Nickel-based superalloy annular piece and forging method thereof
By adding rare earth element La to nickel-based high-temperature alloy and adopting specific forging steps, the problem of degradation of mechanical properties of nickel-based high-temperature alloy ring parts at high temperatures is solved, grain refinement and mechanical properties are achieved, and mechanical properties are improved, providing higher Quality products.
Patent Information
- Application Number
- CN202411078022.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-07
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-08-07
AI Technical Summary
The existing nickel-based high-temperature alloy annular parts have deteriorated mechanical properties due to grain mixing and carbide agglomeration at high temperatures, and there are problems of uneven tissue structure and uneven stress distribution.
The rare earth element La is added to the nickel-based high-temperature alloy blank. Through first-fire heating and insulation, upset punching, rolling ring, second-fire forging and solution treatment, the grain size distribution is controlled to inhibit grain boundary migration and carbonization. The substance agglomerates and increases the recrystallization temperature and forging temperature.
The grain refinement and mechanical properties of nickel-based high-temperature alloy ring parts have been achieved, the high-temperature tensile performance has been significantly improved, and the higher quality products have been provided.
Smart Images

Figure CN118976867A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of metal forging, and in particular relates to a nickel-based high-temperature alloy ring part and a forging method thereof. Background Art
[0002] Nickel-based high-temperature alloy rings are widely used in the aerospace field. Mechanical properties are an important indicator of the quality of high-temperature alloy materials. In the aerospace service environment, the material's load-bearing capacity is required to be high. High-temperature components such as aircraft engine combustion chambers and flame tubes have higher temperature-bearing capacity requirements for materials, and solid solution-strengthened alloys can improve the thermal strength of alloys.
[0003] However, the grains at the grain boundaries of the existing solid solution strengthened nickel-based high-temperature alloy ring parts are easy to grow, resulting in a mixture of large and small grains in the entire alloy, that is, the formation of a mixed crystal structure; and because the solid solution strengthened nickel-based high-temperature alloy ring parts usually contain a large amount of solid solution strengthening elements such as Cr and Mo, these elements are easy to enrich and form carbides in the form of agglomerates. At high temperatures, the presence of these carbides will cause uneven recrystallization and promote nucleation, thereby promoting recrystallization, which will lead to fine grains around the carbides and form a mixed crystal structure in the alloy; at the same time, carbide agglomeration will also lead to uneven stress distribution during thermal deformation, resulting in stress concentration and the formation of microcracks. The presence of mixed crystal structure and microcracks will lead to a decrease in the mechanical properties of the nickel-based high-temperature alloy ring parts.
[0004] In view of this, it is necessary to provide a forging method for a nickel-based high-temperature alloy ring part to prepare a nickel-based high-temperature alloy ring part with uniform grain size distribution and fine grains. Summary of the invention
[0005] Therefore, the present invention provides a forging method for a nickel-based high-temperature alloy ring part, which can solve the technical problem of reduced mechanical properties of the nickel-based high-temperature alloy ring part in the prior art.
[0006] In order to solve the above problems, the present invention provides a forging method of a nickel-based high-temperature alloy ring, comprising the following steps:
[0007] Step 1) heating and heat preservation of a nickel-based high-temperature alloy blank, and then upsetting, punching, and ring rolling in sequence to obtain a ring blank; wherein the nickel-based high-temperature alloy blank contains La element;
[0008] Step 2) performing double-forging on the ring blank, performing solid solution treatment after heat preservation treatment, and obtaining the nickel-based high-temperature alloy ring part after cooling; wherein the temperature of the double-forging is 1130-1150°C.
[0009] Furthermore, in the step 1), the components of the nickel-based high-temperature alloy blank are, by mass percentage, C 0.01-2.25%, Cr 15.50-25.00%, Co 0.10-8.50%, W 0.01-5.00%, Mo 5.00-13.00%, Al 0-1.00%, Ti 0-0.5%, Fe 12.00-22.00%, B 0-1.00%, Mn 0-1.00%, Si≤1.00%, P≤1.00%, S≤0.50%, Cu≤1.00%, La≤0.05%, and the balance is Ni.
[0010] Furthermore, in the step 1), heating and heat preservation of the nickel-based high-temperature alloy blank comprises:
[0011] Place the nickel-based high-temperature alloy billet in a heating furnace, heat the heating furnace to 860-910°C, and keep it warm for 100-130 minutes; continue to heat it to 1130-1150°C, and keep it warm for 130-150 minutes.
