Ni2P / 1T-WS2 / ZnIn2S4 composite catalyst as well as preparation method and application thereof

Through the ultrasonic composite technology of Ni2P/1T-WS2/ZnIn2S4 composite catalyst, the problem of insufficient photocatalytic performance of pure ZnIn2S4 is solved. By forming a Motshotky interface and providing a multi-charge transfer channel, the photocatalytic preparation efficiency of H2O2 is significantly improved. and performance.

CN118976519AActive Publication Date: 2024-11-19HENAN NORMAL UNIV
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411087345.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-09
Publication Date
2024-11-19
Estimated Expiration
2044-08-09

Smart Images

  • Figure CN118976519A_ABST
    Figure CN118976519A_ABST
Patent Text Reader

Abstract

The invention discloses preparation of a Ni2P / 1T-WS2 / ZnIn2S4 composite catalyst and application of the Ni2P / 1T-WS2 / ZnIn2S4 composite catalyst in photocatalytic preparation of H2O2, and belongs to the field of catalytic materials. Ni2P, 1T-WS2 and ZnIn2S4 are prepared by adopting a hydrothermal method, then 1T-WS2 / ZnIn2S4 is prepared by adopting an ultrasonic compounding method, then Ni2P nanoparticles and the 1T-WS2 / ZnIn2S4 are compounded to prepare the ternary double-promoter Ni2P / 1T-WS2 / ZnIn2S4, and the mass ratio of the ZnIn2S4 to the 1T-WS2 to the Ni2P is 1: (0.01-0.2): (0.001-0.1). The ZnIn2S4 and the 1T-WS2 with the metal property form a Mott Schottky junction interface, electrons transmitted from the 1T-WS2 can be effectively captured through introduction of a Ni2P cocatalyst, and Ni2P can provide a large number of active sites in the photocatalytic reaction process. The Ni2P / 1T-WS2 / ZnIn2S4 as a photocatalyst shows excellent performance of photocatalytic preparation of H2O2 under mild reaction conditions.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of inorganic materials, and specifically relates to a Ni2P / 1T-WS2 / ZnIn2S4 composite catalyst, a preparation method thereof, and an application thereof in photocatalytic preparation of H2O2. Background Art

[0002] As a clean and mild oxidant, hydrogen peroxide (H2O2) has many advantages, such as the highest active oxygen content, excellent efficacy in a wide pH range, and non-toxic byproducts produced in the reaction (only water / O2 is produced). Currently, H2O2 has been widely used in various industrial fields such as bleaching, mining and metal processing, detergent applications, wastewater treatment, and chemical organic synthesis. More importantly, H2O2 has perfect solubility in water, providing an easier and safer way for storage and transportation. In industry, H2O2 is produced on a large scale through the energy-intensive anthraquinone method.

[0003] Different from the traditional anthraquinone method, photocatalytic preparation of H2O2 is a potential solar-driven production technology, which has attracted widespread attention due to its advantages such as low energy consumption, green and environmental protection. The core of photocatalytic preparation of H2O2 technology is the catalyst. Among them, ZnIn2S4, as a typical semiconductor photocatalytic material, is regarded as one of the most promising materials for photocatalytic preparation of H2O2 due to its suitable conduction band and valence band positions, easy preparation, low toxicity and excellent photoelectric properties. However, the light response range of pure ZnIn2S4 in practical applications is limited to the ultraviolet light region, and its rapid recombination of photogenerated electrons and holes and photocorrosion seriously affect its photocatalytic performance. In order to improve the photocatalytic performance of ZnIn2S4, a variety of strategies have been explored to modify it, including morphology regulation, construction of heterojunctions, metal or non-metallic element doping, and co-catalyst loading.

