Carbon catalyst containing chlorine defect as well as preparation method and application of carbon catalyst
By preparing chlorine-deficient carbon catalysts, the problems of low selectivity and many side reactions in the dehydrogen chloride reaction are solved, and the efficient preparation of 1,1-difluoro-2-iodoethylene and the efficient utilization of waste polymers are achieved. Improves the performance of the catalyst and the purity of the product.
Patent Information
- Application Number
- CN202411044909.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-11-19
AI Technical Summary
The current dehydrogen chloride reaction has low selectivity and many side reactions, which makes it difficult to improve the preparation efficiency and purity of 1,1-difluoro-2-iodoethylene, and the efficient utilization of waste polyvinyl chloride and polyvinyl chloride is difficult to achieve. .
Using a chlorine-containing carbon catalyst, carbonization treatment is made by mixing chlorine-containing polymer, nickel salt and ulotropine for carbonization, and then acidizing with an acid solution to prepare a carbon catalyst with a high specific surface area for use under mild conditions. Activate 1-chloro-1,1-difluoro-2-iodoethane to achieve its highly selective dehydrogen chloride reaction.
Achieve efficient preparation of 1,1-difluoro-2-iodoethylene, reducing the occurrence of side reactions, improving the selectivity of the catalyst and the purity of the product, and converting waste polyvinyl chloride and polyvinyl chloride into high addition value of carbon catalyst.
Smart Images

Figure CN118976524A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of dechlorination reaction, and in particular to a chlorine-defective carbon catalyst and a preparation method and application thereof. Background Art
[0002] Dehydrochlorination is one of the main methods for preparing halogenated alkenes from chloroalkanes. For example, 1,1-difluoro-2-iodoethylene is an important vulcanization point monomer for preparing high-performance fluororubber. It is usually prepared by dehydrochlorination using 1-chloro-1,1-difluoro-2-iodoethane halogenated alkane as raw material. However, since the CI bond energy in the molecular structure of organic matter is much smaller than that of the C-Cl bond and the CF bond, the 1-chloro-1,1-difluoro-2-iodoethane raw material and the 1,1-difluoro-2-iodoethylene product are more likely to undergo deiodination side reactions, resulting in a variety of by-products such as difluorodichloroethane, iodine chloride, and vinylidene fluoride. The boiling point and properties of difluorodichloroethylene are very close to those of the target product 1,1-difluoro-2-iodoethylene, which also brings certain troubles to the subsequent product refining and separation. Therefore, dehydrochlorination is a very important step in the preparation of 1,1-difluoro-2-iodoethylene, and the catalyst and reaction process conditions are the key to solving this problem.
[0003] At present, researchers have developed a variety of catalytic reaction systems to solve these problems. For example, CN112062651A uses metal chloride catalysts such as CaCl2 to carry out gas-phase 1-chloro-1,1-difluoro-2-iodoethane dehydrochlorination at 400°C; CN113307720A uses ZrI4 / C / Fe2O3 magnetic catalyst to convert the raw material into 1,1-difluoro-2-iodoethylene at 150°C for 7h; CN115716775A uses tetrabutylammonium chloride as a phase inversion catalyst. The invention relates to a method for dechlorinating 1-chloro-1,1-difluoro-2-iodoethane by using a phase transfer catalyst and a copper inhibitor at 75°C in a KOH and NaSO3 aqueous solution; CN118108569A uses a tetrabutylammonium bromide phase transfer catalyst and a copper inhibitor under strong alkaline conditions to dechlorinate 1-chloro-1,1-difluoro-2-iodoethane; EP845482A1 dechlorinates 1-chloro-1,1-difluoro-2-iodoethane with a KOH aqueous solution at 80°C; Akkerman et al. (Synthesis of fluorinated dienes by palladium-catalyzed coupling reactions, Chemistry-An Asian Journal, 2008, 3, 719-731) use potassium tert-butoxide and 1-chloro-1,1-difluoro-2-iodoethane in a tert-butanol solvent at room temperature to dechlorinate. However, the use of homogeneous catalysts such as phase transfer will cause certain problems in the subsequent product separation, and the preparation process of magnetic catalysts such as ZrI4 is very cumbersome, resulting in increased process costs. Therefore, it is of great significance to develop a high-performance, low-cost dehydrochlorination reaction system.
[0004] Polyvinyl chloride (PVC) and polyvinylidene chloride (PVDC) are polymer materials made of vinyl chloride and vinylidene chloride, respectively, and are indispensable materials in modern industry and daily life. At the same time, the huge amount of waste PVC and PVDC produced every year causes certain environmental pollution and waste of resources. The functional application of waste PVC and PVDC is also one of the major challenges facing modern society.
[0005] Therefore, it is of great significance to study a chlorine-defective carbon catalyst, its preparation method and application, and realize the efficient preparation of 1,1-difluoro-2-iodoethylene. Summary of the invention
[0006] The object of the present invention is to provide a chlorine-defective carbon catalyst and a preparation method and application thereof, so as to solve the problems of low selectivity and many side reactions of the catalyst in the dehydrochlorination reaction in the prior art.
[0007] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0008] The present invention provides a method for preparing a chlorine-defective carbon catalyst, comprising the following steps:
[0009] (1) mixing a chlorine-containing polymer, a nickel salt and hexamethylenetetramine and then carbonizing the mixture to obtain a carbonized product;
[0010] (2) The carbonization product and an acid solution are mixed and subjected to acidification treatment to obtain a carbon catalyst containing chlorine defects.
