Preparation method of silver-coated copper powder for HJT battery

By activating and sensitizing copper powder, combined with chemical reduction method, dropwise addition of silver ions and hydrophobic treatment, the problem of incomplete coating and empty shell of the silver-clad copper powder in the prior art is solved, and high-efficiency and low-cost silver-clad copper powder is achieved. Preparation improves the performance and production efficiency of HJT batteries.

CN118976905APending Publication Date: 2024-11-19ZHUHAI GREE NEW MATERIAL CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411088636.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-09
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

The preparation method of silver-clad copper powder in the prior art has problems such as the copper powder surface not being completely covered, the silver plating has low density and smoothness, some internal empty shells and complicated processes, resulting in high cost of HJT batteries and difficult to compete for PERC and TopCon battery.

Method used

By activating alkali and ammonium salt washing of copper powder, the silver ions are sensitized in the reducing metal ion solution. The silver ions are added dropwise by chemical reduction, combined with ultrasonic and mechanical stirring, ensuring smooth and dense coating of the silver layer and being hydrophobic treated and vacuum oven treatment to obtain finished silver-clad copper powder.

Benefits of technology

The complete activation of the copper powder surface layer and the smooth and dense coating of the silver layer are achieved, which avoids empty shell problems, simplifies the process flow, reduces costs, and improves the performance and application efficiency of silver-clad copper powder.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118976905A_ABST
    Figure CN118976905A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of silver-coated copper powder for an HJT battery. The preparation method comprises the following steps: activating copper powder; washing with ammonium salt; sensitizing copper powder: adding the copper powder into a metal ion solution with reducibility; transferring into an AgNO3 solution; chemical reduction method silver plating: adding a reducing agent solution, dropwise adding a silver ion plating solution, and carrying out a silver plating reaction; oleic acid and an oxidation film on the surface layer of the copper powder are thoroughly removed through alkali washing and an ammonium salt solution, and complete activation of the surface layer of the copper powder is achieved; and the activated copper powder is immersed in a reducing metal ion solution, it is ensured that the surface layer of the copper powder adsorbs reducing metal ions, and Ag < + > is reduced in an AgNO3 solution with the extremely low concentration and deposited on the surface of the copper powder. The sensitized silver not only serves as an initial mass point of silver plating, but also can catalyze a subsequent reduction reaction. Silver plating is carried out through a chemical reduction method instead of a replacement method, and a strategy of dropwise adding a plating solution at a high speed and then at a low speed is adopted, so that smoothness, compactness and complete coating of a silver plating layer are ensured, and the quality and the performance of the silver-coated copper powder are remarkably improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of silver-coated copper powder preparation, in particular to a method for preparing silver-coated copper powder for HJT batteries. Background Art

[0002] Photovoltaic power generation is mainly achieved with the help of crystalline silicon solar cells. PERC, TopCon and HJT are the mainstream battery technologies on the market. The photoelectric conversion efficiency of PERC cells is close to the theoretical efficiency limit, and the TopCon cell process is complex. In contrast, HJT cell technology has the advantages of high mass production efficiency, simple core process, and compatibility with BC cells and perovskite stacked cell technology. The core product in the future market must be HJT cells. However, HJT technology requires a greater amount of low-temperature silver paste, which makes the cost of HJT cells higher, resulting in the current stage. HJT cells are still difficult to resist the cost-effectiveness of PERC and TopCon cells. Therefore, under the premise of ensuring the mass production efficiency of HJT cells, how to reduce the cost of low-temperature silver paste is a difficult problem facing the photovoltaic industry.

[0003] Silver-coated copper powder is a material with a copper core coated with a silver layer. This special core-shell structure enables the silver-coated copper powder to maintain the excellent oxidation resistance and electrical conductivity of silver powder, while maintaining the excellent thermal conductivity of copper powder. The addition of copper powder can effectively inhibit the silver migration problem caused by the dissolution of silver at high temperatures. In addition, compared with silver powder, the price of silver-coated copper powder is much lower. Obviously, the silver-coated copper technology takes into account both performance and cost. Using silver-coated copper powder instead of silver powder is an effective way to reduce the cost of HJT batteries. However, the silver-coated copper powder synthesized by the prior art has the following four problems: (1) The surface of the copper powder is not completely coated with the silver layer; (2) The density and smoothness of the silver plating are low; (3) Some of the silver-coated copper powders are empty shells and have collapsed; (4) The process is complicated.

