Automatic control method for continuous casting argon blowing
Through a computer program, the continuous casting argon blowing flow rate is controlled in real time according to the pulling speed, and the problem of insufficient or excessive artificial adjustment of argon in the prior art is solved, and the stability of the continuous casting billet and the reduction of labor intensity of the operator is achieved.
Patent Information
- Application Number
- CN202411084579.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-08
- Publication Date
- 2024-11-19
AI Technical Summary
The existing continuous casting and argon blowing technology requires manual frequent adjustment of the argon flow, which leads to timely impacting the quality of the continuous casting billet. Insufficient or excessive argon blowing will affect the quality of the molten steel, increasing the labor intensity of the operator.
The computer program controls the flow of argon gas, argon gas at the plug rod and the plate in real time according to the pulling speed size, sets the argon gas flow range corresponding to different pulling speeds, and adjusts the argon gas flow through the pulling speed coefficient and width coefficient.
The precision and stability of continuous casting and argon blowing is achieved, reducing the inclusion defects and waste loss of hot coils after rolling, and reducing the labor intensity of operators.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of steelmaking continuous casting and relates to an automatic control method for continuous casting argon blowing. Background Art
[0002] The existing continuous casting billet production includes the following steps: the molten steel smelted in the converter is poured into the ladle, and after being processed in the refining process, it is transported to the continuous casting steel pouring platform. The molten steel flows from the ladle into the tundish, and then flows into the crystallizer through the tundish water inlet, and is cooled in the crystallizer and the continuous casting secondary cooling zone to form a continuous casting slab. In this process, argon is blown into the inner hole of the tundish stopper rod and the upper water inlet to avoid blockage of the upper and lower water inlets of the tundish, and at the same time promote the floating of inclusions in the crystallizer. In addition, argon is blown between the upper and lower water inlet slides to avoid air inhalation between the plates.
[0003] The above-mentioned continuous casting argon blowing has a great influence on the quality of the continuous casting billet. A small amount of argon blowing is not conducive to the floating of inclusions in the molten steel in the crystallizer, and may also cause secondary oxidation of the molten steel due to air inhalation; a large amount of argon blowing will cause the molten steel in the crystallizer to roll over, and the protective slag will be drawn into the billet. Therefore, it is necessary to reduce the argon when the liquid level rolls over, reduce the argon when starting the machine and changing the water port, and then gradually increase the argon flow rate after the casting is normal. Since the argon flow rate needs to be adjusted frequently and manually during the production process, there is a lot of repetitive work, which increases the labor intensity of the operators. In addition, if the flow rate is not adjusted in time, it will also affect the quality of the continuous casting billet. Summary of the invention
[0004] In view of this, an object of the present invention is to provide an automatic control method for continuous casting argon blowing to solve the technical problems existing in the background technology.
[0005] In order to achieve the above object, the present invention provides the following technical solutions:
[0006] The invention discloses an automatic control method for continuous casting argon blowing, which controls the flow of stopper argon, upper nozzle argon and inter-plate argon according to the casting speed, and controls the flow of stopper argon, upper nozzle argon and inter-plate argon in real time through a computer program.
[0007] Optionally, when the pulling speed is less than 0.80 m / min, the flow rate of the stopper argon gas and the upper water inlet argon gas is 1-2 L / min;
[0008] When the pulling speed is 0.80m / min≤<0.90m / min, the flow rate of argon gas for the stopper rod and the upper water inlet is 3-4L / min;
[0009] When the pulling speed is 0.90m / min, the flow rate of argon gas at the stopper rod and the upper water inlet is 4-5L / min;
[0010] When the casting speed is greater than 0.90 m / min, the stopper argon flow rate = standard flow rate × casting speed coefficient × width coefficient, and the upper water inlet argon flow rate is 4-6 L / min; wherein, the casting speed coefficient = 1 + (actual casting speed - average value of maximum casting speed and minimum casting speed) / average value of maximum casting speed and minimum casting speed, and the width coefficient = 1 + (actual width - average value of maximum width and minimum width of the ingot) / average value of maximum width and minimum width of the ingot;
[0011] The argon gas between the plates is controlled at 8-12 L / min and set to a fixed value.
[0012] Optionally, the standard flow rate is set at 9-10 L / min.
[0013] The beneficial effects of the present invention are: the continuous casting argon blowing is accurate and stable, the hot coil inclusion defects after the continuous casting billet is rolled are reduced, the scrap loss is reduced, and the labor intensity of the operators is reduced.
[0014] Other advantages, objectives and features of the present invention will be described in the following description to some extent, and to some extent, will be obvious to those skilled in the art based on the following examination and study, or can be taught from the practice of the present invention. The objectives and other advantages of the present invention can be realized and obtained through the following description. DETAILED DESCRIPTION
[0015] The following describes the embodiments of the present invention through specific examples, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention.
[0016] The invention discloses an automatic control method for continuous casting argon blowing, which controls the flow of stopper argon, upper nozzle argon and inter-plate argon according to the casting speed, and controls the flow of stopper argon, upper nozzle argon and inter-plate argon in real time through a computer program.