[0012] Furthermore, in the step 1), the upsetting and punching is performed in four passes, and the total deformation of the four passes is ≥40%.
[0013] Furthermore, in the step 1), a ring rolling machine is used for ring rolling, and the rolling amount of each round is ≥30%.
[0014] Furthermore, in the step 2), the heat preservation treatment time is 30 to 50 minutes.
[0015] Furthermore, in the step 2), the double-fire forging is single-pass forging or multi-pass forging;
[0016] Among them, the deformation of a single forging pass is 30% to 50%;
[0017] The deformation amount of each pass in the multi-pass forging is 15% to 25%; and the total deformation amount of the multi-pass forging is 50% to 70%.
[0018] Furthermore, in the step 2), the temperature of the solution treatment is 1170-1200° C., and the time of the solution treatment is 20 min-60 min.
[0019] The present invention also provides a nickel-based high-temperature alloy ring part, wherein the average grain size of the nickel-based high-temperature alloy ring part is 7 to 8 levels.
[0020] Furthermore, the nickel-based high-temperature alloy ring has a yield strength of ≥230 MPa, a tensile strength of ≥350 MPa, and an elongation of ≥65%;
[0021] Preferably, the nickel-based high-temperature alloy ring is obtained by any of the forging methods described above.
[0022] Compared with the prior art, the present invention has at least the following beneficial effects:
[0023] 1. The present invention provides a forging method for a nickel-based high-temperature alloy ring. The rare earth La element is added to a nickel-based high-temperature alloy blank. The rare earth La is easily segregated on the grain boundary, and La inhibits the migration of the grain boundary, thereby limiting the formation and growth rate of the crystal nucleus during the recrystallization process, that is, La has a strong solid solution drag effect on the recrystallization, and increases the recrystallization temperature, thereby refining the deformation recrystallization grain size, and then making the distribution of carbides more uniform, avoiding cracks caused by carbide agglomeration, and improving the mixed crystal structure caused by carbides; at the same time, the processing window can be expanded after the rare earth is added, that is, the forging temperature can be increased while avoiding the formation of cracks, so that the degree of grain refinement is improved, thereby improving the mechanical properties of the nickel-based high-temperature alloy ring.
[0024] 2. Furthermore, the present invention provides a nickel-based high-temperature alloy ring part. The nickel-based high-temperature alloy ring part with an average grain size of 7 to 8 and no mixed crystal phenomenon is obtained by the above method, which solves the problems of uneven structure, coarse grains, carbide clusters aggravating crack initiation, etc. of the existing nickel-based high-temperature alloy ring parts, and significantly improves the high-temperature tensile properties of nickel-based high-temperature alloy forgings. In industry, higher quality nickel-based high-temperature alloy ring parts products are provided. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] In order to more clearly illustrate the implementation methods of the present invention or the technical solutions in the prior art, the following briefly introduces the drawings required for the implementation methods or the description of the prior art. The drawings described below are only exemplary, and for ordinary technicians in this field, other implementation drawings can be derived from the provided drawings without creative work.
[0026] Figure 1 The microstructure diagram of the ring-shaped part obtained by the forging method in Example 1 of the present invention;
[0027] Figure 2 The microstructure diagram of the ring part obtained by the forging method in Example 2 of the present invention;
[0028] Figure 3 The microstructure diagram of the ring part obtained by the forging method in Example 3 of the present invention;
[0029] Figure 4 The microstructure diagram of the ring part obtained by the forging method in Example 4 of the present invention;
[0030] Figure 5This is a microstructure diagram of the ring obtained by the forging method in Comparative Example 1 of the present invention;
[0031] Figure 6 This is a microstructure diagram of a ring obtained by the forging method in Comparative Example 2 of the present invention;
[0032] Figure 7 This is a microstructure diagram of a ring obtained by the forging method in Comparative Example 3 of the present invention;
[0033] Figure 8 This is a microstructure diagram of the ring part obtained by the forging method in Comparative Example 4 of the present invention. DETAILED DESCRIPTION
[0034] In order to more clearly illustrate the implementation methods of the present invention or the technical solutions in the prior art, the following briefly introduces the drawings required for the implementation methods or the description of the prior art. The drawings described below are only exemplary, and for ordinary technicians in this field, other implementation drawings can be derived from the provided drawings without creative work.