[0004] In the prior art, patent CN108080651A discloses a method for preparing a nano silver-coated copper material, and the core steps are as follows: (1) reducing a copper salt solution with a reducing agent solution having a neutral pH at 70-90°C; (2) adding a silver-ammonia complex solution to the system. The copper element produced in step (1) and the remaining reducing agent solution reduce the silver-ammonia solution, so that a layer of silver is plated on the surface of the copper element. The surface of the silver-coated copper powder synthesized by this method is rough and uneven, and the silver layer is not dense enough; patent CN116352083A discloses a method for synthesizing a cobalt-modified silver-coated copper powder material, and the core steps are as follows: (1) removing oxides on the surface of the copper powder by alkali washing; (2) using a chemical reduction method to reduce the cobalt salt complex solution with a sodium hypophosphite solution to obtain a cobalt-modified copper powder; (3) using a chemical reduction method to reduce the silver-ammonia complex solution with a glucose solution, and plating a layer of silver powder on the surface of the cobalt-modified copper powder to obtain a cobalt-modified silver-coated copper powder. The silver-coated copper powder synthesized by the method has excellent antioxidant properties, but the reliability of the double-coated powder obtained by plating cobalt on the surface of the copper powder and then plating silver on the surface of the cobalt needs to be investigated, and it is unknown whether the coating is easy to detach, and the introduction of metallic cobalt undoubtedly increases the cost, which is not conducive to production; Patent CN116949438A discloses a method for preparing silver-coated copper by a replacement method and a chemical reduction method, and the core steps are as follows: (1) using glucose and hydrazine hydrate as a composite reducing agent to reduce a copper salt solution to obtain copper powder; (2) using silver nitrate as a silver source, using a replacement method to replace the surface of the copper powder to obtain a silver-coated copper powder; (3) using a silver ammonia solution as a plating solution, tartaric acid and glucose as a composite reducing agent, and using a chemical reduction method to deposit silver on the surface of the pre-coated copper powder to obtain a silver-coated copper powder. The method has many experimental steps, and the replacement reaction in step (2) is difficult to control, which easily causes the interior of the copper powder to be replaced by silver ions and become an empty shell. Therefore, it is urgent to develop a low-cost, high-performance synthesis method for silver-coated copper powder to solve the above problems and enable silver-coated copper powder to be better used in HJT batteries. Summary of the invention

[0005] In order to overcome the above-mentioned shortcomings of the prior art, an object of the present invention is to provide a method for preparing silver-coated copper powder for HJT batteries.

[0006] The technical solution adopted by the present invention to solve the technical problem is: a method for preparing silver-coated copper powder for HJT battery, comprising the following steps:

[0007] (1) Activated copper powder: alkali washing; ammonium salt washing;

[0008] (2) Sensitized copper powder: copper powder is added to a reducing metal ion solution and transferred to an AgNO3 solution;

[0009] (3) Chemical reduction silver plating: Add reducing agent solution, add silver ion plating solution, and carry out silver plating reaction.

[0010] As a further improvement of the present invention: wherein the alkali washing in step (1) comprises the following steps:

[0011] Copper powder and sodium hydroxide solution are added to the batching kettle respectively, and the mixture is treated with ultrasound assistance for 5-15 minutes at 35-45° C. under mechanical stirring at 300-500 rpm. The alkali washing removes grease from the surface of the copper powder.

[0012] As a further improvement of the present invention: the amount of sodium hydroxide solution used is 1000-1200wt% of the amount of copper powder used; the concentration of the sodium hydroxide solution is 0.1-0.5mol / L.

[0013] As a further improvement of the present invention: wherein the ammonium salt washing in step (1) comprises the following steps:

[0014] The copper powder after alkali washing is washed with deionized water until the pH of the washing solution is neutral, and then the copper powder is transferred to an ammonium salt solution. At room temperature, the copper powder is subjected to ultrasonic-assisted treatment for 5-15 minutes under mechanical stirring at 300-500 rpm.

[0015] As a further improvement of the present invention: wherein the reducing metal salt solution in step (2) is stannous chloride solution and ferrous chloride solution.

[0016] As a further improvement of the present invention: wherein the amount of reducing metal ion solution in step (2) is 1000-1200wt% of the amount of copper powder; the concentration of the reducing metal ion solution is 0.1-0.5wt%.

[0017] As a further improvement of the present invention: wherein step (3) comprises the following steps:

[0018] Transfer the sensitized copper powder to the reactor, add the pre-prepared dispersant-reducing agent solution to the reactor, and at 35-45°C, perform ultrasonic-assisted treatment for 5-15 minutes under mechanical stirring at 500-700rpm to evenly disperse the copper powder. Transfer the reactor to a 35-45°C water bath, adjust the stirring speed to 200-400rpm, and drip the plating solution-silver ammonia complex solution into the dispersed copper powder reduction solution. The dripping time is controlled at 40-60 minutes, and the dripping speed is controlled at 4-6mL / min for the first 20-30 minutes, and the dripping speed is adjusted to 1-2mL / min for the remaining time. Continue the reaction for 15-30 minutes after the dripping is completed.