[0004] Among the many modification strategies, co-catalyst loading can not only improve the separation efficiency of photogenerated electrons and holes, but also provide more reactive sites for photoreaction, thus improving the photoactivity of the catalyst. At present, most of the research on co-catalyst loading focuses on the development of a single co-catalyst. Although the photocatalytic performance has been improved to a certain extent, its activity is still far from satisfactory. Summary of the invention

[0005] In order to overcome the above technical defects, the present invention provides a dual promoter Ni2P / 1T-WS2 / ZnIn2S4 that is simple to operate and easy to implement. The present invention uses ZnIn2S4 nanosheets as the main catalyst, and through a simple ultrasonic composite strategy, successfully composites the metal phase 1T-WS2 nanospheres and Ni2P nanoparticles with ZnIn2S4 nanosheets to prepare a dual promoter photocatalytic system and applies it to the photocatalytic preparation of H2O2. In the present invention, the Mott Schottky interface formed by the metal phase 1T-WS2 and ZnIn2S4 can effectively accelerate the transfer and separation of charges; and the introduction of the promoter Ni2P can effectively capture the electrons transferred from 1T-WS2, provide multiple charge transfer channels, and further improve the charge separation performance; on the other hand, it can also provide a large number of active sites for the photoreduction reaction, thereby effectively improving the H2O2 precipitation kinetics. Based on the above advantages, the Ni2P / 1T-WS2 / ZnIn2S4 dual promoter system prepared in the present invention has shown good application in the photocatalytic preparation of H2O2.

[0006] The Ni2P / 1T-WS2 / ZnIn2S4 composite catalyst of the present invention has the following structural characteristics: the mass ratio of ZnIn2S4, 1T-WS2 and Ni2P in the catalyst is 1:0.01-0.2:0.001-0.1; ZnIn2S4 is a nano-sheet structure, 1T-WS2 is a nano-flower ball structure, and Ni2P is a nano-particle structure; the XRD spectrum has the following peaks at 21.58°, 27.69°, 30.45°, 39.77°, 52.47° and 55.58° There are strong diffraction peaks; in XPS, there are binding energies at 161.45eV, 162.65eV, 444.94eV, 452.49eV, 1021.26eV, 1044.38eV, 31.88eV, 33.14eV, 33.91eV, 35.34eV, 37.60eV, 129.55eV, 130.25eV, 853.19eV, 872.64eV, 856.61eV, 877.07eV and 862.37eV;

[0007] from Figure 1It can be clearly observed in the XRD crystal structure of the catalyst that the ZnIn2S4 sample has six strong diffraction peaks at 21.58°, 27.69°, 30.45°, 39.77°, 52.47° and 55.58°, which are consistent with the standard XRD spectrum of the hexagonal ZnIn2S4 phase (JCPDSNo.89-3963). In the 1T-WS2 spectrum, three diffraction peaks appear at 9.3°, 18.3° and 31.9°, which belong to the (002), (004) and (006) crystal planes of 1T-WS2 respectively. The XRD peak shape of pure Ni2P is consistent with the standard XRD spectrum of hexagonal Ni2P (PDF#03-0953), indicating that the prepared Ni2P has a high purity and does not contain other impurities. The peak of WS2 at 9.3° of the three-component Ni2P / 1T-WS2 / ZnIn2S4 composite sample disappeared, which may be due to the influence of Ni2P or the high dispersion of the sample. Compared with the peak of 2H-WS2 at 14.32°(002), the new peak of 1T-WS2(002) moved to 9.3°, proving that the metallic phase 1T-WS2 was prepared.

[0008] from Figure 2 Ni2P / 1T-WS2 / ZnIn2S4XPS shows: S2p 3 / 2 and S2p 1 / 2 The binding energy is between 161.45eV and 162.65eV; In 3d 5 / 2 and In 3d 3 / 2 The binding energies are 444.94eV and 452.49eV; Zn 2p 3 / 2 and Zn 2p 1 / 2 The binding energies are 1021.26eV and 1044.38eV; 4f 7 / 2 -1T and 4f 5 / 2 -1T binding energy is 31.88eV and 33.14eV, 4f 7 / 2 -2H and 4f 5 / 2 -2H binding energy is 33.91eV and 35.34eV, W 6+ The corresponding binding energy is 37.60 eV; P 2p 3 / 2 and P 2p 1 / 2 The binding energies are 129.55eV and 130.25eV, and the characteristic peak at 133.45eV corresponds to the PO bond; Ni 2p 3 / 2 and Ni 2p 1 / 2 The binding energies are 853.19eV and 872.64eV, and the characteristic peak at 862.37eV is a satellite peak. The spectrum shows that five elements, S, In, Zn, W, Ni, and P, exist simultaneously, and no peaks of other impurities are detected, indicating that a high-purity ternary system complex has been successfully prepared.

