Preparation method of sulfur indium magnesium material with photoinduced cathode protection performance
The preparation of indium sulfur magnesium material through hydrothermal method solves the problem of stainless steel corrosion in the marine environment, achieves efficient cathode protection effect, improves the stability and durability of the material, and is suitable for anti-corrosion applications in the marine environment.
Patent Information
- Application Number
- CN202411053868.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-02
- Publication Date
- 2024-11-19
AI Technical Summary
The existing technology is difficult to effectively solve the corrosion problem of stainless steel in the marine environment. Traditional anti-corrosion methods are not effective in the marine environment. The preparation process of indium sulfur magnesium materials is complicated and the stability and durability are insufficient.
The indium sulfide magnesium material was prepared by hydrothermal method, and the synthesis conditions were accurately controlled. The V-shaped shape of MgCl2·6H2O, InCl3·4H2O and thiourea were placed in FTO conductive glass for hydrothermal reaction, and MgIn2S4 material was obtained, showing significant cathodic protection Effect.
It realizes the efficient synthesis of indium sulfur magnesium materials and good metal corrosion resistance, significantly improves the cathodic protection performance during photocatalysis, and is suitable for the corrosion protection of stainless steel in marine environments.
Smart Images

Figure CN118976515A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of photocatalytic materials, and in particular relates to a method for preparing a magnesium indium sulfide material with photoinduced cathode protection performance. Background Art
[0002] Corrosion is a common problem faced by the whole world. According to the survey, the global average corrosion loss value accounts for 3.4% of the global gross national product (GNP). According to the statistics of the team of Academician Hou Baorong, the corrosion cost of my country in 2014 was about 212.78 billion yuan, accounting for about 3.34% of the GDP of that year. The marine environment is complex and harsh, with high salt content, Cl - The electrochemical corrosion of steel structures in the marine environment is particularly serious due to high concentration, rich oxygen and the presence of a large number of microorganisms, coupled with the impact of waves and strong sunlight stimulation. Marine corrosion problems seriously affect marine development and construction projects, causing significant property losses. Marine disasters caused by marine metal corrosion failure are countless, not only causing huge economic losses, but also causing great harm to life ecology. Stainless steel, as an excellent engineering material, is widely used in various fields such as industry and agriculture. It is also widely used in marine engineering and shipbuilding industries. Offshore drilling platforms, offshore oil and gas fields, and seabed mining devices in marine engineering all involve stainless steel materials. However, the corrosion resistance of stainless steel in the marine environment is much worse than that in the ordinary atmospheric environment, because in the marine environment, Cl- can preferentially and selectively adsorb on the passivation film on the surface of stainless steel to destroy the passivation film and form pitting. These pitting pits become active centers to accelerate the corrosion of stainless steel. Traditional steel structure anti-corrosion methods have been unable to meet the development of marine industry. Studies have found that the new anti-corrosion technology, photocathodic protection, has attracted widespread attention due to its strong operability, cleanliness, resource conservation and no power consumption.
[0003] Photocathodic protection technology utilizes the photoelectric effect of semiconductor materials. Through light excitation, electrons are transferred to the metal surface to achieve the effect of slowing down metal corrosion. It has attracted much attention for its environmental friendliness and high efficiency. Magnesium indium sulfide (MgIn2S4), as a new type of semiconductor material, has a special electronic structure and excellent light absorption ability, which makes it show application potential in this technology. However, the preparation process of magnesium indium sulfide is relatively complicated, and the relationship between its photoelectric properties and anti-corrosion performance has not been fully studied. In addition, the stability and durability of magnesium indium sulfide are also key challenges in its preparation. Therefore, studying an effective preparation scheme for magnesium indium sulfide is crucial to promoting the development of this technology. Summary of the invention
[0004] In order to solve the above technical problems, the present invention proposes a method for preparing a magnesium indium sulfide material with photoinduced cathodic protection performance. The magnesium indium sulfide material is prepared by a hydrothermal method. By precisely controlling the synthesis conditions, the efficient synthesis of the magnesium indium sulfide material is achieved. The material exhibits significant cathodic protection effect during the photocatalytic process.
[0005] In order to achieve the above object, the present invention is achieved through the following technical solutions:
[0006] A method for preparing an indium magnesium sulfide material having photoinduced cathodic protection performance comprises the following steps:
[0007] S1: MgCl2·6H2O, InCl3·4H2O and thiourea are mixed and dissolved in deionized water to form a precursor solution;
[0008] S2: Place FTO conductive glass in a V shape in the precursor solution with the conductive surface facing downward, and then perform a hydrothermal reaction;
[0009] S3: Take out the FTO conductive glass after the reaction, wash and dry it to obtain MgIn2S4 material.