[0017] Specifically: when the pulling speed is less than 0.80m / min, the flow rate of argon gas at the stopper rod and the upper water inlet is 1-2L / min;
[0018] When the pulling speed is 0.80m / min≤<0.90m / min, the flow rate of argon gas for the stopper rod and the upper water inlet is 3-4L / min;
[0019] When the pulling speed is 0.90m / min, the flow rate of argon gas at the stopper rod and the upper water inlet is 4-5L / min;
[0020] When the pulling speed is greater than 0.90 m / min, the stopper argon flow rate = standard flow rate × pulling speed coefficient × width coefficient, and the upper water inlet argon flow rate is 4-6 L / min; wherein, the standard flow rate is set at 9-10 L / min, and the pulling speed coefficient is calculated based on the difference between the actual pulling speed and the maximum pulling speed, the minimum pulling speed, the maximum pulling speed coefficient, and the minimum pulling speed coefficient, wherein the maximum pulling speed corresponds to the maximum pulling speed coefficient, and the minimum pulling speed corresponds to the minimum pulling speed coefficient, and the pulling speed coefficient = 1 + (actual pulling speed - the average value of the maximum pulling speed and the minimum pulling speed) / the average value of the maximum pulling speed and the minimum pulling speed; the width coefficient is calculated based on the difference between the actual pulling speed and the maximum width, the minimum width, the maximum width coefficient, and the minimum width coefficient, wherein the maximum width corresponds to the maximum width coefficient, and the minimum width corresponds to the minimum width coefficient, and the width coefficient = 1 + (actual width - the average value of the maximum width and the minimum width of the ingot) / the average value of the maximum width and the minimum width of the ingot;
[0021] The argon gas between the plates is controlled at 8-12 L / min and set to a fixed value.
[0022] The present invention controls the flow of stopper argon, upper water inlet argon, and inter-plate argon according to the drawing speed, and controls the flow of stopper argon, upper water inlet argon, and inter-plate argon in real time through a computer program, thereby achieving accurate and stable argon blowing, reducing hot coil inclusion defects after continuous casting billet rolling, reducing scrap losses, and stabilizing the quality of continuous casting billets. In addition, since the repetitive work of adjusting argon is automatically handled by a computer program, the labor intensity of the operator is reduced.
[0023] Example 1
[0024] Calculation of stopper argon flow rate when pulling speed>0.90m / min.
[0025] The maximum width of a steel plant's ingot casting is 1650mm, the minimum width is 1030mm, the maximum typical pulling speed is 1.40m / min under normal production conditions, and the minimum typical pulling speed is 0.90m / min. The standard flow rate for low-carbon and low-silicon steel is 10L / min, and the standard flow rate for other steels is 9L / min. The corresponding pulling speed is 1.15m / min (the average of the maximum and minimum pulling speeds), and the corresponding width is 1340mm (the average of the maximum and minimum sections).
[0026] Pulling speed coefficient = 1 + (actual pulling speed - 1.15) / 1.15
[0027] Width factor = 1 + (actual width - 1340) / 1340
[0028] For example, the argon flow rate of the stopper rod for 1530 cross-section low-carbon low-silicon steel at a pulling speed of 1.30m / min is:
[0029] Pulling speed coefficient = 1 + (1.30-1.15) / 1.15 = 1.13
[0030] Width factor = 1 + (1530-1340) / 1340 = 1.14
[0031] Stopper rod argon flow rate = standard flow rate × pulling speed coefficient × width coefficient = 10 × 1.13 × 1.14 = 12.9 (L / min).
[0032] Example 2
[0033] From September to December 2023, the hot coil inclusion defect rate of a steel plant reached 0.20%. After applying the continuous casting argon blowing automatic control method of the present invention, the hot coil inclusion defect rate was reduced to below 0.10% from January to February 2024.
[0034] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the purpose and scope of the technical solution, which should be included in the scope of the claims of the present invention.
Claims
1. A method for automatic control of argon blowing in continuous casting, characterized in that: The flow rates of argon gas at the stopper rod, argon gas at the water inlet and argon gas between the plates are controlled according to the drawing speed, and the flow rates of argon gas at the stopper rod, argon gas at the water inlet and argon gas between the plates are controlled in real time through a computer program.
2. The method for automatic control of argon blowing during continuous casting according to claim 1, characterized in that: When the pulling speed is less than 0.80m / min, the flow rate of argon gas at the stopper rod and the upper water inlet is 1-2L / min; When the pulling speed is 0.80m / min≤<0.90m / min, the flow rate of argon gas for the stopper rod and the upper water inlet is 3-4L / min; When the pulling speed is 0.90m / min, the flow rate of argon gas at the stopper rod and the upper water inlet is 4-5L / min; When the casting speed is greater than 0.90 m / min, the stopper argon flow rate = standard flow rate × casting speed coefficient × width coefficient, and the upper water inlet argon flow rate is 4-6 L / min; wherein, the casting speed coefficient = 1 + (actual casting speed - average value of maximum casting speed and minimum casting speed) / average value of maximum casting speed and minimum casting speed, and the width coefficient = 1 + (actual width - average value of maximum width and minimum width of the ingot) / average value of maximum width and minimum width of the ingot; The argon gas between the plates is controlled at 8-12 L / min and set to a fixed value.
3. The method for automatic control of argon blowing during continuous casting according to claim 2, characterized in that: The standard flow rate is set at 9-10L / min.
Citation Information
Cited By
Three-way argon flow control method for ultra-low carbon steel continuous casting tundish
CN120885652A
Continuous casting argon blowing dynamic control system and method
CN121156208A