[0009] from Figure 3 From the SEM sample morphology, it can be seen that the ZnIn2S4 sample exhibits a three-dimensional interlaced ultra-thin nanosheet structure, the 1T-WS2 sample is a nanoflower ball with a diameter of about 5μm, and the Ni2P sample presents irregular coral-like nanoparticle accumulation.

[0010] from Figure 4 TEM and HRTEM clearly show that several different lattice fringes are interlaced, among which the lattice spacing of ZnIn2S4 is 0.321nm and 0.423nm, corresponding to the (001) and (006) crystal planes respectively. 1T-WS2 has a wider lattice spacing of 0.932nm, corresponding to its (002) crystal plane. Ni2P lattice fringes can also be clearly observed, with a lattice spacing of 0.221nm corresponding to its (111) crystal plane. TEM and HRTEM images show that ZnIn2S4, 1T-WS2 and Ni2P are successfully composited together.

[0011] from Figure 5 From the PL study on the charge separation and transfer effects of the samples, it can be seen that the PL spectrum peak intensity of the two-component composite materials 1T-WS2 / ZnIn2S4, Ni2P / ZnIn2S4 and the three-component composite material Ni2P / 1T-WS2 / ZnIn2S4 is significantly weaker than that of pure ZnIn2S4, among which the PL spectrum intensity of the three-component composite material Ni2P / 1T-WS2 / ZnIn2S4 is the weakest. This shows that the co-catalysts 1T-WS2 and Ni2P can quickly transfer photogenerated electrons when combined with ZnIn2S4 respectively, but after Ni2P is compounded with 1T-WS2 / ZnIn2S4, the synergistic effect of the co-catalysts 1T-WS2 and Ni2P further enhances the transfer ability of photogenerated electrons.

[0012] from Figure 6 It can be seen from the transient current spectrum that ZnIn2S4 exhibits a lower current density, indicating that only a small number of photogenerated electrons are involved in the transfer and separation process; compared with ZnIn2S4, the transient photocurrent intensity of the two-component composite samples 1T-WS2 / ZnIn2S4 and Ni2P / ZnIn2S4 is significantly increased, and the three-component composite sample Ni2P / 1T-WS2 / ZnIn2S4 has the highest current intensity, further proving that the introduction of dual co-catalysts 1T-WS2 and Ni2P can quickly transfer electrons in the conduction band of ZnIn2S4 and accelerate the separation of photogenerated electrons and holes.

[0013] from Figure 7It can be seen from the electrochemical impedance spectroscopy that the Nyquist radius is in the following order: ZnIn2S4>1T-WS2 / ZnIn2S4>Ni2P / ZnIn2S4>Ni2P / 1T-WS2 / ZnIn2S4, indicating that the introduction of 1T-WS2 and Ni2P co-catalysts can effectively reduce the interfacial charge transfer resistance, and the photogenerated electrons and holes can be quickly separated; at the same time, the synergistic effect of 1T-WS2 and Ni2P can further accelerate the separation rate of photogenerated electrons and holes, and improve the photocatalytic performance of H2O2 production.

[0014] from Figure 8 The photocatalytic H2O2 production experiment shows that pure ZnIn2S4 exhibits poor H2O2 evolution performance due to rapid charge carrier recombination; when 1T-WS2 or Ni2P is loaded onto ZnIn2S4, the resulting binary composite photocatalyst has improved H2O2 evolution performance; when 1T-WS2 and Ni2P are simultaneously loaded onto ZnIn2S4, the resulting ternary composite photocatalyst has the highest H2O2 evolution performance, indicating that the synergistic effect of 1T-WS2 and Ni2P can greatly improve the H2O2 evolution performance of ZnIn2S4.

[0015] The method for preparing the Ni2P / 1T-WS2 / ZnIn2S4 composite photocatalyst of the present invention comprises the following steps:

[0016] 1) Dissolve zinc chloride, indium chloride and thioacetamide in an ethanol aqueous solution, and subject the solution to a hydrothermal reaction at 160-200° C. to obtain light yellow ZnIn2S4 nanosheets after treatment.

[0017] Furthermore, in the above technical solution, the molar ratio of zinc chloride, indium chloride and thioacetamide is 1:2:4.