[0010] Preferably, the molar ratio of MgCl2·6H2O, InCl3·4H2O and thiourea in the precursor solution in S1 is 1:2:2-4.
[0011] Preferably, the temperature of the hydrothermal reaction in S2 is 160° C. to 200° C., and the reaction time is 6 h to 18 h.
[0012] Preferably, in S3, the FTO conductive glass is washed three times with deionized water and anhydrous ethanol, and then dried at 60° C. under vacuum conditions to obtain the MgIn2S4 material.
[0013] The beneficial effects of the present invention are:
[0014] The indium magnesium sulfur material was prepared by a hydrothermal method, and the efficient synthesis of the indium magnesium sulfur material was achieved by precisely controlling the synthesis conditions. The material exhibited significant cathodic protection effects during the photocatalytic process and had good metal anti-corrosion effects. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings required for describing the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without paying creative work.
[0016] Figure 1This is the polarization potential-time curve of MgIn2S4 in 0.1M Na2SO4 solution under dark state and light-irradiation cyclic light-cutting conditions.
[0017] Figure 2 This is the polarization potential-current density curve of MgIn2S4 in 0.1M Na2SO4 solution under dark state and light-irradiation cyclic light-cutting conditions.
[0018] Figure 3 This is a polarization current density-time curve of MgIn2S4 in 0.1M Na2SO4 solution under dark state and light-irradiation cyclic light-cutting conditions.
[0019] Figure 4 This is the dark state electrochemical impedance spectroscopy (EIS) curve of MgIn2S4 in 0.1M Na2SO4 solution.
[0020] Figure 5 This is the dark state Mott-Schottky (MS) curve of MgIn2S4 in 0.1M Na2SO4 solution.
[0021] Figure 6 This is a graph showing the degree of matching between the corresponding peak positions of MgIn2S4 and the standard card.
[0022] Figure 7 The bandgap width diagram was inferred from the UV-visible diffuse reflectance of the prepared MgIn2S4 material for testing.
[0023] Figure 8 This is the polarization potential-time curve of the photocathodic protection of white copper B10 by MgIn2S4 in 3.5ωt% NaCl solution under dark state and light cyclic cutting conditions.
[0024] Fig. 9 This is the polarization current density-time curve of the photocathodic protection of white copper B10 by MgIn2S4 in 3.5ωt% NaCl solution under dark state and light cyclic cutting conditions.
[0025] Fig.10 This is the polarization potential-time curve of the photocathodic protection of carbon steel Q235 by MgIn2S4 in 3.5ωt% NaCl solution under dark state and light cyclic cutting conditions.
[0026] Fig.11 This is the polarization current density-time curve of the photocathodic protection of carbon steel Q235 by MgIn2S4 in 3.5ωt% NaCl solution under dark state and light cyclic cutting conditions.
[0027] Fig.12This is the polarization potential-time curve of the photocathodic protection of 316LSS by MgIn2S4 in 3.5ωt% NaCl solution under dark state and light-cycle cutting conditions.
[0028] Fig.13 This is the polarization current density-time curve of the photocathodic protection of 316LSS by MgIn2S4 in 3.5ωt% NaCl solution under dark state and light cyclic cutting conditions.
[0029] Fig.14 This is the polarization potential-time curve of MgIn2S4 in 3.5ωt% NaCl solution for photocathodic protection of 304SS under dark state and light-cycle cutting conditions.
[0030] Fig.15 This is the polarization current density-time curve of MgIn2S4 photocathodic protection performance test on 304SS in 3.5ωt% NaCl solution under dark state and light cycle cutting conditions. DETAILED DESCRIPTION
[0031] The technical solutions in the embodiments of the present invention will be described clearly and completely below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments.
[0032] Example 1
[0033] A method for preparing an indium magnesium sulfide material having photoinduced cathodic protection performance comprises the following steps:
[0034] S1: preparing a precursor solution, comprising mixing and dissolving 1.5 mmol MgCl2·6H2O, 3 mmol InCl3·4H2O and 3 mmol thiourea in 50 mL of deionized water;
[0035] S2: Put two clean FTO conductive glasses (size 2*1cm 2 ) was placed in a 50 mL polytetrafluoroethylene-lined stainless steel autoclave with the conductive surface facing downward in a V shape, and the autoclave containing the FTO conductive glass was placed in a drying oven for hydrothermal reaction at 180 ° C for 12 hours;
[0036] S3: The FTO conductive glass after the reaction was taken out, washed with deionized water and anhydrous ethanol for 3 times, and then dried under vacuum at 60° C. for 30 minutes to obtain MgIn2S4 material.