[0035] The present invention provides a forging method for a nickel-based high-temperature alloy ring, comprising the following steps:
[0036] Step 1) heating and heat preservation of a nickel-based high-temperature alloy blank, and then upsetting, punching, and ring rolling are performed in sequence to obtain a ring blank; wherein the nickel-based high-temperature alloy blank contains La element;
[0037] Step 2) performing double-fire forging on the ring blank, performing solid solution treatment after heat preservation treatment, and obtaining a nickel-based high-temperature alloy ring part after cooling; wherein the temperature of the double-fire forging is 1130-1150°C.
[0038] Based on the above method, the purpose of heating and heat preservation in one fire is to make the nickel-based high-temperature alloy billet heated evenly, give time for the structure transformation, soften the billet, reduce the deformation resistance, and increase the forging temperature to increase the operable time during the forging process; after the second fire forging and heat preservation, the ring billet material undergoes more complete recrystallization, making the material easier to deform. The reason for adding a heat preservation in the middle is that the temperature of the first fire is low and the processable temperature range is narrow. In order to prevent the temperature from being lower than the initial forging temperature during the forging process, it is heated and kept again. A wide processable window can reduce the number of forging fires and improve production efficiency. By adding the rare earth La element to the nickel-based high-temperature alloy billet, the rare earth La is easily segregated on the grain boundary, and La inhibits the migration of the grain boundary, thereby limiting the formation and growth rate of the crystal nucleus during the recrystallization process, that is, La has a strong solid solution drag effect on recrystallization, delays recrystallization, and increases the recrystallization temperature, thereby refining the deformation recrystallization grain size, and then making the carbide precipitation phase finer and more dispersed, and the distribution of carbides more uniform, avoiding cracks caused by carbide agglomeration, and improving the mixed crystal structure caused by carbides; at the same time, due to the pinning of the rare earth La on the grain boundary, and the reduction and uniform distribution of the carbide size, the growth of the grains is hindered, thereby obtaining a higher forging temperature, and a higher forging temperature can promote the uniform distribution of elements, make the grain size more uniform, which is conducive to the formation of a more uniform and finer grain structure. In addition, the increase in forging temperature is beneficial to the plasticity of the alloy, improves the ductility of the alloy during the forging process, makes it easier to form, speeds up the forging process, and improves forging efficiency and productivity; high-temperature forging can reduce defects such as pores and segregation, thereby obtaining higher-quality nickel-based high-temperature alloy rings. That is, rare earth addition + high-temperature forging can obtain nickel-based high-temperature rings with more uniform grain distribution and finer grains, thereby improving the mechanical properties of nickel-based high-temperature alloy rings;
[0039] Among them, after rare earth elements are added, they are equivalent to solute elements, and their solubility is extremely low. The grain boundary structure is looser than that in the grain, which makes the distortion energy different. Or due to the existence of vacancies, the energy of solute atoms in the crystal is higher than that in the grain boundary, so the solute atoms tend to spontaneously concentrate on the grain boundary, that is, the rare earth element La tends to be segregated on the grain boundary. After rare earth addition, the processing window is expanded, the number of forgings can be reduced, and the production efficiency can be improved.
[0040] In some embodiments, in step 1), the components of the nickel-based high-temperature alloy blank are, by mass percentage, C0.01-2.25%, Cr15.50-25.00%, Co0.10-8.50%, W0.01-5.00%, Mo5.00-13.00%, Al0-1.00%, Ti0-0.5%, Fe12.00-22.00%, B0-1.00%, Mn0-1.00%, Si≤1.00%, P≤1.00%, S≤0.50%, Cu≤1.00%, La≤0.05%, and the balance is Ni. The rare earth La element content needs to be controlled within the range of 0.5%, otherwise it is not conducive to the oxidation resistance of the alloy.
[0041] In some embodiments, in step 1), heating and heat preservation of the nickel-based high-temperature alloy blank comprises:
[0042] Place the nickel-based high-temperature alloy billet in a heating furnace, heat the heating furnace to 860-910°C, and keep it warm for 100-130 minutes; continue to heat it to 1130-1150°C, and keep it warm for 130-150 minutes.
[0043] In some embodiments, in step 1), the upsetting and punching is performed in four passes, and the total deformation of the four passes is ≥40%.
[0044] In some embodiments, in step 1), a ring rolling mill is used for ring rolling, and the rolling amount of each round is ≥30%.
[0045] In some embodiments, in step 2), the insulation treatment time is 30 to 50 minutes.