[0018] 2) Dissolve tungsten chloride and thioacetamide in N,N-dimethylformamide, and subject the solution to a hydrothermal reaction at 180-220° C. to obtain black 1T-WS2 nanoflower balls.

[0019] Furthermore, in the above technical solution, the molar ratio of tungsten chloride to thioacetamide is 1:10.

[0020] 3) red phosphorus and nickel chloride are dissolved in deionized water, and the solution is subjected to a hydrothermal reaction at 140-180° C. to obtain black Ni2P nanoparticles after treatment.

[0021] Furthermore, in the above technical solution, the molar ratio of red phosphorus to nickel chloride is 1:6.

[0022] 4) The ZnIn2S4 nanosheets obtained in step 1) and the 1T-WS2 nanoflower balls obtained in step 2) are dispersed in an aqueous solution and subjected to ultrasonic stirring treatment to obtain a 1T-WS2 / ZnIn2S4 composite photocatalyst.

[0023] Furthermore, in the above technical solution, the mass ratio of ZnIn2S4 to 1T-WS2 is 1:0.01-0.2.

[0024] 5) Dispersing the Ni2P obtained in step 3) and the 1T-WS2 / ZnIn2S4 complex obtained in step 4) into an aqueous solution, subjecting the mixture to ultrasonic stirring treatment, and obtaining a Ni2P / 1T-WS2 / ZnIn2S4 ternary dual-promoter system.

[0025] Furthermore, in the above technical solution, the mass ratio of ZnIn2S4 to 1T-WS2 is 1:0.001-0.1.

[0026] Photocatalytic production of H2O2 operating conditions: light source 300W xenon lamp; catalyst 100mg; deionized water 90mL; isopropanol 10mL. Figure 8 It can be seen that the photocatalytic H2O2 production rate of pure ZnIn2S4 is 0.65mmol g -1 h -1 The photocatalytic H2O2 production rate of Ni2P / ZnIn2S4 was 2.16mmol g -1 h -1 The photocatalytic H2O2 production rate of 1T-WS2 / ZnIn2S4 was 2.84 mmol g -1 h -1 The photocatalytic H2O2 production rate of Ni2P / 1T-WS2 / ZnIn2S4 was 6.34mmol g -1 h -1 , showing significantly enhanced photocatalytic H2O2 production performance.

[0027] Beneficial effects of the present invention:

[0028] The Ni2P / 1T-WS2 / ZnIn2S4 ternary dual promoter system of the present invention, the metal phase 1T-WS2 embedded between ZnIn2S4 and Ni2P forms a Mott Schottky interface with ZnIn2S4, which can effectively accelerate the transfer and separation of charges. The introduction of the promoter Ni2P can effectively capture the electrons transferred from 1T-WS2, provide multiple charge transfer channels, and further improve the charge separation performance; on the other hand, it can also provide a large number of active sites for the photoreduction reaction, thereby greatly improving the photocatalytic H2O2 precipitation performance of the Ni2P / 1T-WS2 / ZnIn2S4 dual promoter. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 XRD patterns of ZnIn2S4, 1T-WS2, Ni2P, Ni2P / ZnIn2S4, 1T-WS2 / ZnIn2S4 and Ni2P / 1T-WS2 / ZnIn2S4 prepared in Example 1 of the present invention;

[0030] Figure 2 XPS spectra of ZnIn2S4, 1T-WS2, Ni2P and Ni2P / 1T-WS2 / ZnIn2S4 prepared in Example 1 of the present invention;

[0031] Figure 3 SEM images of ZnIn2S4, 1T-WS2, Ni2P and Ni2P / 1T-WS2 / ZnIn2S4 prepared in Example 1 of the present invention;

[0032] Figure 4 TEM (a) and HRTEM (b) images of Ni2P / 1T-WS2 / ZnIn2S4 prepared in Example 1 of the present invention;

[0033] Figure 5 PL spectra of ZnIn2S4, 1T-WS2 / ZnIn2S4, Ni2P / ZnIn2S4, and Ni2P / 1T-WS2 / ZnIn2S4 prepared in Example 1 of the present invention;