[0037] Example 2
[0038] The photoelectric performance test of MgIn2S4 material, the specific steps are as follows:
[0039] (1) Test environment of the photoelectric performance of magnesium indium sulfide under light-induced and dark conditions: Use an electrochemical cell device made of polytetrafluoroethylene to test the polarization curves under light and dark conditions related to the photoelectric performance in a three-electrode system. In this experiment, magnesium indium sulfide material is used as the photoelectrode, Ag / AgCl reference electrode and Pt sheet electrode are used as the working electrode, reference electrode and counter electrode to form a three-electrode system, and 0.1M Na2SO4 solution is used as the electrolyte solution environment. The photoinduced test experiment uses a xenon lamp with an intensity of AM 1.5G as the light source to simulate sunlight for the experiment. The solution environment and light intensity can be changed in a targeted manner according to the different systems and contents being studied.
[0040] (2) Dark state and light-induced OCP test:
[0041] First, the dark OCP was tested in the above experimental environment (time: 400s) to keep the magnesium indium sulfide electrode in a stable and activated state. Then the light-induced OCP was tested (time: 400s). During the light-induced test, the dark state and light state were switched every 50s to obtain Figure 1 Photoinduced OCP diagram shown.
[0042] (3) Photoinduced polarization curve test: In the above test environment, an electrochemical workstation is used to test the polarization potential-current density iV curve of the working electrode under light (such as Figure 2 As shown) and polarization current density-time it curve (as shown Figure 3 In order to reduce the influence of polarization on the physicochemical properties of the electrode surface, the test potential range was ±200 mV of the photoinduced OCP value of the indium magnesium sulfate electrode, and the scanning speed was 1.66 mV / s.
[0043] (4) Dark state EIS and MS curve test: same as the above test environment (0.1MNa2SO4).
[0044] (5) Results: Figures 1 to 5 As shown in the figure, the test results show that the MgIn2S4 material prepared in this experiment has good photoelectric properties. Its photoinduced potential shift under light is -0.272V, and the photocurrent reaches 6mA at 1V bias and 1.8mA at 0V bias. In addition, the EIS and MS test results also indirectly explain the basic principle of the photoelectric properties of the MgIn2S4 material.
[0045] Example 3
[0046] Photocathodic protection performance test, the specific steps are as follows:
[0047] (1) Test environment for the photocathodic protection performance of magnesium indium sulfide under light-induced and dark conditions: Using an electrochemical cell device made of polytetrafluoroethylene, the polarization curves under light and dark conditions related to the photoelectric performance were tested in a three-electrode system. In this experiment, magnesium indium sulfide material was used as the photoelectrode, Ag / AgCl reference electrode and metal materials of different materials (nickel silver B10, carbon steel Q235, 316LSS, 304SS) were used as the working electrode, reference electrode and counter electrode to form a three-electrode system, and 3.5ωt% NaCl solution was used as the electrolyte solution environment. The photo-induced test experiment used a xenon lamp intensity AM 1.5G as the light source to simulate sunlight for the experiment. The solution environment and light intensity can be changed in a targeted manner according to the different systems and contents being studied.
[0048] (2) Photoinduced and dark-state OCP test of indium magnesium sulfate electrode: The purpose of testing dark-state OCP in this experiment is to make the indium magnesium sulfate electrode in a stable and activated state in the electrolyte environment of 3.5ωt% NaCl solution, and also to provide a good environment for the electrode when testing photoinduced OCP later. First, use a wire to connect the working electrode (indium magnesium sulfate electrode) and the counter electrode (different metals such as nickel silver B10, carbon steel Q235, 316LSS, 304SS), clamp the counter electrode with the working electrode clamp, and clamp the Ag / AgCl reference electrode with the reference electrode clamp. The above experimental connection method needs to test the OCP in the dark and light conditions respectively. The specific operation is to test the OCP values of the working electrode in the dark and light conditions respectively through the electrochemical workstation.