[0019] As a further improvement of the present invention: wherein the dispersant in step (3) is one of polyvinyl alcohol, polyvinyl pyrrolidone, polyethylene glycol, gelatin and polypeptide.

[0020] As a further improvement of the present invention: wherein the reducing agent in step (3) is one of sodium borohydride, ascorbic acid, glucose, hydrazine hydrate and tartaric acid.

[0021] As a further improvement of the present invention: wherein the concentration of the dispersant in step (3) is 0.5-1wt% (relative to the concentration of the aqueous phase); the amount of silver nitrate is determined according to a silver-to-copper mass ratio of 1:1; and ammonia water is added dropwise to the silver nitrate solution until the precipitate is just dissolved, which is the optimal amount of ammonia water.

[0022] As a further improvement of the present invention: it also includes a hydrophobic treatment step and a post-treatment, and the hydrophobic treatment includes the following steps:

[0023] Add anhydrous ethanol solution of octadecanoic acid into the kettle, and treat for 10-20 minutes at 35-45°C under mechanical stirring at 200-400 rpm;

[0024] The post-processing comprises the following steps:

[0025] The pretreated copper powder was washed with deionized water and treated in a vacuum oven at 60° C. for 12 h to obtain a finished silver-coated copper powder.

[0026] Compared with the prior art, the present invention has the following beneficial effects:

[0027] (1) The present invention completely removes the oleic acid and oxide film on the surface of the copper powder by alkali washing and ammonium salt solution washing, thereby solving the problem that the surface oxide film cannot be completely removed in the prior art, and the surface of the copper powder is completely activated;

[0028] (2) adding the activated copper powder to a reducing metal ion solution, stirring at room temperature for a certain period of time, so that the copper powder is fully immersed in the reducing metal ion solution, so that a small amount of reducing metal ions are adsorbed on its surface; after washing the copper powder with deionized water, transferring it to an extremely low concentration AgNO3 solution, stirring at room temperature for a certain period of time, a small amount of reducing ions adsorbed on the surface of the copper powder can reduce Ag+ to Ag, and adsorb on the surface of the copper powder;

[0029] (3) The Ag adsorbed on the surface of the copper powder after sensitization has two functions: 1) as a particle on the surface of the copper powder, during the subsequent silver plating, silver will be deposited around the particle; 2) as a catalyst for the subsequent chemical reduction silver plating, controlling the rate at the beginning of the reaction

[0030] (4) Using chemical reduction instead of replacement silver plating can ensure that there is no hollow shell in the copper powder. In addition, dripping the plating solution in a fast and then slow manner can ensure that the coating is smooth and dense, and the surface of the copper powder is thoroughly coated. The reason is that the rapid dripping of the plating solution in the early stage of the reaction can make silver deposit quickly and roughly on the surface of the copper powder, and the silver layer is not dense at this time; reducing the dripping speed of the plating solution in the middle and late stages of the reaction can make silver slowly deposit in the gaps of the silver layer, thereby increasing the continuity and density of the silver layer, and finally turning it into a smooth silver layer. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] In order to more clearly illustrate the technical solution, the drawings required for use in the implementation will be briefly introduced below. Obviously, the drawings described below are only some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.

[0032] Figure 1 This is a SEM image of the silver-coated copper powder prepared in the embodiment of the present invention.

[0033] Figure 2 The figure is a histogram of the thin disc resistance value of the silver-coated copper powder prepared in the second embodiment of the present invention subjected to resistivity test.

[0034] Figure 3 This is a microscopic picture of the effect of silk-screen printing of the silver-coated copper powder slurry prepared by the present invention.

[0035] Figure 4 This is the SEM image of the polyhedron silver-coated copper powder of the present invention.

[0036] Figure 5 The figure is the XRD pattern of the silver-coated copper powder prepared in the present invention. DETAILED DESCRIPTION

[0037] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be clearly and completely described below in conjunction with the specific embodiments of the present invention and the corresponding drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0038] It should be noted that the terms "first", "second", etc. in the specification and claims of the present invention and the above-mentioned drawings are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the data used in this way can be interchanged where appropriate, so that the embodiments of the present invention described herein can be implemented in an order other than those illustrated or described herein. In addition, the terms "including" and "having" and any variations thereof are intended to cover non-exclusive inclusions, for example, a process, method, system, product or device that includes a series of steps or units is not necessarily limited to those steps or units that are clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods, products or devices.