[0011] Preferably, in step (1), the chlorine-containing polymer comprises polyvinyl chloride or polyvinyl dichloride; the nickel salt comprises one or more of nickel nitrate, nickel carbonate and nickel acetate; the molar ratio of chlorine in the chlorine-containing polymer to nickel in the nickel salt is 1:1 to 10; and the molar ratio of carbon in the chlorine-containing polymer to nitrogen in hexamethylenetetramine is 0.5 to 2:1.
[0012] Preferably, in step (1), the carbonization treatment is carried out in an inert atmosphere, wherein the inert atmosphere comprises a nitrogen atmosphere, an argon atmosphere or a helium atmosphere, and the gas flow rate of the inert atmosphere is 10 to 100 mL / min.
[0013] Preferably, in step (1), the heating rate of the carbonization treatment is 0.5 to 5°C / min, the temperature of the carbonization treatment is 200 to 350°C, and the time of the carbonization treatment is 2 to 12 hours.
[0014] Preferably, in step (2), the acid solution is a sulfuric acid solution or a nitric acid solution, and the concentration of the acid solution is 5 to 10 mol / L;
[0015] The mass volume ratio of the chlorine-containing polymer to the acid solution is 1 g:5-200 mL.
[0016] Preferably, in step (2), the temperature of the acidification treatment is 80 to 120° C., and the time of the acidification treatment is 2 to 12 hours.
[0017] The present invention provides a chlorine-defective carbon catalyst prepared by the above-mentioned method for preparing the chlorine-defective carbon catalyst.
[0018] The present invention provides an application of the above-mentioned chlorine-defective carbon catalyst, comprising the following steps: dispersing 1-chloro-1,1-difluoro-2-iodoethane and a chlorine-defective carbon catalyst in water, reacting the obtained dispersion to obtain 1,1-difluoro-2-iodoethylene.
[0019] Preferably, the mass concentration of 1-chloro-1,1-difluoro-2-iodoethane in the dispersion is 10-50%; the mass ratio of 1-chloro-1,1-difluoro-2-iodoethane to the chlorine-defective carbon catalyst is 1:0.05-0.5.
[0020] Preferably, the reaction temperature is 80-150° C., and the reaction time is 1-6 hours.
[0021] Beneficial effects of the present invention:
[0022] (1) The present invention prepares a chlorine-defective carbon catalyst from discarded polyvinyl chloride (PVC) and polyvinyl dichloride (PVDC). The chlorine-defective carbon catalyst has a function of selective dehydrochlorination, thereby realizing high value-added applications of PVC or PVDC.
[0023] (2) When preparing the chlorine-defective carbon catalyst, the present invention uses nickel salt as a dechlorinating agent and urotropine as a nitrogen source and a pore-forming agent, which can effectively remove the chlorine in the structure of discarded polyvinyl chloride (PVC) and polyvinyl dichloride (PVDC) during carbonization treatment to obtain a chlorine-defective carbon catalyst with a high specific surface area.
[0024] (3) The chlorine-deficient carbon catalyst prepared by the present invention can highly selectively activate the C-Cl bond in the molecular structure of 1-chloro-1,1-difluoro-2-iodoethane, thereby allowing it to undergo a dehydrochlorination reaction under mild conditions to obtain the target product 1,1-difluoro-2-iodoethylene, while no deiodination reaction occurs. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 This is a nitrogen adsorption-desorption curve of the chlorine-defective carbon catalyst prepared in Example 1;
[0026] Figure 2 This is the TEM image of the chlorine-defective carbon catalyst prepared in Example 1. DETAILED DESCRIPTION
[0027] The present invention provides a method for preparing a chlorine-defective carbon catalyst, comprising the following steps:
[0028] (1) mixing a chlorine-containing polymer, a nickel salt and hexamethylenetetramine and then carbonizing the mixture to obtain a carbonized product;
[0029] (2) The carbonization product and an acid solution are mixed and subjected to acidification treatment to obtain a carbon catalyst containing chlorine defects.
[0030] In the present invention, in the step (1), the chlorine-containing polymer comprises polyvinyl chloride or polyvinyl dichloride, preferably polyvinyl chloride; the nickel salt comprises one or more of nickel nitrate, nickel carbonate and nickel acetate, preferably nickel nitrate and / or nickel acetate, more preferably nickel nitrate; the molar ratio of chlorine in the chlorine-containing polymer to nickel in the nickel salt is 1:1-10, preferably 1:2-9, more preferably 1:3-6; the molar ratio of carbon in the chlorine-containing polymer to nitrogen in hexamine is 0.5-2:1, preferably 0.6-1.5:1, more preferably 0.9-1.2:1.
[0031] In the present invention, if the Ni / Cl molar ratio is too large, the Cl content in the chlorine-deficient carbon catalyst will decrease, and vice versa, but too high or too low Cl content in the catalyst is not conducive to catalytic performance. If the C / N molar ratio decreases (i.e., the amount of urotropine increases), the specific surface area of the chlorine-deficient carbon catalyst will decrease, and the catalytic performance will also decrease.
[0032] In the present invention, in the step (1), the carbonization treatment is carried out in an inert atmosphere, wherein the inert atmosphere comprises a nitrogen atmosphere, an argon atmosphere or a helium atmosphere, preferably a nitrogen atmosphere or an argon atmosphere, and more preferably a nitrogen atmosphere, and the gas flow rate of the inert atmosphere is 10 to 100 mL / min, preferably 30 to 80 mL / min, and more preferably 40 to 60 mL / min.
