkaline sites and a weak CO2 adsorption capacity; while the catalyst in Example 2 has peaks at <100°C, 160°C and 280°C, among which the peak at <100°C represents physically adsorbed CO2, which can represent a weak alkaline site, and the peak near 160°C can represent a medium alkaline site, and the medium alkaline site of Example 2 is much higher than that of Comparative Example 10, indicating that Example 2 has good adsorption and desorption capabilities for CO2 within the reaction temperature range and is more suitable for catalyzing CO2 hydrogenation to produce methanol.

[0145] 2. The conversion rate, methanol selectivity and methanol yield of the catalysts in the above examples and comparative examples were tested. The specific steps are as follows:

[0146] Weigh 0.5 g of 20-40 mesh catalyst particles and load them into a stainless steel tube fixed bed reactor, then introduce raw gas (H2: 72%, CO2: 24%, N2: 4%), maintain the reaction pressure at 3 MPa, adjust the gas flow rate to 30 mL / min, then heat to 250°C at 15°C / min for continuous reaction for 5 h, collect the water and methanol produced by the product through a condenser, and analyze the remaining reaction tail gas through a gas chromatograph. The gas chromatograph collects the product tail gas every ten minutes, and ends after 3 hours to obtain the product tail gas at different time points. Calculate according to formula 2-6, and finally get the CO2 conversion rate at each time point Methanol Selectivity S MeOH And methanol yield Y MeOH The average value is taken as the catalyst evaluation result. The test results are shown in Table 1.

[0147] Table 1

[0148]

[0149]

[0150] From Table 1, we can see that:

[0151] The catalysts in Examples 1 to 9 have higher comprehensive performance in the production of methanol from carbon dioxide hydrogenation. Specifically, in the reaction of producing methanol from carbon dioxide hydrogenation, the catalyst in Example 2 has a carbon dioxide conversion rate of 14.4%, a methanol selectivity of 72.1%, and a methanol yield of 10.4%; while the catalyst in Comparative Example 1 has a carbon dioxide conversion rate of 14.5%, a methanol selectivity of only 34.2%, and a methanol yield of 5.0%; it can be seen that the catalyst of the present invention can significantly improve the CO2 conversion rate, methanol selectivity and methanol yield.

[0152] 3. The catalyst prepared in Example 1 was subjected to a stability test, comprising the following steps:

[0153] 0.5 g of 20-40 mesh catalyst particles were added to a stainless steel fixed bed reactor, and then a raw mixed gas (H2: 72%, CO2: 24%, N2: 4%) was introduced (flow rate was 30 mL / min), the pressure was adjusted to 3 MPa through a back pressure valve, and the temperature was increased to 250°C, 280°C, and 310°C at a heating rate of 15°C / min, respectively. The reaction was carried out under this condition, and the tail gas generated during the reaction was introduced into a gas chromatograph with an injection interval of 10 min. After the reaction was stable for 1 h, data points were recorded, and the average of the six data points generated each hour was taken as the catalyst evaluation result within this hour. The CO2 conversion rate, methanol selectivity, and methanol yield at different temperatures were calculated by Formulas 2 to 6, and the experiment was stopped after 10 h.

[0154] The test results are as follows Figure 3 As shown by Figure 3 It can be seen that during the 10 h continuous reaction, the performance of the catalyst did not show a significant decline, indicating that it has good stability.

[0155] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A catalyst for preparing methanol by hydrogenating carbon dioxide, characterized in that: It has the chemical composition of formula 1, and the content of Cu element is 3-40wt%, Cu a Zn b TiO x Formula 1 In formula 1, 0<a≤2.1, 0<b≤2.1, x=2+a+b; In the H2-TPR test of the catalyst, the initial reduction temperature of the catalyst is not higher than 135°C.

2. A method for preparing the catalyst for hydrogenating carbon dioxide to methanol according to claim 1, characterized in that: The following steps are involved: (1) adding an organic solvent solution including an organic titanate dropwise to an aqueous solution including a copper salt, a zinc salt, and a complexing agent to obtain a mixed solution, heating the mixed solution to 40 to 70° C. and stirring, reacting for 1 to 4 hours, then heating the mixed solution to 80 to 100° C. until the residual water content is less than 30%, stopping stirring, and maintaining the temperature for 1 to 4 hours for aging to obtain a first product; In the mixed solution, the molar concentration of the organic titanate is 0.015-0.4 mol / L, the molar concentration of the copper salt is 0.02-0.4 mol / L, the molar concentration of the zinc salt is 0.03-0.75 mol / L, and the molar concentration of the complexing agent is 0.1-2.5 mol / L; (2) Drying the first product to obtain a catalyst precursor, and calcining the catalyst precursor to obtain the catalyst.

3. The method for preparing a catalyst for preparing methanol by hydrogenation of carbon dioxide according to claim 2, characterized in that: In step (1), the dropping speed is 0.05 to 1 mL / s.

4. The catalyst for preparing methanol by hydrogenation of carbon dioxide according to claim 2 or 3, characterized in that: In step (1), the stirring speed is 60 to 400 r / min.

5. The method for preparing the catalyst for preparing methanol by hydrogenation of carbon dioxide according to any one of claims 2 to 4, characterized in that: In step (2), the drying temperature is 105-150° C. and the drying time is 2-6 hours.

6. The method for preparing a catalyst for preparing methanol by hydrogenation of carbon dioxide according to any one of claims 2 to 5, characterized in that: In step (2), the heating rate during the roasting process is 1.5-2°C / min, the roasting temperature is 350-550°C, and the holding time is 3-6h.

7. The method for preparing a catalyst for preparing methanol by hydrogenation of carbon dioxide according to any one of claims 2 to 6, characterized in that: The organic titanate includes at least one of tetrabutyl titanate and titanium isopropoxide; And / or, the copper salt includes at least one of copper nitrate trihydrate and anhydrous copper acetate; And / or, the zinc salt includes at least one of anhydrous zinc acetate and zinc nitrate; And / or, the complexing agent includes at least one of chitosan, glucose, citric acid and fructose.

8. A method for preparing methanol by hydrogenating carbon dioxide, characterized in that: Methanol is obtained by hydrogenating carbon dioxide using the catalyst described in claim 1 or the catalyst prepared by the method for preparing the catalyst for hydrogenating carbon dioxide to methanol described in any one of claims 2 to 7.

9. The method for preparing methanol by hydrogenating carbon dioxide according to claim 8, characterized in that: The following steps are involved: The catalyst is placed in a reactor, a raw material mixed gas is introduced at a flow rate of 15 to 85 mL / min, and a carbon dioxide hydrogenation to methanol reaction is carried out at 230 to 310° C. and 1 to 5 MPa; The raw mixed gas includes hydrogen, carbon dioxide and nitrogen; The volume ratio of the hydrogen to the carbon dioxide is (3-5):1, and the volume percentage of the nitrogen is 4-10%.

Citation Information

Patent Citations

  • Catalyst used for CO hydrogenation to prepare isobutanol, and method for preparing isobutanol through CO hydrogenation

    CN105080545A

  • Catalyst for synthesizing methanol through hydrogenation of carbon dioxide and preparation method of catalyst

    CN109999833A

  • Catalyst for synthesizing methanol through carbon dioxide hydrogenation, preparation method and application

    CN112755996A

  • Catalyst for synthesizing methanol from carbon dioxide as well as preparation method and application of catalyst

    CN113842914A

  • Catalyst for preparing methanol through hydrogenation of carbon dioxide and preparation method thereof

    CN114029063A