[0039] At present, photovoltaic power generation mainly relies on crystalline silicon solar cells, among which HJT cells are regarded as the core technology of the future due to their efficient, simple process and compatibility. However, the high demand for low-temperature silver paste by HJT cells has led to high costs, making it difficult to compete with PERC and TopCon cells in terms of cost performance. Silver-coated copper powder has the advantages of excellent performance and low cost, and is an effective way to reduce the cost of HJT cells. However, the existing synthesis method of silver-coated copper powder technology leads to a rough surface of silver-coated copper powder, and the silver layer is not dense. The synthesis method of cobalt-modified silver-coated copper powder material has excellent antioxidant properties, but the reliability of the double-coated powder obtained by plating cobalt on the surface of copper powder and then plating silver on the surface of cobalt remains to be investigated. It is unknown whether the coating is easy to detach, and the introduction of metallic cobalt undoubtedly increases the cost, which is not conducive to production. The replacement method and chemical reduction method are used to prepare silver-coated copper powder in combination, which has many steps and the replacement reaction is difficult to control, which is easy to cause empty shells. The existing technology has problems such as incomplete coating, poor coating quality, internal empty shells and complex processes. It is urgent to develop a high-performance and low-cost synthesis method of silver-coated copper powder.

[0040] In view of the problems in the prior art, the present invention provides a method for preparing silver-coated copper powder for HJT batteries, comprising the following steps:

[0041] (1) Activated copper powder: alkali washing; ammonium salt washing;

[0042] (2) Sensitized copper powder: copper powder is added to a reducing metal ion solution and transferred to an AgNO3 solution;

[0043] (3) Chemical reduction silver plating: Add reducing agent solution, add silver ion plating solution, and carry out silver plating reaction.

[0044] The invention uses alkali washing and ammonium salt solution washing to completely remove oleic acid and oxide film on the surface of copper powder and activate the surface of copper powder; fully immerse copper powder in reducing metal ion solution so that a small amount of reducing metal ions are adsorbed on the surface of copper powder, and then reduce Ag+ in extremely low concentration AgNO3 solution and adsorb it on the surface of copper powder; the adsorbed Ag acts as particles and catalyst to promote subsequent chemical reduction silver plating and ensure that copper powder does not have empty shells; a fast-then-slow dripping method is adopted to make the plating smooth and dense, and completely cover the surface of copper powder, thereby solving the problems of incomplete plating and empty shells in the prior art.

[0045] As an embodiment of the present invention, the alkali washing in step (1) comprises the following steps: adding copper powder and sodium hydroxide solution to a batching kettle respectively, and ultrasonically treating for 5-15 minutes at 35-45°C under mechanical stirring at 300-500rpm. The alkali washing removes grease from the surface of the copper powder.

[0046] Alkaline washing can effectively remove grease from the surface of copper powder, ensuring that there are no pollutants on the surface of copper powder in subsequent steps; mechanical stirring and ultrasonic assisted treatment ensure that the surface of copper powder is evenly contacted with sodium hydroxide solution, improving the uniformity and thoroughness of the cleaning effect; treatment under temperature control of 35-45°C helps to improve the cleaning efficiency and avoid the damage of high temperature to the structure of copper powder; avoid high temperature conditions, the reaction rate of copper powder with oxygen in the air will be significantly accelerated, and it is easy to form a layer of copper oxide on the surface of copper powder. High temperature will cause the thermal motion of copper powder particles to intensify, which is easy to cause agglomeration between particles. The surface area of ​​the agglomerated copper powder particles is reduced, which reduces the activation effect and also leads to uneven distribution of the subsequent silver plating layer; at high temperature, the grains of copper powder are prone to grow, resulting in a reduction in the interface between grains, thereby reducing the mechanical strength and conductivity of copper powder. Grain growth will cause adverse changes in the physical and chemical properties of copper powder, affecting its subsequent processing performance. At the same time, at high temperatures, the microstructure of the copper powder surface may change, increasing the surface roughness. This will affect the uniformity of the subsequent silver plating process and the density of the coating, resulting in a decrease in the performance of the final product; high temperature treatment may cause thermal stress inside the copper powder, especially in the case of rapid heating or cooling. The accumulation of this stress may cause microcracks or ruptures in the copper powder particles, further affecting its structural integrity and functional performance. Ultrasonic assisted treatment takes 5-15 minutes to complete the cleaning step in a short time, ensuring the high efficiency and production efficiency of the process.

[0047] As an embodiment of the present invention: the amount of sodium hydroxide solution used is 1000-1200wt% of the amount of copper powder used; the concentration of the sodium hydroxide solution is 0.1-0.5mol / L.

[0048] The use of 1000-1200wt% sodium hydroxide solution can ensure that the solution is in full contact with the copper powder, and that the grease and impurities on the surface of the copper powder are completely removed; the concentration of the sodium hydroxide solution is 0.1-0.5mol / L. Within this concentration range, the alkali solution can effectively remove grease and oxide film, and avoid excessive corrosion of the copper powder. The lower concentration of alkali solution reduces the corrosion effect on the surface of the copper powder, maintains the integrity and structural stability of the copper powder; provides a stable chemical environment, helps to evenly remove grease and oxides on the surface of the copper powder, avoids local overreaction caused by excessive concentration, and thus ensures the uniformity of the copper powder surface; the optimized solution dosage and concentration can also reduce the waste of chemical reagents and reduce production costs.