[0033] In the present invention, in the step (1), the heating rate of the carbonization treatment is 0.5 to 5°C / min, preferably 0.8 to 4°C / min, and more preferably 1 to 3°C / min. The temperature of the carbonization treatment is 200 to 350°C, preferably 210 to 300°C, and more preferably 230 to 270°C. The time of the carbonization treatment is 2 to 12 hours, preferably 4 to 10 hours, and more preferably 4 to 8 hours.
[0034] In the present invention, if the heating rate is too fast, the specific surface area and Cl content of the carbon catalyst containing chlorine defects will decrease, reducing the catalytic performance; if the heating rate is too slow, the Cl content will also decrease, and the slow heating rate will affect the preparation efficiency of the carbon catalyst containing chlorine defects. If the temperature of the carbonization treatment is too high, the specific surface area and Cl content of the carbon catalyst containing chlorine defects will decrease, reducing the catalytic performance; if the temperature of the carbonization treatment is too low, the specific surface area will also decrease, and the Cl content will increase.
[0035] In the present invention, in step (2), the acid solution is a sulfuric acid solution or a nitric acid solution, preferably a nitric acid solution, and the concentration of the acid solution is 5 to 10 mol / L, preferably 6 to 9 mol / L, and more preferably 6 to 8 mol / L;
[0036] The mass volume ratio of the chlorine-containing polymer to the acid solution is 1 g: 5 to 200 mL, preferably 1 g: 10 to 100 mL, and more preferably 1 g: 30 to 50 mL.
[0037] In the present invention, in step (2), the temperature of the acidification treatment is 80 to 120°C, preferably 90 to 110°C, and more preferably 90°C, 95°C, 100°C, 105°C or 110°C; the time of the acidification treatment is 2 to 12h, preferably 4 to 10h, and more preferably 6 to 8h.
[0038] The present invention provides a chlorine-defective carbon catalyst prepared by the above-mentioned method for preparing the chlorine-defective carbon catalyst.
[0039] The present invention provides an application of the above-mentioned chlorine-defective carbon catalyst, comprising the following steps: dispersing 1-chloro-1,1-difluoro-2-iodoethane and a chlorine-defective carbon catalyst in water, reacting the obtained dispersion to obtain 1,1-difluoro-2-iodoethylene.
[0040] In the present invention, the mass concentration of 1-chloro-1,1-difluoro-2-iodoethane in the dispersion is 10-50%, preferably 15-40%, and more preferably 20-35%; the mass ratio of 1-chloro-1,1-difluoro-2-iodoethane to the chlorine-defective carbon catalyst is 1:0.05-0.5, preferably 1:0.08-0.4, and more preferably 1:0.1-0.3.
[0041] In the present invention, the reaction temperature is 80-150°C, preferably 90-140°C, more preferably 100-130°C, and the reaction time is 1-6h, preferably 2-5h, more preferably 2h, 3h, 4h.
[0042] The technical solutions provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention.
[0043] The Cl content in the polyvinyl chloride and polyvinyl dichloride used in the embodiments of the present invention is as follows: the Cl content in the polyvinyl chloride is 16 mmol / g, and the Cl content in the polyvinyl dichloride is 20.6 mmol / g.
[0044] Example 1
[0045] 5 g of PVC, 2.4 g of nickel nitrate and 6.2 g of urotropine were mixed evenly, wherein the molar ratio of Cl in PVC and Ni in nickel nitrate was 1:6, and the molar ratio of C in PVC and N in urotropine was 0.9:1. The obtained mixture was transferred to a high-temperature tube furnace, and nitrogen was filled at a flow rate of 50 mL / min. In a nitrogen atmosphere, the temperature was increased to 250°C at a heating rate of 1.0°C / min, and carbonization treatment was carried out at 250°C for 4 hours to obtain a carbonized product.
[0046] 2 g of the carbonized product was mixed with 80 mL of sulfuric acid solution (concentration of 6 mol / L), and the mixture was acidified at 90° C. for 5 h. The acidified product was dried at 100° C. for 4 h to obtain a chlorine-defective carbon catalyst.
[0047] Example 2
[0048] 5 g of PVDC, 12.2 g of nickel carbonate and 2.4 g of urotropine were mixed evenly, wherein the molar ratio of Cl in PVDC and Ni in nickel carbonate was 1:1, and the molar ratio of C in PVDC and N in urotropine was 1.5:1. The obtained mixture was transferred to a high-temperature tube furnace, and nitrogen was filled at a flow rate of 100 mL / min. In a nitrogen atmosphere, the temperature was increased to 270°C at a heating rate of 2.5°C / min, and carbonization treatment was carried out at 270°C for 6 hours to obtain a carbonized product.
[0049] 2 g of the carbonized product was mixed with 60 mL of sulfuric acid solution (concentration of 8 mol / L), and the mixture was acidified at 95° C. for 8 h. The acidified product was dried at 120° C. for 2 h to obtain a chlorine-defective carbon catalyst.
