Novel alloy tool electrode for electrical discharge machining and preparation method of novel alloy tool electrode
By designing new alloy tool electrodes with high melting point metal raw materials and copper alloys, the problems of electrocorrosion loss during discharge processing and the reduction of bonding agent performance at high temperatures are solved, and higher electrocorrosion resistance and processing performance are achieved.
Patent Information
- Application Number
- CN202411087197.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-09
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-08-09
AI Technical Summary
The existing electrodes and tool electrodes have problems with large electrocorrosion losses and short life in discharge processing, especially under high temperature conditions, which reduces the mechanical properties and wear resistance of the bonding agent, resulting in poor processing efficiency and quality.
Design a new alloy tool electrode using metal raw material powder with high melting point and high mechanical properties, add copper or copper alloy powder, and prepare it through ball milling and cold pressing sintering to form a new type with high electrical corrosion resistance, wear resistance and high temperature stability. Alloy tool electrode.
Significantly reduce the electrocorrosion loss of electrodes and tool electrodes, extend service life, improve processing efficiency and surface quality, and avoid rapid wear of bonding agents and abrasive fall.
Smart Images

Figure CN118976951A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of electrical machining, and in particular relates to a novel alloy tool electrode for electrical discharge machining and a preparation method thereof. Background Art
[0002] At present, both electrodes and tool electrodes have the problem of being eroded by discharge effect, which is difficult to avoid. The metal raw materials currently used to prepare electrodes and tool electrodes have insufficient electro-erosion resistance, resulting in large electrode and tool electrode losses and short lifespan during processing, affecting processing efficiency and processing quality. Discharge machining is an important processing method in the field of material processing. In discharge machining, high discharge temperature is inevitable. According to different processing principles, it can be divided into electric spark discharge machining, electrochemical discharge machining, and composite processing methods based on the two, such as electric spark discharge assisted grinding and electrochemical discharge assisted grinding. These methods all involve gasification and etching of the processed material through the discharge effect of electrodes (only metal components) or tool electrodes (abrasive and metal binder components). However, it is precisely because of the existence of the discharge effect that existing studies have shown that these processing methods all have the problem of electrode and tool electrode being eroded by discharge effect, and it is difficult to avoid from the perspective of processing principles. In addition, for EDM and electrochemical discharge assisted grinding, the tool electrode (composed of abrasive and metal binder) faces the problem of reduced mechanical properties and wear resistance of the binder due to high discharge temperature (i.e., high temperature softening of the binder), in addition to the electrolytic erosion loss of the binder. This makes the binder easily worn by the hard phase too quickly during the processing, and the holding force of the binder on the abrasive will also decrease, resulting in premature and excessive shedding of the abrasive, thus greatly shortening the service life of the tool electrode. In addition, the problems of low processing efficiency, poor surface quality, and low processing accuracy caused by the loss of electrodes and tool electrodes cannot be ignored. Summary of the invention
[0003] In view of the above problems, the present invention proposes a new alloy tool electrode for electric discharge machining and a preparation method thereof, which is used to prepare electrodes and tool electrodes. By selecting metal raw material powders with high melting points and high mechanical properties, a new alloy with higher electro-corrosion resistance, high-temperature mechanical properties and wear resistance, high-temperature stability and high-temperature creep resistance is designed. On the one hand, the high electro-corrosion resistance of the new alloy can reduce the electro-corrosion loss of electrodes and tool electrodes. On the other hand, the high-temperature mechanical properties, wear resistance, and high-temperature stability of the new alloy can avoid rapid wear of tool electrode binders and abrasive shedding. Therefore, the new alloy can improve the service life and processing performance of electrodes and tool electrodes. In addition, a certain proportion of copper or copper alloy can be added to the new alloy powder to form a new alloy-reinforced copper-based composite material, which can simultaneously ensure the conductivity, electro-corrosion resistance, high-temperature mechanical properties and wear resistance of electrodes and tool electrodes.