[0034] Figure 6 Transient current spectra of ZnIn2S4, 1T-WS2 / ZnIn2S4, Ni2P / ZnIn2S4, and Ni2P / 1T-WS2 / ZnIn2S4 prepared in Example 1 of the present invention;

[0035] Figure 7 Electrochemical impedance spectra of ZnIn2S4, 1T-WS2 / ZnIn2S4, Ni2P / ZnIn2S4, and Ni2P / 1T-WS2 / ZnIn2S4 prepared in Example 1 of the present invention;

[0036] Figure 8 The photocatalytic H2O2 production effect diagram of ZnIn2S4, 1T-WS2 / ZnIn2S4, Ni2P / ZnIn2S4, and Ni2P / 1T-WS2 / ZnIn2S4 prepared in Example 1 of the present invention; DETAILED DESCRIPTION

[0037] The present invention is further described below in conjunction with the embodiments. It should be noted that the present invention is not limited to the following embodiments.

[0038] Example 1

[0039] 1) Preparation of ZnIn2S4 nanosheets: 15mL of deionized water and 15mL of anhydrous ethanol were measured and poured into a 50mL beaker to prepare a 50% ethanol aqueous solution, and 0.0545g of ZnCl2, 0.1769g of InCl3 and 0.2404g of CH3CSNH2(TAA) were added in sequence under stirring. Stirring was carried out at room temperature for 10min, and the solution dissolved to a clear state was transferred to a 50mL polytetrafluoroethylene autoclave, and kept in an oven at 180°C for 24h. After the autoclave was naturally cooled to room temperature, it was filtered with a 1000mL suction flask. During the filtration process, it was washed three times with deionized water and anhydrous ethanol respectively, and then the obtained yellow solid sample was transferred to a vacuum drying oven at 60°C and dried for 12h, and ground to obtain a light yellow sample ZnIn2S4 nanosheet.

[0040] 2) Preparation of 1T-WS2 nano flower balls: Weigh 0.7932g WCl6 and 1.5026g TAA in turn and add them to 60mL N,N-dimethylformamide (DMF) and stir vigorously for 1h, then transfer to an ultrasonic machine for ultrasonication for 1h, and then transfer to a 100mL polytetrafluoroethylene high-pressure reactor and keep it in a 200°C oven for 24h. After the reactor is naturally cooled to room temperature, it is filtered with a 1000mL suction bottle and washed with anhydrous ethanol several times during the filtration process. Then, the obtained black solid sample is placed in a 60°C vacuum drying oven and kept for 12h to finally obtain a black powdery solid 1T-WS2 nano flower ball.

[0041] 3) Preparation of Ni2P nanoparticles: Weigh 0.094g NiCl2·6H2O and 0.049g red phosphorus, add them to 30mL 30% ethanol solution in sequence, stir for 30min, then ultrasonicate for 1h, transfer to a 100mL polytetrafluoroethylene reactor, and keep in a 150℃ oven for 12h. After the reaction is cooled to room temperature naturally, wash with deionized water and anhydrous ethanol several times, and then place the obtained black solid sample in a 60℃ vacuum drying oven for 12h to obtain black powdered Ni2P nanoparticles.

[0042] 4) Preparation of 1T-WS2 / ZnIn2S4 composite photocatalyst: Take 5.0 mg of 1T-WS2 obtained in step 2), disperse it in 50 mL of deionized water and ultrasonicate it for 30 min to make it evenly dispersed, then add 0.1 g of ZnIn2S4 sample, continue ultrasonicate it for 90 min and stir it vigorously at room temperature for 10 h, then wash it with deionized water and anhydrous ethanol three times respectively, and then keep it in a vacuum drying oven at 60°C for 12 h to obtain the composite sample 1T-WS2 / ZnIn2S4.

[0043] 5) Preparation of Ni2P / 1T-WS2 / ZnIn2S4 ternary composite photocatalyst: Take 1.0 mg of Ni2P obtained in step 3), disperse it in 50 mL of deionized water and ultrasonicate for 30 min, then take 0.1 g of the 1T-WS2 / ZnIn2S4 two-component composite sample obtained in step 4), continue ultrasonicate for 90 min and vigorously stir for 10 h at room temperature, then wash it three times with deionized water and anhydrous ethanol respectively, and then keep it in a vacuum drying oven at 60°C for 12 h to obtain the dual-cocatalyst Ni2P / 1T-WS2 / ZnIn2S4 system.