[0046] In some embodiments, in step 2), the double-fire forging is single-pass forging or multi-pass forging;
[0047] Among them, the deformation of a single forging pass is 30% to 50%;
[0048] The deformation of each pass in multi-pass forging is 15% to 25%; and the total deformation of multi-pass forging is 50% to 70%. A large cumulative deformation in one forging may cause insufficient equipment tonnage or alloy cracking. In this case, multi-pass forging can be used to solve the crack problem.
[0049] In some embodiments, in step 2), the temperature of the solution treatment is 1170-1200° C., and the time of the solution treatment is 20 min-60 min.
[0050] The present invention also provides a nickel-based high-temperature ring part. The average grain size of the nickel-based high-temperature alloy ring part is 7-8 levels.
[0051] In some embodiments, the yield strength of the ring is ≥230 MPa, the tensile strength is ≥350 MPa, and the elongation is ≥65%;
[0052] Preferably, the nickel-based high-temperature alloy ring is obtained by any of the forging methods mentioned above.
[0053] The present invention is further described below in conjunction with specific embodiments.
[0054] Example 1
[0055] The present embodiment provides a forging method for a nickel-based high-temperature alloy ring, wherein the components of the nickel-based high-temperature alloy blank used are, by mass percentage, C1.25%, Cr20.00%, Co5.50%, W3.00%, Mo8.00%, Al0.5%, Ti0.5%, Fe15.00%, B0.5%, Mn0.5%, Si0.5%, P0.5%, S0.2%, Cu0.5%, La0.025%, and the balance is Ni; the blank size is
[0056] The specific steps include:
[0057] Step 1) placing the nickel-based high-temperature alloy billet in a heating furnace for one-fire heating and heat preservation, wherein the heating furnace is heated to 890° C., kept warm for 100 minutes, and then further heated to 1130° C., kept warm for 130 minutes, and then placed in a fast forging machine for punching to obtain a semi-finished ring part, wherein the punching is four-pass forging, and the total deformation is 40%; then the semi-finished ring part is rolled, and the rolling amount of each fire is 30% to obtain a ring billet;
[0058] Step 2) The obtained ring blank is placed in a double-fire forging process, the double-fire forging temperature is 1130°C, the double-fire forging is a single forging process, the deformation amount is 40%, and then the ring blank is heat-treated for 30 minutes, and then the temperature is raised to 1180°C for solution treatment, the solution treatment time is 50 minutes, and the nickel-based high-temperature alloy ring is obtained after air cooling.
[0059] The microstructure of the nickel-based high-temperature alloy ring prepared in this embodiment is as follows: Figure 1 As shown, the average grain size of the ring part is level 8. After the ring part is pickled and polished, the mechanical properties are tested. The results are shown in Table 1. It can be seen that the yield strength is 240 MPa, the tensile strength is 350 MPa, and the elongation is 78%.
[0060] Example 2
[0061] The present embodiment provides a forging method for a nickel-based high-temperature alloy ring, wherein the components of the nickel-based high-temperature alloy blank used are, by mass percentage, C1.25%, Cr20.00%, Co5.50%, W3.00%, Mo8.00%, Al0.5%, Ti0.5%, Fe15.00%, B0.5%, Mn0.5%, Si0.5%, P0.5%, S0.2%, Cu0.5%, La0.025%, and the balance is Ni; the blank size is
[0062] The specific steps include:
[0063] Step 1) placing the nickel-based high-temperature alloy billet in a heating furnace for one-fire heating and heat preservation, wherein the heating furnace is heated to 890° C., kept warm for 100 minutes, and then further heated to 1150° C., kept warm for 130 minutes, and then placed in a fast forging machine for punching to obtain a semi-finished ring part, wherein the punching is four-pass forging, and the total deformation is 40%; then the semi-finished ring part is rolled, and the rolling amount of each fire is 30% to obtain a ring billet;
[0064] Step 2) The obtained ring blank is placed in a double-fire forging process, the double-fire forging temperature is 1150°C, the double-fire forging is a single forging process, the deformation amount is 50%, and then the ring blank is heat-treated for 30 minutes, and then the temperature is raised to 1180°C for solution treatment, the solution treatment time is 50 minutes, and the nickel-based high-temperature alloy ring is obtained after air cooling after being taken out of the furnace.
[0065] The microstructure of the nickel-based high-temperature alloy ring prepared in this embodiment is as follows: Figure 2 As shown, the average grain size of the ring part is level 8. After the ring part is pickled and polished, the mechanical properties are tested. The results are shown in Table 1. It can be seen that the yield strength is 230 MPa, the tensile strength is 450 MPa, and the elongation is 88%.