[0004] One of the purposes of the present invention is to provide a new alloy tool electrode for electric discharge machining, the new alloy tool electrode is composed of the following components in parts by weight: 20-150 parts of new alloy powder, 1-100 parts of copper or copper alloy powder, and 5-30 parts of abrasive;
[0005] The novel alloy powder is prepared by mixing more than four elements of W, Nb, Mo, Ta, Zr, V, Ti and Hf in a molar ratio of (0.5-1.5):(0.5-1.5), and has a particle size of 5-150 μm.
[0006] The abrasive is one of uncoated diamond, W-coated diamond and Ti-coated diamond, and the particle size is 5-600 μm;
[0007] Furthermore, the novel alloy tool electrode is composed of the following components in parts by weight: 30-120 parts of novel alloy powder, 5-80 parts of copper or copper alloy powder, and 10-25 parts of abrasive;
[0008] The novel alloy powder is prepared by mixing more than four elements of W, Nb, Mo, Ta, Zr, V, Ti and Hf in a molar ratio of (0.5-1.5):(0.5-1.5), and has a particle size of 5-120 μm.
[0009] The abrasive is one of uncoated diamond, W-coated diamond and Ti-coated diamond, and has a particle size of 5-500 μm.
[0010] Furthermore, the novel alloy tool electrode is composed of the following components in parts by weight: 30-100 parts of novel alloy powder, 5-70 parts of copper or copper alloy powder, and 10-20 parts of abrasive;
[0011] The novel alloy powder is prepared by mixing more than four elements of W, Nb, Mo, Ta, Zr, V, Ti and Hf in a molar ratio of (0.5-1.5):(0.5-1.5), and has a particle size of 5-100 μm.
[0012] The abrasive is one of uncoated diamond, W-coated diamond and Ti-coated diamond, and has a particle size of 5-400 μm.
[0013] The second object of the present invention is to provide a method for preparing the novel alloy tool electrode for electric discharge machining, the method for preparing the novel alloy tool electrode comprising the following steps:
[0014] (1) Weighing the new alloy powder according to the required weight, and ball milling the new alloy powder in an argon / nitrogen atmosphere for 5-50 hours, with a ball-to-powder ratio of (10-30):1 and a rotation speed of 200-500 rpm;
[0015] (2) Weighing copper or copper alloy powder and abrasive according to the required weight proportions, mixing with the novel alloy powder obtained in step (1) and ball milling, wherein the ball mill speed is 100-250 r / min, the ball milling time is 1-10 h, the protective atmosphere is argon or nitrogen, and the total volume of the raw materials does not exceed 2 / 3 of the volume of the ball mill;
[0016] (3) placing the mixed material obtained in step (2) into a cold pressing mold for cold pressing to obtain a green body, wherein the green body has a green body density of 40 to 60% and a cold pressing pressure of 100 to 250 MPa;
[0017] (4) hot pressing and sintering the green body obtained above, heating to 750-1450°C at a heating rate of 40-100°C / min, keeping the temperature for 5-40min, the sintering pressure in the heating stage is 20-100MPa, the protective atmosphere is argon or nitrogen, and cooling to room temperature with the furnace to obtain the novel alloy tool electrode.
[0018] Compared with the prior art, the present invention has the following beneficial effects:
[0019] (1) The present invention proposes a designed new alloy used as an electrode material and a tool electrode binder material for electric discharge machining. Through a special composition design, it has extremely high electro-corrosion resistance, solving the serious problem of electro-corrosion loss of electrodes and tool electrodes in electric discharge machining; at the same time, the new alloy also has excellent high-temperature mechanical properties, wear resistance, high-temperature stability, etc., which can avoid rapid wear of the tool electrode binder and abrasive shedding under high discharge temperatures; it can improve the service life of electrodes and tool electrodes, machining efficiency, machining surface quality and machining accuracy, etc.;
[0020] (2) Compared with the currently commonly used electrode materials, the new alloy designed in the present invention has higher electro-corrosion resistance, can better cope with the environment and conditions during discharge machining, avoids serious electro-corrosion loss, thereby extending the service life of the electrode and tool electrode, and improving the machining performance.