[0049] As an embodiment of the present invention: wherein the ammonium salt washing in step (1) comprises the following steps:

[0050] The copper powder after alkali washing is washed with deionized water until the pH of the washing solution is neutral, and then the copper powder is transferred to an ammonium salt solution. At room temperature, the copper powder is subjected to ultrasonic-assisted treatment for 5-15 minutes under mechanical stirring at 300-500 rpm.

[0051] Use deionized water to wash the copper powder after alkali washing to ensure that the pH value of the washing liquid reaches neutrality. This step neutralizes the residual alkali solution, avoids unnecessary side reactions during the ammonium salt washing process, and ensures the purity of the copper powder; the ammonium salt solution has excellent cleaning ability and can further remove tiny residues and impurities on the surface of the copper powder, especially a small amount of organic or inorganic matter that may remain after alkali washing. This process improves the cleanliness of the copper powder surface and ensures the effect of subsequent sensitization and silver plating steps; the ammonium salt solution can effectively maintain the activation state of the copper powder and provide good pretreatment conditions for the subsequent sensitization steps; under the mechanical stirring of 300-500rpm, combined with 5-15 minutes of ultrasonic assisted treatment, ensure that the ammonium salt solution can evenly contact each copper powder and improve the cleaning efficiency; the treatment is carried out at room temperature to avoid the damage of high temperature to the copper powder structure, while also reducing energy consumption and saving costs. Room temperature treatment can maintain the structural stability of the copper powder and prevent grain growth and surface roughness increase caused by high temperature. The copper powder surface after ammonium salt washing is clean and activated, providing an ideal foundation for subsequent sensitization and silver plating processes. The clean copper powder surface is conducive to the adsorption and uniform deposition of silver ions, ensuring the quality and performance of the final coating.

[0052] As an embodiment of the present invention: wherein the reducing metal salt solution in step (2) is stannous chloride solution and ferrous chloride solution; the amount of reducing metal ion solution used is 1000-1200wt% of the amount of copper powder used; and the concentration of the reducing metal ion solution is 0.1-0.5wt%.

[0053] Stannous chloride and ferrous chloride, as reducing metal salts, can effectively reduce the surface of copper powder to form a sensitized layer. The sensitized layer formed by the reducing metal ions on the surface of copper powder can promote the subsequent reduction and deposition of silver ions, and improve the efficiency and uniformity of the silver plating process; the use of 1000-1200wt% reducing metal ion solution ensures that the copper powder can be fully immersed and fully contacted with the reducing ions during the treatment process. This high proportion of dosage ensures that the surface of the copper powder is uniformly reduced and effectively enhances the formation and quality of the sensitized layer; the concentration range of 0.1-0.5wt% provides a moderate reducing metal ion concentration, which can not only effectively carry out sensitization treatment, but also avoid side reactions that may be caused by excessively high concentrations. The moderate concentration ensures the stability and controllability of the reduction reaction, while reducing unnecessary chemical reagent consumption; the reducing effect of stannous chloride and ferrous chloride can be uniformly deposited on the surface of copper powder, and can also react with subsequent silver ions to improve the uniformity and stability of the silver plating layer. The high proportion of solution dosage and moderate concentration ensure the integrity and uniformity of the sensitized layer, avoiding the problems of uneven deposition and insufficient sensitization; using stannous chloride and ferrous chloride as reducing agents can effectively control the reaction rate and conditions and provide a stable sensitized layer. The layer formed by these reducing metal ions on the surface of copper powder can serve as a good foundation for subsequent silver plating, improving the performance and consistency of the final product.

[0054] As an embodiment of the present invention: wherein step (3) includes the following steps:

[0055] Transfer the sensitized copper powder to the reactor, add the pre-prepared dispersant-reducing agent solution to the reactor, and at 35-45°C, perform ultrasonic-assisted treatment for 5-15 minutes under mechanical stirring at 500-700rpm to evenly disperse the copper powder. Transfer the reactor to a 35-45°C water bath, adjust the stirring speed to 200-400rpm, and drip the plating solution-silver ammonia complex solution into the dispersed copper powder reduction solution. The dripping time is controlled at 40-60 minutes, and the dripping speed is controlled at 4-6mL / min for the first 20-30 minutes, and the dripping speed is adjusted to 1-2mL / min for the remaining time. Continue the reaction for 15-30 minutes after the dripping is completed.

[0056] The dispersant is one of polyvinyl alcohol, polyvinyl pyrrolidone, polyethylene glycol, gelatin and polypeptide; the reducing agent is one of sodium borohydride, ascorbic acid, glucose, hydrazine hydrate and tartaric acid; the concentration of the dispersant is 0.5-1wt% (relative to the concentration of the water phase); the amount of silver nitrate is determined according to the silver-copper mass ratio of 1:1; ammonia water is added dropwise to the silver nitrate solution until the precipitate is just dissolved, which is the optimal amount of ammonia water.