[0044] Example 2

[0045] 1) Preparation of ZnIn2S4 nanosheets: 15mL of deionized water and 15mL of anhydrous ethanol were measured and poured into a 50mL beaker to prepare a 50% ethanol aqueous solution, and 0.0545g of ZnCl2, 0.1769g of InCl3 and 0.2404g of CH3CSNH2(TAA) were added in sequence under stirring. Stirring was carried out at room temperature for 10min, and the solution dissolved to a clear state was transferred to a 50mL polytetrafluoroethylene autoclave, and kept in a 160℃ oven for 24h. After the autoclave was naturally cooled to room temperature, it was filtered with a 1000mL suction flask. During the filtration process, it was washed three times with deionized water and anhydrous ethanol respectively, and then the obtained yellow solid sample was transferred to a vacuum drying oven at 60℃ and dried for 12h, and ground to obtain a light yellow sample ZnIn2S4 nanosheet.

[0046] 2) Preparation of 1T-WS2 nano flower balls: Weigh 0.7932g WCl6 and 1.5026g TAA in turn and add them to 60mL N,N-dimethylformamide (DMF) and stir vigorously for 1h, then transfer to an ultrasonic machine for ultrasonication for 1h, and then transfer to a 100mL polytetrafluoroethylene high-pressure reactor and keep it in a 180°C oven for 24h. After the reactor is naturally cooled to room temperature, it is filtered with a 1000mL suction bottle and washed with anhydrous ethanol several times during the filtration process. Then, the obtained black solid sample is placed in a vacuum drying oven at 60°C and kept for 12h to finally obtain a black powdery solid 1T-WS2 nano flower ball.

[0047] 3) Preparation of Ni2P nanoparticles: Weigh 0.094g NiCl2·6H2O and 0.049g red phosphorus, add them to 30mL 30% ethanol solution in sequence, stir for 30min, then ultrasonicate for 1h, transfer to a 100mL polytetrafluoroethylene reactor, and keep in a 140℃ oven for 12h. After the reaction is cooled to room temperature naturally, wash with deionized water and anhydrous ethanol several times, and then place the obtained black solid sample in a 60℃ vacuum drying oven for 12h to obtain black powdered Ni2P nanoparticles.

[0048] 4) Preparation of 1T-WS2 / ZnIn2S4 composite photocatalyst: Take 1.0 mg of 1T-WS2 obtained in step 2) and disperse it in 50 mL of deionized water and ultrasonicate it for 30 minutes to make it evenly dispersed. Then add 0.1 g of ZnIn2S4 sample, continue ultrasonicate it for 90 minutes and stir it vigorously at room temperature for 10 hours, then wash it with deionized water and anhydrous ethanol three times respectively, and then keep it in a vacuum drying oven at 60°C for 12 hours to obtain the composite sample 1T-WS2 / ZnIn2S4.

[0049] 5) Preparation of Ni2P / 1T-WS2 / ZnIn2S4 ternary composite photocatalyst: Take 0.1 mg of Ni2P obtained in step 3), disperse it in 50 mL of deionized water and ultrasonicate it for 30 min, then take 0.1 g of the 1T-WS2 / ZnIn2S4 two-component composite sample obtained in step 4), continue ultrasonicate it for 90 min and stir it vigorously at room temperature for 10 h, then wash it three times with deionized water and anhydrous ethanol respectively, and then keep it in a vacuum drying oven at 60°C for 12 h to obtain the dual-cocatalyst Ni2P / 1T-WS2 / ZnIn2S4 system.

[0050] Example 3

[0051] 1) Preparation of ZnIn2S4 nanosheets: 15mL of deionized water and 15mL of anhydrous ethanol were measured and poured into a 50mL beaker to prepare a 50% ethanol aqueous solution. 0.0545g of ZnCl2, 0.1769g of InCl3 and 0.2404g of CH3CSNH2(TAA) were added in sequence under stirring. Stirring was carried out at room temperature for 10min, and the solution dissolved to a clear state was transferred to a 50mL polytetrafluoroethylene autoclave, and kept in a 200℃ oven for 24h. After the autoclave was naturally cooled to room temperature, it was filtered with a 1000mL suction flask. During the filtration process, it was washed three times with deionized water and anhydrous ethanol respectively, and then the obtained yellow solid sample was transferred to a vacuum drying oven at 60℃ and dried for 12h, and ground to obtain a light yellow sample ZnIn2S4 nanosheet.