[0066] Example 3
[0067] The present embodiment provides a forging method for a nickel-based high-temperature alloy ring, wherein the components of the nickel-based high-temperature alloy blank used are, by mass percentage, C1.25%, Cr20.00%, Co5.50%, W3.00%, Mo8.00%, Al0.5%, Ti0.5%, Fe15.00%, B0.5%, Mn0.5%, Si0.5%, P0.5%, S0.2%, Cu0.5%, La0.03%, and the balance is Ni; the blank size is
[0068] The specific steps include:
[0069] Step 1) placing the nickel-based high-temperature alloy billet in a heating furnace for one-fire heating and heat preservation, wherein the heating furnace is heated to 890° C., kept warm for 100 minutes, and then further heated to 1130° C., kept warm for 130 minutes, and then placed in a fast forging machine for punching to obtain a semi-finished ring part, wherein the punching is four-pass forging, and the total deformation is 40%; then the semi-finished ring part is rolled, and the rolling amount of each fire is 30% to obtain a ring billet;
[0070] Step 2) The obtained ring blank is placed in a two-fire forging process, the two-fire forging temperature is 1130° C., the two-fire forging process is four-pass forging, the deformation amount of each pass is 15.5%, and the total deformation amount of the four-pass forging is 62%. Each pass is heat-insulated for 30 minutes, and then the temperature is raised to 1180° C. for solution treatment. The solution treatment time is 50 minutes. After being taken out of the furnace and air-cooled, a nickel-based high-temperature alloy ring is obtained.
[0071] The microstructure of the nickel-based high-temperature alloy ring prepared in this embodiment is as follows: Figure 3 As shown, the average grain size of the ring part is level 8. After the ring part is pickled and polished, the mechanical properties are tested. The results are shown in Table 1. It can be seen that the yield strength is 237 MPa, the tensile strength is 390 MPa, and the elongation is 70%.
[0072] Example 4
[0073] The present embodiment provides a forging method for a nickel-based high-temperature alloy ring, wherein the components of the nickel-based high-temperature alloy blank used are, by mass percentage, C1.25%, Cr20.00%, Co5.50%, W3.00%, Mo8.00%, Al0.5%, Ti0.5%, Fe15.00%, B0.5%, Mn0.5%, Si0.5%, P0.5%, S0.2%, Cu0.5%, La0.03%, and the balance is Ni; the blank size is
[0074] The specific steps include:
[0075] Step 1) placing the nickel-based high-temperature alloy billet in a heating furnace for one-fire heating and heat preservation, wherein the heating furnace is heated to 890° C., kept warm for 100 minutes, and then further heated to 1150° C., kept warm for 130 minutes, and then placed in a fast forging machine for punching to obtain a semi-finished ring part, wherein the punching is four-pass forging, and the total deformation is 40%; then the semi-finished ring part is rolled, and the rolling amount of each fire is 30% to obtain a ring billet;
[0076] Step 2) The obtained ring blank is placed in a two-fire forging process, the two-fire forging temperature is 1150° C., the two-fire forging process is four-pass forging, the deformation amount of each pass is 15.5%, and the total deformation amount of the four-pass forging is 62%. Each pass is heat-insulated for 30 minutes, and then the temperature is raised to 1180° C. for solution treatment. The solution treatment time is 50 minutes. After being taken out of the furnace and air-cooled, a nickel-based high-temperature alloy ring is obtained.
[0077] The microstructure of the nickel-based high-temperature alloy ring prepared in this embodiment is as follows: Figure 4 As shown, the average grain size of the ring part is level 7. After the ring part is pickled and polished, the mechanical properties are tested. The results are shown in Table 1. It can be seen that the yield strength is 238 MPa, the tensile strength is 400 MPa, and the elongation is 77%.