[0057] Transfer the sensitized copper powder to the reactor and add the pre-prepared dispersant-reducing agent solution. At a temperature of 35-45°C, use 500-700rpm mechanical stirring and ultrasonic assisted treatment for 5-15 minutes to fully disperse the copper powder. The combination of ultrasonic and mechanical stirring can effectively break the agglomeration between copper powder particles, ensure that each copper powder can be evenly exposed to the reducing agent and dispersant, and help form a uniform silver plating layer; transfer the dispersed copper powder solution to a 35-45°C water bath, and adjust the stirring speed to 200-400rpm to provide a stable reaction environment. This temperature and stirring speed ensure the uniformity and stability of the silver plating reaction, and prevent uneven plating due to temperature fluctuations or uneven stirring; add the plating solution to the dispersed copper powder reducing solution, and the dropping time is controlled within 40-60 minutes. The drop rate is controlled at 4-6mL / min for the first 20-30 minutes, and the drop rate is adjusted to 1-2mL / min for the remaining time. This gradual dripping method enables the silver-ammonia complex solution to be evenly deposited on the surface of the copper powder, avoiding the problem of uneven coating or excessive local deposition caused by rapid dripping; the reaction is continued for 15-30 minutes after the dripping is completed to completely reduce the silver and deposit it on the surface of the copper powder. Extending the reaction time helps to ensure the complete deposition and good adhesion of the silver layer, improve the continuity and density of the coating, and ultimately form a smooth and uniform silver-coated copper powder. By optimizing the selection and concentration of the dispersant, the type of reducing agent, the amount of silver nitrate, and the optimal amount of ammonia water, the sensitization and silver plating effects of the copper powder can be effectively improved, ensuring that the quality and performance of the final silver-coated copper powder meet the requirements of HJT batteries.

[0058] As an embodiment of the present invention: it also includes a hydrophobic treatment step and a post-treatment, and the hydrophobic treatment includes the following steps:

[0059] Add anhydrous ethanol solution of octadecanoic acid into the kettle, and treat for 10-20 minutes at 35-45°C under mechanical stirring at 200-400 rpm;

[0060] The post-processing comprises the following steps:

[0061] The pretreated copper powder was washed with deionized water and treated in a vacuum oven at 60° C. for 12 h to obtain a finished silver-coated copper powder.

[0062] It can enhance the hydrophobicity of copper powder and prevent the influence of moisture and water on copper powder; improve the stability and treatment effect of copper powder in subsequent processes; form a stable hydrophobic layer to improve the dispersibility and treatment performance of copper powder; ensure the cleanliness of the copper powder surface through deionized water washing, providing a clean foundation for subsequent treatment; vacuum drying can effectively remove moisture and solvents, prevent oxidation, and ensure the stability and quality of copper powder.

[0063] The following is a specific implementation of a method for preparing silver-coated copper powder for HJT batteries of the present invention:

[0064] Implementation case 1:

[0065] A method for preparing silver-coated copper powder for HJT battery comprises the following steps:

[0066] (1) Activated copper powder:

[0067] Alkaline washing: add 25g copper powder and 250g sodium hydroxide solution into the batching kettle, respectively, the concentration of the sodium hydroxide solution is 0.3mol / L; at 40°C, under mechanical stirring at 350rpm, ultrasonic-assisted treatment for 15min;

[0068] Ammonium salt washing: the copper powder after alkali washing is washed with deionized water until the pH of the washing solution is neutral, and then the copper powder is transferred to an ammonium salt solution, the ammonium salt solution is an ammonium fluoride solution, the amount of the ammonium salt solution is 250g, and the concentration of the ammonium salt solution is 1.5wt%; at room temperature, under the action of mechanical stirring at 350rpm, ultrasonic-assisted treatment is performed for 15min, and after washing with deionized water, a thoroughly activated copper powder is obtained.

[0069] (2) Sensitized copper powder:

[0070] The activated copper powder is transferred to a new batching kettle, and a certain amount of reducing metal salt solution is added into the kettle, wherein the reducing metal salt solution is stannous chloride solution, the amount of reducing metal salt solution is 250g, and the concentration of reducing metal ion solution is 0.1wt%; at room temperature, the copper powder is treated under mechanical stirring at 250rpm for 35min; then the copper powder is washed with deionized water to obtain copper powder with reducing metal ions adsorbed on the surface, and the sensitization of the copper powder is completed.