[0052] 2) Preparation of 1T-WS2 nano flower balls: Weigh 0.7932g WCl6 and 1.5026g TAA in turn and add them to 60mL N,N-dimethylformamide (DMF) and stir vigorously for 1h, then transfer to an ultrasonic machine for ultrasonication for 1h, and then transfer to a 100mL polytetrafluoroethylene high-pressure reactor and keep it in a 220°C oven for 24h. After the reactor is naturally cooled to room temperature, it is filtered with a 1000mL suction bottle and washed with anhydrous ethanol several times during the filtration process. Then, the obtained black solid sample is placed in a 60°C vacuum drying oven and kept for 12h to finally obtain a black powdery solid 1T-WS2 nano flower ball.

[0053] 3) Preparation of Ni2P nanoparticles: Weigh 0.094g NiCl2·6H2O and 0.049g red phosphorus, add them to 30mL 30% ethanol solution in sequence, stir for 30min, then ultrasonicate for 1h, transfer to a 100mL polytetrafluoroethylene reactor, and keep in an oven at 180℃ for 12h. After the reaction is cooled to room temperature naturally, wash with deionized water and anhydrous ethanol several times, and then place the obtained black solid sample in a vacuum drying oven at 60℃ for 12h to obtain black powdered Ni2P nanoparticles.

[0054] 4) Preparation of 1T-WS2 / ZnIn2S4 composite photocatalyst: Take 20 mg of 1T-WS2 obtained in step 2), disperse it in 50 mL of deionized water and ultrasonicate it for 30 min to make it evenly dispersed, then add 0.1 g of ZnIn2S4 sample, continue ultrasonicate it for 90 min and stir it vigorously at room temperature for 10 h, then wash it with deionized water and anhydrous ethanol three times respectively, and then keep it in a vacuum drying oven at 60 ° C for 12 h to obtain the composite sample 1T-WS2 / ZnIn2S4.

[0055] 5) Preparation of Ni2P / 1T-WS2 / ZnIn2S4 ternary composite photocatalyst: Take 10 mg of Ni2P obtained in step 3), disperse it in 50 mL of deionized water and ultrasonicate for 30 min, then take 0.1 g of the 1T-WS2 / ZnIn2S4 two-component composite sample obtained in step 4), continue ultrasonicate for 90 min and vigorously stir for 10 h at room temperature, then wash it three times with deionized water and anhydrous ethanol respectively, and then keep it in a vacuum drying oven at 60°C for 12 h to obtain the dual-cocatalyst Ni2P / 1T-WS2 / ZnIn2S4 system.

[0056] Example 4 Photocatalytic H2O2 production experiment:

[0057] 100 mg of the catalyst was evenly dispersed in a mixed solution containing 10 mL of isopropanol and 90 mL of water. After ultrasonic treatment for 10 min, oxygen was continuously introduced and stirred for 30 min in the dark. A 300 W xenon lamp was used as the light source for the photocatalytic H2O2 production experiment. Figure 8 It can be seen that the photocatalytic H2O2 evolution rate of pure ZnIn2S4 is 0.65mmol g -1 h -1 The photocatalytic H2O2 evolution rate of the Ni2P / 1T-WS2 / ZnIn2S4 dual-promoter system obtained in Example 1 was as high as 6.34 mmol g -1 h -1 , showing significantly enhanced photocatalytic H2O2 evolution performance.

[0058] The composite photocatalyst prepared by using Example 2-3 can obtain a similar effect of producing hydrogen peroxide.

[0059] The above embodiments describe the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited by the above embodiments, and the above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the scope of the principles of the present invention, the present invention may have various changes and improvements, and these changes and improvements all fall within the scope of protection of the present invention.