[0050] Example 3
[0051] 5 g of PVDC, 9.1 g of nickel acetate and 3.0 g of urotropine were mixed evenly, wherein the molar ratio of Cl in PVDC and Ni in nickel acetate was 1:2, and the molar ratio of C in PVDC and N in urotropine was 1.2:1. The obtained mixture was transferred to a high-temperature tube furnace, and nitrogen was filled at a flow rate of 80 mL / min. In a nitrogen atmosphere, the temperature was increased to 210°C at a heating rate of 0.5°C / min, and carbonization treatment was carried out at 210°C for 2 h to obtain a carbonized product.
[0052] 2 g of the carbonized product was mixed with 100 mL of sulfuric acid solution (with a concentration of 10 mol / L), and the mixture was acidified at 105° C. for 3 h. The acidified product was dried at 110° C. for 3 h to obtain a chlorine-defective carbon catalyst.
[0053] Example 4
[0054] 5 g of PVC, 1.9 g of nickel carbonate and 9.3 g of urotropine were mixed evenly, wherein the molar ratio of Cl in PVC and Ni in nickel carbonate was 1:5, and the molar ratio of C in PVC and N in urotropine was 0.6:1. The obtained mixture was transferred to a high-temperature tube furnace, and nitrogen was filled at a flow rate of 50 mL / min. In a nitrogen atmosphere, the temperature was increased to 200°C at a heating rate of 3.0°C / min, and carbonization treatment was carried out at 200°C for 8 hours to obtain a carbonized product.
[0055] 2 g of the carbonized product was mixed with 120 mL of sulfuric acid solution (concentration of 9 mol / L), and the mixture was acidified at 80° C. for 12 h. The acidified product was dried at 105° C. for 5 h to obtain a chlorine-defective carbon catalyst.
[0056] Example 5
[0057] 5 g of PVDC, 1.5 g of nickel carbonate and 7.2 g of urotropine were mixed evenly, wherein the molar ratio of Cl in PVDC and Ni in nickel carbonate was 1:8, and the molar ratio of C in PVDC and N in urotropine was 0.5:1. The obtained mixture was transferred to a high-temperature tube furnace, and nitrogen was filled at a flow rate of 70 mL / min. In a nitrogen atmosphere, the temperature was increased to 310°C at a heating rate of 5.0°C / min, and carbonization treatment was carried out at 310°C for 10 hours to obtain a carbonized product.
[0058] 2 g of the carbonized product was mixed with 160 mL of sulfuric acid solution (concentration of 5 mol / L), and the mixture was acidified at 85° C. for 10 h. The acidified product was dried at 95° C. for 6 h to obtain a chlorine-defective carbon catalyst.
[0059] Example 6
[0060] 5 g of PVC, 4.7 g of nickel acetate and 3.1 g of urotropine were mixed evenly, wherein the molar ratio of Cl in PVC and Ni in nickel acetate was 1:3, and the molar ratio of C in PVC and N in urotropine was 1.8:1. The obtained mixture was transferred to a high-temperature tube furnace, and nitrogen was filled at a flow rate of 100 mL / min. In a nitrogen atmosphere, the temperature was increased to 330°C at a heating rate of 3.5°C / min, and carbonization treatment was carried out at 330°C for 12 hours to obtain a carbonized product.
[0061] 2 g of the carbonized product was mixed with 40 mL of sulfuric acid solution (concentration of 7 mol / L), and the mixture was acidified at 110° C. for 8 h. The acidified product was dried at 115° C. for 2 h to obtain a chlorine-defective carbon catalyst.
[0062] Example 7
[0063] 5 g of PVC, 2.1 g of nickel nitrate and 7.0 g of urotropine were mixed evenly, wherein the molar ratio of Cl in PVC and Ni in nickel nitrate was 1:7, and the molar ratio of C in PVC and N in urotropine was 0.8:1. The obtained mixture was transferred to a high-temperature tube furnace, and argon was filled at a flow rate of 40 mL / min. In an argon atmosphere, the temperature was raised to 350°C at a heating rate of 4.0°C / min, and carbonization treatment was carried out at 350°C for 5 hours to obtain a carbonized product.
[0064] 2 g of the carbonized product was mixed with 20 mL of nitric acid solution (concentration of 8.5 mol / L), and the mixture was acidified at 120° C. for 6 h. The acidified product was dried at 100° C. for 4 h to obtain a chlorine-defective carbon catalyst.
[0065] Example 8
[0066] 5 g of PVDC, 2.1 g of nickel nitrate and 1.8 g of urotropine were mixed evenly, wherein the molar ratio of Cl in PVDC and Ni in nickel nitrate was 1:9, and the molar ratio of C in PVDC and N in urotropine was 2:1. The obtained mixture was transferred to a high-temperature tube furnace, and helium was filled at a flow rate of 100 mL / min. In the helium atmosphere, the temperature was increased to 230°C at a heating rate of 2.0°C / min, and the mixture was carbonized at 230°C for 7 hours to obtain a carbonized product.
[0067] 2 g of the carbonized product was mixed with 140 mL of nitric acid solution (concentration of 9.5 mol / L), and the mixture was acidified at 115° C. for 7 h. The acidified product was dried at 105° C. for 3 h to obtain a chlorine-defective carbon catalyst.
[0068] Example 9
[0069] 5 g of PVC, 1.4 g of nickel acetate and 3.5 g of urotropine were mixed evenly, wherein the molar ratio of Cl in PVC to Ni in nickel acetate was 1:10, and the molar ratio of C in PVC to N in urotropine was 1.6:1. The obtained mixture was transferred to a high-temperature tube furnace, and helium was filled at a flow rate of 60 mL / min. In the helium atmosphere, the temperature was increased to 300°C at a heating rate of 4.5°C / min, and carbonization treatment was carried out at 300°C for 9 hours to obtain a carbonized product.