[0071] (3) Chemical reduction silver plating:

[0072] The sensitized copper powder is transferred to the reactor, and the pre-prepared dispersant-reducing agent solution is added to the reactor, the reducing agent is ascorbic acid, the reducing agent dosage is 30.51g, the dispersant is polyethylene glycol, and the dispersant concentration is 0.8wt%; at 35°C, under the mechanical stirring of 500-700rpm, ultrasonic assisted treatment is performed for 5-15min to make the copper powder evenly dispersed. Next, the reactor is transferred to a 35°C water bath, the stirring speed is adjusted to 300rpm, and the plating solution-silver ammonia complex solution is added dropwise to the dispersed copper powder reduction solution, and the amount of silver nitrate is 39.37g; the dropping time is controlled at 40-60min, the dropping speed is controlled at 5mL / min for the first 20-30min, and the dropping speed for the remaining time is adjusted to 2mL / min. After the drop addition is completed, the reaction is continued for 15-30min.

[0073] (4) Hydrophobic treatment:

[0074] After the reaction, an anhydrous ethanol solution of octadecanoic acid was added to the kettle, and treated for 15 minutes at 35°C under mechanical stirring at 200-400rpm. The concentration of octadecanoic acid was 0.05wt%; the concentration of anhydrous ethanol was 0.5wt%; the concentrations of octadecanoic acid and anhydrous ethanol were both relative to the aqueous phase in the system.

[0075] (5) Post-processing

[0076] The pretreated copper powder was washed with deionized water and treated in a vacuum oven at 60° C. for 12 h to obtain a finished silver-coated copper powder.

[0077] Implementation case 2:

[0078] A method for preparing silver-coated copper powder for HJT battery comprises the following steps:

[0079] (1) Activated copper powder:

[0080] Alkaline washing: add 25g copper powder and 300g sodium hydroxide solution into the batching kettle, respectively, the concentration of the sodium hydroxide solution is 0.10mol / L; at 35°C, under mechanical stirring at 400rpm, ultrasonic-assisted treatment for 10min;

[0081] Ammonium salt washing: the copper powder after alkali washing is washed with deionized water until the pH of the washing solution is neutral, and then the copper powder is transferred to an ammonium salt solution, the ammonium salt solution is an ammonium sulfate solution, the amount of the ammonium salt solution is 300g, and the concentration of the ammonium salt solution is 2.0wt%; at room temperature, under the action of mechanical stirring at 500rpm, ultrasonic-assisted treatment is performed for 10min, and after washing with deionized water, a thoroughly activated copper powder is obtained.

[0082] (2) Sensitized copper powder:

[0083] The activated copper powder is transferred to a new batching kettle, and a certain amount of reducing metal salt solution is added into the kettle, wherein the reducing metal salt solution is ferrous chloride solution, the amount of reducing metal salt solution is 300g, and the concentration of reducing metal ion solution is 0.3wt%; at room temperature, the mixture is treated under mechanical stirring at 200rpm for 50min; then the copper powder is washed with deionized water to obtain copper powder with reducing metal ions adsorbed on the surface, and the sensitization of the copper powder is completed.

[0084] (3) Chemical reduction silver plating:

[0085] The sensitized copper powder is transferred to the reactor, and the pre-prepared dispersant-reducing agent solution is added to the reactor, the reducing agent is sodium borohydride, the reducing agent dosage is 13.16g, the dispersant is gelatin, and the dispersant concentration is 0.6wt%; at 30°C, under the mechanical stirring of 500-700rpm, ultrasonic assisted treatment is performed for 5-15min to make the copper powder evenly dispersed. Next, the reactor is transferred to a 30°C water bath, the stirring speed is adjusted to 250rpm, and the plating solution-silver ammonia complex solution is added to the dispersed copper powder reduction solution, and the amount of silver nitrate is 39.37g; the dropping time is controlled at 40-60min, the dropping speed is controlled at 4mL / min for the first 20-30min, and the dropping speed for the remaining time is adjusted to 1mL / min. After the drop addition is completed, the reaction is continued for 15-30min.

[0086] (4) Hydrophobic treatment:

[0087] After the reaction, an anhydrous ethanol solution of octadecanoic acid was added to the kettle, and treated at 30°C for 20 minutes under mechanical stirring at 250 rpm. The concentration of octadecanoic acid was 0.08 wt%; the concentration of anhydrous ethanol was 0.8 wt%; the concentrations of octadecanoic acid and anhydrous ethanol were both relative to the aqueous phase in the system.

[0088] (5) Post-processing

[0089] The pretreated copper powder was washed with deionized water and treated in a vacuum oven at 60° C. for 12 h to obtain a finished silver-coated copper powder.