[0078] Comparative Example 1
[0079] The comparative example provides a forging method for a nickel-based high-temperature alloy ring, wherein the components of the nickel-based high-temperature alloy blank used are as follows by mass percentage: C1.25%, Cr20.00%, Co5.50%, W3.00%, Mo8.00%, Al0.5%, Ti0.5%, Fe15.00%, B0.5%, Mn0.5%, Si0.5%, P0.5%, S0.2%, Cu0.5%, and the balance is Ni; the blank size is
[0080] The specific steps include:
[0081] Step 1) placing the nickel-based high-temperature alloy billet in a heating furnace for one-fire heating and heat preservation, wherein the heating furnace is heated to 890° C., kept warm for 100 minutes, and then further heated to 1110° C., kept warm for 130 minutes, and then placed in a fast forging machine for punching to obtain a semi-finished ring part, wherein the punching is four-pass forging, and the total deformation is 40%; then the semi-finished ring part is rolled, and the rolling amount of each fire is 30% to obtain a ring billet;
[0082] Step 2) The obtained ring blank is placed in a heating and heat preservation process, heated to 950°C for two times, and kept warm for 50 minutes, and then forged and heated for three times. The heating temperature of the three-fire forging is 1130°C, and the three-fire forging is a forging process. The deformation amount is 40%, and then the ring blank is heat-treated for 30 minutes, and then heated to 1180°C for solution treatment. The solution treatment time is 50 minutes. After being taken out of the furnace and air-cooled, a nickel-based high-temperature alloy ring is obtained.
[0083] This comparative example uses the traditional forging method to forge the ring. Since La element is not added to the blank, the first heating temperature is low and the processing window is narrow. In order to prevent the temperature from being lower than the initial forging temperature during the forging process and affecting the forging effect, a heating and heat preservation step is added before forging. The microstructure of the nickel-based high-temperature alloy ring prepared in this comparative example is shown in FIG. Figure 5 As shown in the figure, the grains are coarse, the grain size can only reach level 4, there is obvious mixed crystal phenomenon, and the surface is rough; there is obvious carbide cluster phenomenon in the organization; after pickling and polishing the ring, the mechanical properties are tested. The results are shown in Table 1. It can be seen that the yield strength is 200MPa, the tensile strength is 330MPa, and the elongation is 44%. This is because the La element is not added, there is a lack of fine dispersed precipitation phases to pin the grain boundaries, it is difficult to limit the migration speed of the grain boundaries, and the grains are coarse and uneven; the forging temperature and holding time are low, and the degree of grain refinement is low; the initial forging temperature is low, cracks are easy to occur during the forging process, and no effective solution treatment is carried out. The carbides form agglomerations, which promote crack propagation, and the performance of the ring is far from meeting the production requirements.
[0084] Comparative Example 2
[0085] This comparative example provides a forging method for a nickel-based high-temperature alloy ring, wherein the components of the nickel-based high-temperature alloy blank used are the same as those in Example 1, that is, calculated by mass percentage: C1.25%, Cr20.00%, Co5.50%, W3.00%, Mo8.00%, Al0.5%, Ti0.5%, Fe15.00%, B0.5%, Mn0.5%, Si0.5%, P0.5%, S0.2%, Cu0.5%, La0.025%, and the balance is Ni; the blank size is φ210mm*500mm;
[0086] The specific steps include:
[0087] Step 1) placing the nickel-based high-temperature alloy billet in a heating furnace for one-fire heating and heat preservation, wherein the heating furnace is heated to 890° C., kept warm for 100 minutes, and then further heated to 1130° C., kept warm for 130 minutes, and then placed in a fast forging machine for punching to obtain a semi-finished ring part, wherein the punching is four-pass forging, and the total deformation is 40%; then the semi-finished ring part is rolled, and the rolling amount of each fire is 30% to obtain a ring billet;
[0088] Step 2) The obtained ring blank is placed in a double-fire forging process, the double-fire forging temperature is 1110°C, the double-fire forging is a single forging process, the deformation amount is 40%, and then the ring blank is heat-treated for 30 minutes, and then the temperature is raised to 1180°C for solution treatment, the solution treatment time is 50 minutes, and the nickel-based high-temperature alloy ring is obtained after being air-cooled out of the furnace.
[0089] In this comparative example, the ring is forged by a conventional forging method. The microstructure of the prepared nickel-based high-temperature alloy ring is as follows: Figure 6 As shown in the figure, the grains are coarse and the grain size can only reach level 5. After pickling and polishing, the ring is tested for mechanical properties. The results are shown in Table 1. It can be seen that the yield strength is 220MPa, the tensile strength is 360MPa, and the elongation is 62%. This is because the addition of La element can pin the grain boundary and limit the migration speed of the grain boundary, thereby increasing the recrystallization temperature. However, the forging temperature is low, the recrystallization is insufficient, and therefore the degree of grain refinement is low.