[0070] 2 g of the carbonized product was mixed with 200 mL of nitric acid solution (concentration of 6.5 mol / L), and the mixture was acidified at 100° C. for 5 h. The acidified product was dried at 110° C. for 3 h to obtain a chlorine-defective carbon catalyst.
[0071] The chlorine-deficient carbon catalysts prepared in Examples 1 to 9 are denoted as AI, respectively.
[0072] Example 10
[0073] 20 g of 1-chloro-1,1-difluoro-2-iodoethane and 2 g of a chlorine-deficient carbon catalyst (A) were dispersed in 100 mL of deionized water, and then placed in a 300 mL high-pressure reactor. The air in the high-pressure reactor was completely replaced with nitrogen. The temperature was raised to 100 ° C. and reacted for 2 hours. After the reaction was completed, the temperature was lowered to room temperature. After filtering to remove the catalyst, the liquid product was allowed to stand for stratification, and the organic phase was taken to obtain 1,1-difluoro-2-iodoethylene.
[0074] Embodiment 11
[0075] 40 g of 1-chloro-1,1-difluoro-2-iodoethane and 2 g of a chlorine-deficient carbon catalyst (B) were dispersed in 100 mL of deionized water, and then placed in a 300 mL high-pressure reactor. The air in the high-pressure reactor was completely replaced with nitrogen. The temperature was raised to 120° C. and reacted for 4 hours. After the reaction was completed, the temperature was lowered to room temperature. After filtering to remove the catalyst, the liquid product was allowed to stand and separate, and the organic phase was taken to obtain 1,1-difluoro-2-iodoethylene.
[0076] Example 12
[0077] 50 g of 1-chloro-1,1-difluoro-2-iodoethane and 7.5 g of a chlorine-deficient carbon catalyst (C) were dispersed in 100 mL of deionized water, and then placed in a 300 mL high-pressure reactor. The air in the high-pressure reactor was completely replaced with nitrogen. The temperature was raised to 80° C. and reacted for 3 hours. After the reaction was completed, the temperature was lowered to room temperature. After filtering to remove the catalyst, the liquid product was allowed to stand and stratify, and the organic phase was taken to obtain 1,1-difluoro-2-iodoethylene.
[0078] Example 13
[0079] 35 g of 1-chloro-1,1-difluoro-2-iodoethane and 8.75 g of a chlorine-deficient carbon catalyst (D) were dispersed in 100 mL of deionized water, and then placed in a 300 mL high-pressure reactor. The air in the high-pressure reactor was completely replaced with nitrogen. The temperature was raised to 90° C. for reaction for 1 h. After the reaction was completed, the temperature was lowered to room temperature. After filtering to remove the catalyst, the liquid product was allowed to stand and separate, and the organic phase was taken to obtain 1,1-difluoro-2-iodoethylene.
[0080] Embodiment 14
[0081] 10 g of 1-chloro-1,1-difluoro-2-iodoethane and 3 g of a chlorine-deficient carbon catalyst (E) were dispersed in 100 mL of deionized water, and then placed in a 300 mL high-pressure reactor. The air in the high-pressure reactor was completely replaced with nitrogen. The temperature was raised to 130° C. and reacted for 5 hours. After the reaction was completed, the temperature was lowered to room temperature. After filtering to remove the catalyst, the liquid product was allowed to stand and separate, and the organic phase was taken to obtain 1,1-difluoro-2-iodoethylene.
[0082] Embodiment 15
[0083] 30 g of 1-chloro-1,1-difluoro-2-iodoethane and 12 g of a chlorine-deficient carbon catalyst (F) were dispersed in 100 mL of deionized water, and then placed in a 300 mL high-pressure reactor. The air in the high-pressure reactor was completely replaced with nitrogen. The temperature was raised to 150° C. and reacted for 6 hours. After the reaction was completed, the temperature was lowered to room temperature. After filtering to remove the catalyst, the liquid product was allowed to stand and separate, and the organic phase was taken to obtain 1,1-difluoro-2-iodoethylene.
[0084] Example 16
[0085] 25 g of 1-chloro-1,1-difluoro-2-iodoethane and 12.5 g of a chlorine-deficient carbon catalyst (G) were dispersed in 100 mL of deionized water, and then placed in a 300 mL high-pressure reactor. The air in the high-pressure reactor was completely replaced with nitrogen. The temperature was raised to 140° C. and reacted for 3 h. After the reaction was completed, the temperature was lowered to room temperature. After filtering to remove the catalyst, the liquid product was allowed to stand and stratify, and the organic phase was taken to obtain 1,1-difluoro-2-iodoethylene.
[0086] Embodiment 17
[0087] 15 g of 1-chloro-1,1-difluoro-2-iodoethane and 6.5 g of a chlorine-deficient carbon catalyst (H) were dispersed in 100 mL of deionized water, and then placed in a 300 mL high-pressure reactor. The air in the high-pressure reactor was completely replaced with nitrogen. The temperature was raised to 110° C. and reacted for 4 hours. After the reaction was completed, the temperature was lowered to room temperature. After filtering to remove the catalyst, the liquid product was allowed to stand and separate, and the organic phase was taken to obtain 1,1-difluoro-2-iodoethylene.