[0090] The resistivity test of the silver-coated copper powder prepared in the implementation case 2 was carried out, and the results were as follows:

[0091]

[0092]

[0093] The resistivity of copper oxidation caused by incomplete coating in the prior art is as follows:

[0094]

[0095] The silver-coated copper powder was made into slurry, and the adhesion of the slurry was tested. The test results are as follows:

[0096]

[0097] The main functions of the present invention are:

[0098] The present invention provides a method for preparing silver-coated copper powder for HJT batteries, comprising the following steps: thoroughly removing oleic acid and oxide film on the surface of the copper powder by alkaline washing and ammonium salt solution, thereby achieving complete activation of the surface of the copper powder; immersing the activated copper powder in a reducing metal ion solution to ensure that the surface of the copper powder adsorbs reducing metal ions, and reducing and depositing Ag+ on the surface of the copper powder in an extremely low concentration AgNO3 solution. The sensitized silver not only serves as the starting point for silver plating, but also catalyzes subsequent reduction reactions. Silver plating is performed by chemical reduction rather than displacement, and a fast followed by slow dripping plating solution strategy is adopted to ensure that the silver coating is smooth, dense and completely coated, thereby significantly improving the quality and performance of the silver-coated copper powder.

[0099] In summary, after reading the present invention document, ordinary technicians in this field can make various other corresponding transformation schemes based on the technical scheme and technical concept of the present invention without creative mental work, which all fall within the scope of protection of the present invention.

Claims

1. A method for preparing silver-coated copper powder for HJT battery, characterized in that: The following steps are involved: (1) Activated copper powder: alkali washing; ammonium salt washing; (2) Sensitized copper powder: copper powder is added to a reducing metal ion solution and transferred to an AgNO3 solution; (3) Chemical reduction silver plating: Add reducing agent solution, add silver ion plating solution, and carry out silver plating reaction.

2. The method for preparing silver-coated copper powder for HJT battery according to claim 1, characterized in that: Wherein the alkali washing in step (1) comprises the following steps: Copper powder and sodium hydroxide solution are added to the batching kettle respectively, and ultrasonic-assisted treatment is performed for 5-15 minutes at 35-45° C. under mechanical stirring at 300-500 rpm.

3. The method for preparing silver-coated copper powder for HJT battery according to claim 2, characterized in that: The dosage of the sodium hydroxide solution is 1000-1200wt% of the dosage of the copper powder; and the concentration of the sodium hydroxide solution is 0.1-0.5mol / L.

4. The method for preparing silver-coated copper powder for HJT battery according to claim 1, characterized in that: Wherein the ammonium salt washing in step (1) comprises the following steps: The copper powder after alkali washing is washed with deionized water until the pH of the washing solution is neutral, and then the copper powder is transferred to an ammonium salt solution. At room temperature, the copper powder is subjected to ultrasonic-assisted treatment for 5-15 minutes under mechanical stirring at 300-500 rpm.

5. The method for preparing silver-coated copper powder for HJT battery according to claim 1, characterized in that: The reducing metal salt solution in step (2) is stannous chloride solution and ferrous chloride solution.

6. The method for preparing silver-coated copper powder for HJT battery according to claim 5, characterized in that: The amount of reducing metal ion solution in step (2) is 1000-1200wt% of the amount of copper powder; the concentration of the reducing metal ion solution is 0.1-0.5wt%.

7. The method for preparing silver-coated copper powder for HJT battery according to claim 1, characterized in that: Wherein step (3) comprises the following steps: The sensitized copper powder is transferred to the reactor, and the pre-prepared dispersant-reducing agent solution is added to the reactor. At 35-45°C, under the action of mechanical stirring at 500-700rpm, ultrasonic-assisted treatment is performed for 5-15min to evenly disperse the copper powder. The reactor is transferred to a water bath at 35-45°C, and the stirring speed is adjusted to 200-400rpm. The plating solution-silver ammonia complex solution is added dropwise to the dispersed copper powder reduction solution. The dropping time is controlled at 40-60min, and the dropping speed is controlled at 4-6mL / min for the first 20-30min. The dropping speed for the remaining time is adjusted to 1-2mL / min. After the dropping is completed, the reaction is continued for 15-30min.

8. The method for preparing silver-coated copper powder for HJT battery according to claim 7, characterized in that: The dispersant is one of polyvinyl alcohol, polyvinyl pyrrolidone, polyethylene glycol, gelatin and polypeptide.

9. The method for preparing silver-coated copper powder for HJT battery according to claim 7, characterized in that: The reducing agent is one of sodium borohydride, ascorbic acid, glucose, hydrazine hydrate and tartaric acid.

10. The method for preparing silver-coated copper powder for HJT battery according to claim 1, characterized in that: It also includes a hydrophobic treatment step and a post-treatment, wherein the hydrophobic treatment includes the following steps: Add anhydrous ethanol solution of octadecanoic acid into the kettle, and treat for 10-20 minutes at 35-45°C under mechanical stirring at 200-400 rpm; The post-processing comprises the following steps: The pretreated copper powder was washed with deionized water and treated in a vacuum oven at 60° C. for 12 h to obtain a finished silver-coated copper powder.