[0090] Comparative Example 3
[0091] This comparative example provides a forging method for a nickel-based high-temperature alloy ring, wherein the components of the nickel-based high-temperature alloy blank used are, by mass percentage, C1.25%, Cr20.00%, Co5.50%, W3.00%, Mo8.00%, Al0.5%, Ti0.5%, Fe15.00%, B0.5%, Mn0.5%, Si0.5%, P0.5%, S0.2%, Cu0.5%, and the balance is Ni; the blank size is φ210mm*500mm;
[0092] The specific steps include:
[0093] Step 1) placing the nickel-based high-temperature alloy billet in a heating furnace for one-fire heating and heat preservation, wherein the heating furnace is heated to 890° C., kept warm for 100 minutes, and then further heated to 1130° C., kept warm for 130 minutes, and then placed in a fast forging machine for punching to obtain a semi-finished ring part, wherein the punching is four-pass forging, and the total deformation is 40%; then the semi-finished ring part is rolled, and the rolling amount of each fire is 30% to obtain a ring billet;
[0094] Step 2) The obtained ring blank is placed in a double-fire forging process, the double-fire forging temperature is 1130°C, the double-fire forging is a single forging process, the deformation amount is 40%, and then the ring blank is heat-treated for 30 minutes, and then the temperature is raised to 1180°C for solution treatment, the solution treatment time is 50 minutes, and the nickel-based high-temperature alloy ring is obtained after air cooling.
[0095] The microstructure of the nickel-based high-temperature alloy ring prepared in this comparative example is as follows: Figure 7 As shown in the figure, the grains are coarse, the grain size can only reach level 5, there is an obvious mixed crystal phenomenon, and the surface is rough; after pickling and polishing the ring, the mechanical properties are tested. The results are shown in Table 1. It can be seen that the yield strength is 210MPa, the tensile strength is 340MPa, and the elongation is 50%. This is because the La element is not added, there is a lack of fine dispersed precipitation phases to pin the grain boundaries, it is difficult to limit the migration speed of the grain boundaries, and the grains are coarse and uneven.
[0096] Comparative Example 4
[0097] This comparative example provides a forging method for a nickel-based high-temperature alloy ring, wherein the components of the nickel-based high-temperature alloy blank used are as follows by mass percentage: C1.25%, Cr20.00%, Co5.50%, W3.00%, Mo8.00%, Al0.5%, Ti0.5%, Fe15.00%, B0.5%, Mn0.5%, Si0.5%, P0.5%, S0.2%, Cu0.5%, La0.03%, and the balance is Ni; the blank size is φ210mm*500mm;
[0098] The specific steps include:
[0099] Step 1) placing the nickel-based high-temperature alloy billet in a heating furnace for one-fire heating and heat preservation, wherein the heating furnace is heated to 890° C., kept warm for 100 minutes, and then further heated to 1130° C., kept warm for 130 minutes, and then placed in a fast forging machine for punching to obtain a semi-finished ring part, wherein the punching is four-pass forging, and the total deformation is 40%; then the semi-finished ring part is rolled, and the rolling amount of each fire is 30% to obtain a ring billet;
[0100] Step 2) The obtained ring blank is placed in a double-fire forging process, the double-fire forging temperature is 1170°C, the double-fire forging is a single forging process, the deformation amount is 40%, and then the ring blank is heat-treated for 30 minutes, and then the temperature is raised to 1180°C for solution treatment, the solution treatment time is 50 minutes, and the nickel-based high-temperature alloy ring is obtained after being air-cooled out of the furnace.
[0101] The microstructure of the nickel-based high-temperature alloy ring prepared in this comparative example is as follows: Figure 8 As shown in the figure, the grains are coarse and the grain size can only reach level 5; after pickling and polishing the ring parts, the mechanical properties are tested. The results are shown in Table 1. It can be seen that the yield strength is 215MPa, the tensile strength is 340MPa, and the elongation is 55%. Although La can limit the growth of grains, the temperature cannot be too high. Since the forging temperature is much higher than the recrystallization temperature, the grains will resume growth, the grains cannot reach the optimal degree of refinement, and the grains will coarsen, thus affecting the material properties.