[0049] (3) Photoinduced polarization curve test: In the above test environment, the connection method is changed so that the working electrode clamp clamps the working electrode (indium magnesium sulfide electrode), and the auxiliary electrode clamp and the counter electrode clamp clamp the counter electrode (different metals such as nickel silver B10, carbon steel Q235, 316LSS, 304SS). The above experimental connection method is used to test the it curve of the working electrode under light in the electrochemical workstation. In order to reduce the influence of polarization on the physical and chemical properties of the electrode surface, the test potential range is ±200mV of the dark state OCP value of the semiconductor electrode, and the scanning speed is 1.66mV / s.
[0050] (4) Result description. According to the performance test of the photocathodic protection of different metals (nickel silver B10, carbon steel Q235, 316LSS, 304SS), the photoinduced OCP and photoinduced IT diagram (see Appendix) were read. Figures 8 to 15 ), which correspond to the photocathodic protection of four metals, namely, nickel silver B10, carbon steel Q235, 316LSS and 304SS. It can be seen intuitively that the magnesium indium sulfide material prepared by the present invention can protect all metal materials, among which the protection performance for nickel silver B10, 316LSS and 304SS is the best, and it can also protect carbon steel Q235, but the protection performance is weaker.
[0051] In summary, a series of photoelectric performance tests were conducted on the MgIn2S4 material, including photocurrent density measurement, electrochemical impedance spectroscopy analysis, open circuit potential monitoring, etc., as well as evaluation of the photocathodic protection efficiency of different metal materials. These tests not only verified the photoelectric conversion efficiency of the material, but also revealed its anti-corrosion potential in practical applications.
[0052] In addition, the present invention also utilizes X-ray diffraction (XRD) (Appendix Figure 6 ) technology accurately analyzes the crystal structure of the material to ensure the crystallinity and phase purity of the material. Figure 7 ) technology further revealed the material's absorption characteristics of light, providing important information for understanding its photocatalytic mechanism. Through these in-depth material characterizations, not only the high-quality synthesis of indium magnesium sulfide materials is ensured, but also a solid scientific foundation is provided for the application of materials in the field of photoinduced cathodic protection.
[0053] The preferred embodiments of the present invention disclosed above are only used to help illustrate the present invention. The preferred embodiments do not describe all details in detail, nor do they limit the invention to only the specific embodiments described. Obviously, many modifications and changes can be made according to the content of this specification.
Claims
1. A method for preparing an indium magnesium sulfide material having photoinduced cathodic protection performance, characterized in that: The following steps are involved: S1: MgCl2·6H2O, InCl3·4H2O and thiourea are mixed and dissolved in deionized water to form a precursor solution; S2: Place FTO conductive glass in a V shape in the precursor solution with the conductive surface facing downward, and then perform a hydrothermal reaction; S3: Take out the FTO conductive glass after the reaction, wash and dry it to obtain MgIn2S4 material.
2. The method for preparing magnesium indium sulfide material with photoinduced cathodic protection performance according to claim 1, characterized in that: The molar ratio of MgCl2·6H2O, InCl3·4H2O and thiourea in the precursor solution in S1 is 1:2:2-4.
3. The method for preparing the magnesium indium sulfide material with photoinduced cathodic protection performance according to claim 1, characterized in that: The temperature of the hydrothermal reaction in S2 is 160° C. to 200° C., and the reaction time is 6 h to 18 h.
4. The method for preparing the magnesium indium sulfide material with photoinduced cathodic protection performance according to claim 1, characterized in that: In the S3, the FTO conductive glass is washed three times with deionized water and anhydrous ethanol, and then dried under vacuum conditions at 60° C. to obtain the MgIn2S4 material.
5. Use of the magnesium indium sulfide material prepared according to any one of claims 1 to 4 in metal corrosion protection.
Citation Information
Patent Citations
Preparation method for modified electrode material-silver indium sulfide
CN108845006A
Ultrathin MgIn2S4 nanosheet sterilization photocatalytic material and preparation method thereof
CN113751027A
Porous composite photoelectric energy storage material for photoinduced continuous cathodic protection as well as preparation and application of porous composite photoelectric energy storage material
CN114134506A
MnIn2S4 / TiO2 nanotube bundle composite photo-anode material and preparation method and application thereof
CN114277375A
Photonic use of intermediate band materials on a chalcogenide-type semiconductor
US20100206351A1
Cited By
Method for synthesizing regular flower-ball-shaped nanometer sulfur indium magnesium by one-pot method
CN120309003A