[0088] Embodiment 18
[0089] 45 g of 1-chloro-1,1-difluoro-2-iodoethane and 15 g of a chlorine-deficient carbon catalyst (I) were dispersed in 100 mL of deionized water, and then placed in a 300 mL autoclave. The air in the autoclave was completely replaced with nitrogen. The temperature was raised to 120° C. and reacted for 5 h. After the reaction was completed, the temperature was lowered to room temperature. After filtering to remove the catalyst, the liquid product was allowed to stand and separate, and the organic phase was taken to obtain 1,1-difluoro-2-iodoethylene.
[0090] Comparative Example 1
[0091] 5 g of PVC and 6.2 g of urotropine were mixed evenly, wherein the molar ratio of C in PVC to N in urotropine was 0.9:1. The obtained mixture was transferred to a high-temperature tube furnace, and nitrogen was filled at a flow rate of 50 mL / min. In a nitrogen atmosphere, the temperature was increased to 450°C at a heating rate of 1.0°C / min. The mixture was carbonized at 450°C for 4 hours to obtain a carbonized product.
[0092] 0.5 g of the carbonized product was mixed with 20 mL of sulfuric acid solution (concentration of 6 mol / L), and acidified at 90°C for 4 h. The acidified product was dried at 100°C for 4 h to obtain a chlorine-defective carbon catalyst, which was recorded as C-1.
[0093] 20 g of 1-chloro-1,1-difluoro-2-iodoethane and 2 g of chlorine-deficient carbon catalyst (C-1) were dispersed in 100 mL of deionized water, and then placed in a 300 mL high-pressure reactor. The air in the high-pressure reactor was completely replaced with nitrogen. The temperature was raised to 120 ° C and reacted for 2 hours. After the reaction was completed, the temperature was lowered to room temperature. After filtering to remove the catalyst, the liquid product was allowed to stand and stratify, and the organic phase was taken to obtain 1,1-difluoro-2-iodoethylene.
[0094] Comparative Example 2
[0095] 5 g of PVC and 2.4 g of nickel nitrate were evenly mixed, wherein the molar ratio of Cl in PVC to Ni in nickel nitrate was 1:6, and the obtained mixture was transferred to a high-temperature tube furnace, and nitrogen was filled at a flow rate of 50 mL / min. In a nitrogen atmosphere, the temperature was increased to 450°C at a heating rate of 1.0°C / min, and carbonization treatment was carried out at 450°C for 4 hours to obtain a carbonized product.
[0096] Take 0.5 g of the carbonized product and mix it with 20 mL of sulfuric acid solution (concentration of 6 mol / L), acidify it at 90°C for 4 h, and dry the acidified product at ***°C for *** h to obtain a chlorine-defective carbon catalyst, which is recorded as C-2.
[0097] 20 g of 1-chloro-1,1-difluoro-2-iodoethane and 2 g of chlorine-deficient carbon catalyst (C-2) were dispersed in 100 mL of deionized water, and then placed in a 300 mL high-pressure reactor. The air in the high-pressure reactor was replaced with nitrogen. The temperature was raised to 120 ° C and reacted for 2 hours. After the reaction was completed, the temperature was lowered to room temperature. After filtering to remove the catalyst, the liquid product was allowed to stand and stratify, and the organic phase was taken to obtain 1,1-difluoro-2-iodoethylene.
[0098] Comparative Example 3
[0099] 5 g of PVC, 2.4 g of nickel nitrate and 6.2 g of urotropine were mixed evenly, wherein the molar ratio of Cl in PVC and Ni in nickel nitrate was 1:6, and the molar ratio of C in PVC and N in urotropine was 0.9:1. The obtained mixture was transferred to a high-temperature tube furnace, and nitrogen was filled at a flow rate of 50 mL / min. In a nitrogen atmosphere, the temperature was raised to 250°C at a heating rate of 10°C / min, and carbonization treatment was carried out at 250°C for 4 hours to obtain a carbonized product.
[0100] 0.5 g of the carbonized product was mixed with 20 mL of sulfuric acid solution (concentration of 6 mol / L), and acidified at 90°C for 5 h. The acidified product was dried at 100°C for 4 h to obtain a chlorine-defective carbon catalyst, which was recorded as C-3.
[0101] 20 g of 1-chloro-1,1-difluoro-2-iodoethane and 2 g of a chlorine-deficient carbon catalyst (C-3) were dispersed in 100 mL of deionized water, and then placed in a 300 mL high-pressure reactor. The air in the high-pressure reactor was completely replaced with nitrogen. The temperature was raised to 100 ° C and reacted for 2 hours. After the reaction was completed, the temperature was lowered to room temperature. After filtering to remove the catalyst, the liquid product was allowed to stand for stratification, and the organic phase was taken to obtain 1,1-difluoro-2-iodoethylene.
[0102] Comparative Example 4
[0103] The difference from Comparative Example 3 is that the heating rate is 0.1°C / min, and a carbon catalyst containing chlorine defects is obtained, which is recorded as C-4.
[0104] 20 g of 1-chloro-1,1-difluoro-2-iodoethane and 2 g of a chlorine-deficient carbon catalyst (C-4) were dispersed in 100 mL of deionized water, and then placed in a 300 mL high-pressure reactor. The air in the high-pressure reactor was completely replaced with nitrogen. The temperature was raised to 100 ° C and reacted for 2 hours. After the reaction was completed, the temperature was lowered to room temperature. After filtering to remove the catalyst, the liquid product was allowed to stand and separate into layers, and the organic phase was taken to obtain 1,1-difluoro-2-iodoethylene.