Claims

1. Ni2P / 1T-WS2 / ZnIn2S4 composite catalyst, characterized by: The mass ratio of ZnIn2S4, 1T-WS2 and Ni2P in the catalyst is 1:0.01-0.2:0.001-0.1; ZnIn2S4 in the catalyst is a nanosheet structure, 1T-WS2 is a nanoflower ball structure, and Ni2P is a nanoparticle structure; the XRD spectrum has strong diffraction peaks at 21.58°, 27.69°, 30.45°, 39.77°, 52.47° and 55.58°; the XPS spectrum has a peak at 161.4 There are binding energies at 5eV, 162.65eV, 444.94eV, 452.49eV, 1021.26eV, 1044.38eV, 31.88eV, 33.14eV, 33.91eV, 35.34eV, 37.60eV, 129.55eV, 130.25eV, 853.19eV, 872.64eV, 856.61eV, 877.07eV and 862.37eV.

2. The method for preparing the Ni2P / 1T-WS2 / ZnIn2S4 composite catalyst according to claim 1, characterized in that: The steps include: 1) Dissolving zinc chloride, indium chloride and thioacetamide in a 30% ethanol aqueous solution, subjecting the solution to a hydrothermal reaction at 160-200° C., and obtaining light yellow ZnIn2S4 nanosheets after treatment; 2) dissolving tungsten chloride and thioacetamide in N,N-dimethylformamide, subjecting the solution to a hydrothermal reaction at 180-220° C., and obtaining black 1T-WS2 nanoflower balls after treatment; 3) dissolving red phosphorus and nickel chloride in deionized water, subjecting the solution to a hydrothermal reaction at 140-180° C., and obtaining black Ni2P nanoparticles after treatment; 4) dispersing the ZnIn2S4 nanosheets obtained in step 1) and the 1T-WS2 nanoflower balls obtained in step 2) into an aqueous solution, and subjecting them to ultrasonic stirring treatment to obtain a 1T-WS2 / ZnIn2S4 composite photocatalyst; 5) The Ni2P nanoparticles obtained in step 3) and the 1T-WS2 / ZnIn2S4 complex obtained in step 4) are dispersed in an aqueous solution and subjected to ultrasonic stirring treatment to obtain a Ni2P / 1T-WS2 / ZnIn2S4 ternary dual-promoter composite catalyst.

3. The method for preparing the composite photocatalyst according to claim 2, characterized in that: In step 1), the molar ratio of zinc chloride, indium chloride and thioacetamide is 1:2:

4.

4. The method for preparing the composite photocatalyst according to claim 2, characterized in that: In step 2), the molar ratio of tungsten chloride to thioacetamide is 1:

10.

5. The method for preparing the composite photocatalyst according to claim 2, characterized in that: In step 3), the molar ratio of red phosphorus to nickel chloride is 1:

6.

6. The method for preparing the composite photocatalyst according to claim 2, characterized in that: In step 4), the mass ratio of ZnIn2S4 to 1T-WS2 is 1:0.01-0.

2.

7. The method for preparing the composite photocatalyst according to claim 2, characterized in that: In step 5), the mass ratio of ZnIn2S4 to Ni2P is 1:0.001-0.

1.

8. The method for preparing the Ni2P / 1T-WS2 / ZnIn2S4 composite catalyst according to claim 2, characterized in that: The composite photocatalyst is a dual-cocatalyst system that forms a Mott-Schottky junction interface.

9. Use of the Ni2P / 1T-WS2 / ZnIn2S4 composite catalyst as claimed in claim 1 in photocatalytic preparation of H2O2.

10. The use of the Ni2P / 1T-WS2 / ZnIn2S4 composite catalyst in photocatalytic preparation of H2O2 according to claim 9, characterized in that: The operating conditions are as follows: light source: 300W xenon lamp; catalyst: 100mg; deionized water: 90mL; isopropanol: 10mL.

Citation Information

Patent Citations

  • Heavy oil hydrogenation protection catalyst, preparation and applications thereof

    CN102989491A

  • WS2 / ZnIn2S4 composite visible light catalyst and preparation method thereof

    CN108479810A

  • Preparation of nickel phosphide loaded sulfur indium zinc nano microsphere composite material and its application in photocatalytic hydrogen production

    CN110560105A

  • Preparation method of flaky tungsten sulfide / tungsten phosphide / carbon catalytic material

    CN111604073A

  • Preparation method and application of Ni2P / ZnIn2S4 heterojunction photocatalyst

    CN114950506A