[0102] Table 1 Mechanical properties test results of nickel-based high-temperature alloy rings of the embodiments of the present invention and the comparative examples
[0103] Implementation Yield strength MPa Tensile strength MPa Elongation % Example 1 240 350 78 Example 2 230 450 88 Example 3 237 390 70 Example 4 238 400 77 Comparative Example 1 200 330 44 Comparative Example 2 220 360 62 Comparative Example 3 210 340 50 Comparative Example 4 215 340 55
[0104] It can be seen from the accompanying drawings and Table 1 that by adding rare earth elements and strictly controlling the forging temperature, the problems of uneven structure of nickel-based high-temperature alloy ring parts, the presence of coarse grains, and carbide clusters that aggravate crack initiation are solved, and the mechanical properties of nickel-based high-temperature alloy forgings are significantly improved. In industry, higher quality nickel-based high-temperature alloy ring parts products are provided.
[0105] It is easy for those skilled in the art to understand that, without conflict, the advantageous technical features of the above-mentioned methods can be freely combined and superimposed.
[0106] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principle of the present invention shall be included in the protection scope of the present invention. The above description is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and variations can be made without departing from the technical principles of the present invention. These improvements and variations should also be regarded as the protection scope of the present invention.
Claims
1. A forging method for a nickel-based high-temperature alloy ring. It is characterized in that The following steps are involved: Step 1) heating and heat preservation of a nickel-based high-temperature alloy blank, and then upsetting, punching, and ring rolling in sequence to obtain a ring blank; wherein the nickel-based high-temperature alloy blank contains La element; Step 2) performing double-forging on the ring blank, performing solid solution treatment after heat preservation treatment, and obtaining the nickel-based high-temperature alloy ring part after cooling; wherein the temperature of the double-forging is 1130-1150°C.
2. The forging method of the nickel-based high-temperature alloy ring according to claim 1, It is characterized in that In the step 1), the components of the nickel-based high-temperature alloy blank are, by mass percentage, C 0.01-2.25%, Cr 15.50-25.00%, Co 0.10-8.50%, W 0.01-5.00%, Mo 5.00-13.00%, Al 0-1.00%, Ti 0-0.5%, Fe 12.00-22.00%, B 0-1.00%, Mn 0-1.00%, Si≤1.00%, P≤1.00%, S≤0.50%, Cu≤1.00%, La≤0.05%, and the balance is Ni.
3. The forging method of the nickel-based high-temperature alloy ring according to claim 1 or 2, It is characterized in that In the step 1), heating and heat preservation of the nickel-based high-temperature alloy blank comprises: Place the nickel-based high-temperature alloy billet in a heating furnace, heat the heating furnace to 860-910°C, and keep it warm for 100-130 minutes; continue to heat it to 1130-1150°C, and keep it warm for 130-150 minutes.
4. The forging method of the nickel-based high-temperature alloy ring according to claim 1, It is characterized in that In the step 1), the upsetting and punching is performed in four passes, and the total deformation of the four passes is ≥40%.
5. The forging method of the nickel-based high-temperature alloy ring according to claim 1, It is characterized in that In the step 1), a ring rolling machine is used to roll the rings, and the rolling amount of each round is ≥30%.
6. The forging method of the nickel-based high-temperature alloy ring according to claim 1, It is characterized in that In the step 2), the heat preservation treatment time is 30 to 50 minutes.
7. The forging method of the nickel-based high-temperature alloy ring according to claim 6, It is characterized in that In the step 2), the double-fire forging is single-pass forging or multi-pass forging; Among them, the deformation of a single forging pass is 30% to 50%; The deformation amount of each pass in the multi-pass forging is 15% to 25%; and the total deformation amount of the multi-pass forging is 50% to 70%.
8. The forging method of the nickel-based high-temperature alloy ring according to claim 1, It is characterized in that In the step 2), the temperature of the solution treatment is 1170-1200° C., and the time of the solution treatment is 20 min-60 min.
9. A nickel-based high-temperature alloy ring, It is characterized in that The average grain size of the nickel-based high-temperature alloy ring is 7-8.
10. The nickel-based high-temperature alloy ring according to claim 9, It is characterized in that The nickel-based high-temperature alloy ring has a yield strength of ≥230MPa, a tensile strength of ≥350MPa, and an elongation of ≥65%; Preferably, the nickel-based high-temperature alloy ring is obtained by the forging method described in any one of claims 1 to 8.
Citation Information
Patent Citations
Nickel-based superalloy plate and preparation method thereof
CN110983111A
Nickel-based plate and preparation method therefor
CN112553505A
High-temperature high-resistance nickel-based alloy and preparation method thereof
CN115717205A
Heat-resistant forged nickel-based alloy and product thereof
CN115768911A
Nickel-based heat-resistant wrought alloy and article made from same
WO2021246908A1