[0105] Comparative Example 5
[0106] The difference from Comparative Example 3 is that the temperature of the carbonization treatment is 500°C, and a carbon catalyst containing chlorine defects is obtained, which is recorded as C-5.
[0107] 20 g of 1-chloro-1,1-difluoro-2-iodoethane and 2 g of a chlorine-deficient carbon catalyst (C-5) were dispersed in 100 mL of deionized water, and then placed in a 300 mL autoclave. The air in the autoclave was completely replaced with nitrogen. The temperature was raised to 100 ° C and reacted for 2 hours. After the reaction was completed, the temperature was lowered to room temperature. After filtering to remove the catalyst, the liquid product was allowed to stand for stratification, and the organic phase was taken to obtain 1,1-difluoro-2-iodoethylene.
[0108] Comparative Example 6
[0109] The difference from Comparative Example 3 is that the temperature of the carbonization treatment is 150°C, and a carbon catalyst containing chlorine defects is obtained, which is recorded as C-6.
[0110] 20 g of 1-chloro-1,1-difluoro-2-iodoethane and 2 g of a chlorine-deficient carbon catalyst (C-6) were dispersed in 100 mL of deionized water, and then placed in a 300 mL high-pressure reactor. The air in the high-pressure reactor was completely replaced with nitrogen. The temperature was raised to 100 ° C and reacted for 2 hours. After the reaction was completed, the temperature was lowered to room temperature. After filtering to remove the catalyst, the liquid product was allowed to stand and separate into layers, and the organic phase was taken to obtain 1,1-difluoro-2-iodoethylene.
[0111] Performance Verification:
[0112] (1) The specific surface area and Cl content of the chlorine-deficient carbon catalysts prepared in Examples 1 to 9 and Comparative Examples 1 to 6 were measured:
[0113] The specific surface area test method of carbon catalyst containing chlorine defects: The test was carried out using the ASAP2020 physical adsorption instrument of Micromeritics, USA. The sample was first vacuum degassed at 150°C for 10 hours, and then the sample was placed at -196°C for N2 adsorption and desorption experiments to obtain the N2 adsorption and desorption curve. The BET (Brunauer-Emmett-Teller) calculation method was used to obtain the specific surface area data (m 2 / g).
[0114] Test method for Cl content of chlorine-defective carbon catalyst (refer to GB / T 7139-2023 Determination of chlorine content of plastic vinyl chloride homopolymer and copolymer). Weigh 0.25g of dry sample and 5.0g of sodium peroxide respectively and place them in a combustion bomb. After sufficient combustion, pour the material into 100mL of distilled water to dissolve, and then use 0.1mol / L silver nitrate solution as the standard titrant to titrate on a potentiometric titrator. Calculate the Cl content (x) in the sample according to the following formula: where C, M, V1, V2 and m are the molar concentration of silver nitrate (mol / L), the molar mass of Cl (g / mol), the volume of silver nitrate titrant consumed by the sample (mL), the volume of silver nitrate titrant consumed by the blank sample (mL) and the mass of the sample (g), respectively.
[0115] Figure 1 The nitrogen adsorption-desorption curve of the chlorine-defective carbon catalyst prepared in Example 1 is shown in FIG. Figure 1 It can be seen that the obtained carbon catalyst has a higher specific surface area.
[0116] The specific surface area and Cl content test results of the chlorine-defective carbon catalyst are shown in Table 1:
[0117] Table 1 Test results of specific surface area and Cl content of chlorine-deficient carbon catalysts
[0118]
[0119]
[0120] (2) Figure 2 TEM image of the chlorine-defective carbon catalyst prepared in Example 1. Figure 2 It can be seen that the prepared chlorine-defective carbon catalyst is a carbon material with nanoscale pore size.
[0121] (3) The conversion rate of 1-chloro-1,1-difluoro-2-iodoethane and the selectivity of 1,1-difluoro-2-iodoethylene in Examples 10 to 18 and Comparative Examples 1 to 6 were measured. The results are shown in Table 2:
[0122] Calculation method of the yield of 1,1-difluoro-2-iodoethylene product: Agilent Model 8890 gas chromatograph was used for testing. The liquid products of each embodiment and comparative example were collected for quantitative analysis in a gas chromatograph, the injection port temperature was 240°C, the column oven was 100°C for 5 minutes, then the temperature was increased to 150°C at a rate of 5°C / min, and maintained for 5 minutes, the chromatographic column was an HP-5 capillary column, the chromatographic column was 30m long, the diameter was 0.25mm, the film thickness was 0.25um, the chromatographic column carrier gas was helium, the column flow rate was 0.5mL / min, the detector was an FID detector, and the detector temperature was 250°C. 1,1-difluoro-2-iodoethylene product yield = m(1,1-difluoro-2-iodoethylene) / m(1-chloro-1,1-difluoro-2-iodoethane)×100%, wherein m(1,1-difluoro-2-iodoethylene) and m(1-chloro-1,1-difluoro-2-iodoethane) are the mass (g) of 1,1-difluoro-2-iodoethylene quantified in gas chromatography and the mass (g) of 1-chloro-1,1-difluoro-2-iodoethane added before the reaction, respectively.
[0123] Table 2 Test results of conversion rate of 1-chloro-1,1-difluoro-2-iodoethane and selectivity of 1,1-difluoro-2-iodoethylene in Examples 10 to 18 and Comparative Examples 1 to 6
[0124]
[0125]
[0126] From the test results in Tables 1 and 2, it can be seen that the type of chlorine-containing polymer, the type of nickel salt, the mass ratio of the two, the temperature of carbonization treatment, the heating rate of carbonization treatment and the conditions of acidification treatment in the preparation process of chlorine-defective carbon catalyst have an effect on the specific surface area and chlorine content of the chlorine-defective carbon catalyst, and thus affect the product yield of 1,1-difluoro-2-iodoethylene prepared by dehydrochlorination of 1-chloro-1,1-difluoro-2-iodoethane. In addition, the concentration of 1-chloro-1,1-difluoro-2-iodoethane, the amount of catalyst, the reaction temperature and the reaction time also have a certain effect on the yield of 1,1-difluoro-2-iodoethylene.
[0127] As can be seen from the above embodiments, the present invention provides a chlorine-defective carbon catalyst and its preparation method and application. First, a chlorine-containing polymer, a nickel salt and urotropine are mixed and carbonized to obtain a carbonized product; then the carbonized product and an acid solution are mixed and acidified to obtain a chlorine-defective carbon catalyst. The present invention uses nickel salt as a dechlorinating agent and urotropine as a nitrogen source and a pore-forming agent, which can effectively remove the chlorine from the structure of discarded polyvinyl chloride (PVC) and polyvinyl dichloride (PVDC) during carbonization treatment to obtain a chlorine-defective carbon catalyst with a high specific surface area. The above-prepared chlorine-defective carbon catalyst can highly selectively activate the C-Cl bond in the molecular structure of 1-chloro-1,1-difluoro-2-iodoethane, so that it undergoes a dehydrochlorination reaction under mild conditions to obtain the target product 1,1-difluoro-2-iodoethylene.
[0128] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing a chlorine-defective carbon catalyst, It is characterized in that The steps include: (1) mixing a chlorine-containing polymer, a nickel salt and hexamethylenetetramine and then carbonizing the mixture to obtain a carbonized product; (2) The carbonization product and an acid solution are mixed and subjected to an acidification treatment to obtain a carbon catalyst containing chlorine defects.
2. The method for preparing the chlorine-deficient carbon catalyst according to claim 1, It is characterized in that In the step (1), the chlorine-containing polymer comprises polyvinyl chloride or polyvinyl dichloride; the nickel salt comprises one or more of nickel nitrate, nickel carbonate and nickel acetate; the molar ratio of chlorine in the chlorine-containing polymer to nickel in the nickel salt is 1:1 to 10; and the molar ratio of carbon in the chlorine-containing polymer to nitrogen in hexamethylenetetramine is 0.5 to 2:
1.
3. The method for preparing the chlorine-deficient carbon catalyst according to claim 1 or 2, It is characterized in that In the step (1), the carbonization treatment is carried out in an inert atmosphere, wherein the inert atmosphere comprises a nitrogen atmosphere, an argon atmosphere or a helium atmosphere, and the gas flow rate of the inert atmosphere is 10 to 100 mL / min.
4. The method for preparing the chlorine-deficient carbon catalyst according to claim 3, It is characterized in that In the step (1), the heating rate of the carbonization treatment is 0.5 to 5°C / min, the temperature of the carbonization treatment is 200 to 350°C, and the time of the carbonization treatment is 2 to 12 hours.
5. A method for preparing a chlorine-deficient carbon catalyst according to claim 1, 2 or 4, It is characterized in that In the step (2), the acid solution is a sulfuric acid solution or a nitric acid solution, and the concentration of the acid solution is 5 to 10 mol / L; The mass volume ratio of the chlorine-containing polymer to the acid solution is 1 g:5-200 mL.
6. The method for preparing the chlorine-deficient carbon catalyst according to claim 5, It is characterized in that In the step (2), the temperature of the acidification treatment is 80 to 120° C., and the time of the acidification treatment is 2 to 12 hours.
7. A chlorine-deficient carbon catalyst obtained by the method for preparing a chlorine-deficient carbon catalyst according to any one of claims 1 to 6.
8. Use of the chlorine-deficient carbon catalyst according to claim 7, It is characterized in that The method comprises the following steps: dispersing 1-chloro-1,1-difluoro-2-iodoethane and a carbon catalyst containing chlorine defects in water, and reacting the obtained dispersion to obtain 1,1-difluoro-2-iodoethylene.
9. Use of the chlorine-deficient carbon catalyst according to claim 8, It is characterized in that The mass concentration of 1-chloro-1,1-difluoro-2-iodoethane in the dispersion is 10-50%; the mass ratio of 1-chloro-1,1-difluoro-2-iodoethane to the chlorine-defective carbon catalyst is 1:0.05-0.
5.
10. Use of the chlorine-deficient carbon catalyst according to claim 8 or 9, It is characterized in that The reaction temperature is 80-150° C., and the reaction time is 1-6 hours.
Citation Information
Patent Citations
Method for preparation of nitrogen doped activated carbon from chlorine-containing organic polymer waste
CN103183345A
Synthesis method of 1, 1-difluoro-2-iodoethylene
CN112062651A
Preparation method and application of waste plastic derived carbon coated metal nanoparticle catalyst
CN118237580A
Method of hydrodechlorinating chloroaromatic compounds
RU2402512C1