[0021] (3) Compared with the commonly used tool electrode binder materials, the new alloy designed in the present invention has more excellent high-temperature mechanical properties, wear resistance, high-temperature stability, etc., which can avoid the rapid wear of the tool electrode binder and the shedding of abrasives, extend the service life of the tool electrode, and improve the processing performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 This is a graph showing the results of an electro-corrosion experiment on the electrode material of Example 1 of the present invention.
[0023] Figure 2This is a diagram of tool electrode wear and average material removal rate in Example 1 of the present invention.
[0024] Figure 3 This is a diagram showing the electro-corrosion test results of the electrode material of Example 2 of the present invention.
[0025] Figure 4 This is a diagram of tool electrode wear and average material removal rate in Example 2 of the present invention. DETAILED DESCRIPTION
[0026] The following is a summary of the embodiments Figure 1-4 The present invention is described in further detail.
[0027] Example 1
[0028] A method for preparing a novel alloy tool electrode for electric discharge machining, the method comprising the following steps:
[0029] (1) Weigh W, Nb, Mo, Ta, and Cr powders in a molar ratio of 1:1:1:1:1, with a particle size of 20 μm, and put them into a ball mill for alloying at a ball-to-material ratio of 20:1 for 50 h;
[0030] (2) 80 parts of the novel alloy powder prepared in step (1), 8 parts of copper powder and 12 parts of Ti-plated diamond abrasive, all with a particle size of 200 μm, were placed in a planetary ball mill and mixed thoroughly, wherein the ball mill speed was 150 rpm and the ball milling time was 6 h;
[0031] (3) placing the mixed powder obtained in step (2) into a mold for cold pressing to obtain a green body with a compact density of 65% and a cold pressing pressure of 240 MPa;
[0032] (4) hot pressing and sintering the green body obtained in step (3), heating the green body to 1400° C. at a heating rate of 75° C. / min, keeping the temperature for 5 min, and cooling the green body in the furnace to obtain a sintered block containing an abrasive.
[0033] After sintering, there are no obvious pores and cracks in the binder, and the degree of densification is high. At the same time, the hardness and compressive strength reach 841HV and 3500MPa respectively. The binder has a good embedding effect on diamond. The single pulse electrocorrosion experiment found that under the same conditions, the maximum depth and maximum width of the electrocorrosion pit on the new alloy substrate are significantly reduced compared with the control group (pure copper substrate). Figure 1 The tool electrodes with certain shapes and sizes were used in electrochemical discharge assisted grinding and drilling of aluminum-based silicon carbide composite materials. The results showed that the loss of the new alloy diamond tool electrode was significantly reduced compared with the pure Cu binder diamond tool electrode, while the average material removal rate was greatly improved. Figure 2As shown. In summary, the obtained new alloy diamond tool electrode has high wear resistance, electrical corrosion resistance and processing efficiency.
[0034] Example 2
[0035] A method for preparing a novel alloy tool electrode for electric discharge machining, the method comprising the following steps:
[0036] (1) W, Nb, Mo, Ta, and V powders were prepared in a molar ratio of 1:1:1:1:1, with a particle size of 20 μm; they were alloyed in a ball mill with a ball-to-material ratio of 20:1 for 50 h;
[0037] (2) 70 parts of the novel alloy powder obtained in step (1), 18 parts of copper powder, and 12 parts of Ti-coated diamond abrasive, wherein the particle size of the copper powder is 20 μm, and the particle size of the Ti-coated diamond abrasive is 200 μm, are placed in a planetary ball mill and mixed thoroughly, wherein the ball mill speed is 200 rpm, and the ball milling time is 8 h;
[0038] (3) placing the mixed powder obtained in step (3) into a mold for cold pressing to obtain a green body with a compact density of 55% and a cold pressing pressure of 200 MPa; hot pressing and sintering the green body obtained above, heating the green body to 1150°C at a heating rate of 100°C / min, keeping the temperature for 10 minutes, and cooling in the furnace to obtain a sintered block containing abrasive.
[0039] After sintering, there are no obvious pores and cracks in the binder, and the degree of densification is high. At the same time, the hardness and compressive strength reach 700HV and 2480MPa respectively. The binder has a good embedding effect on diamond. The single pulse electrocorrosion experiment found that under the same conditions, the maximum depth and maximum width of the electrocorrosion pit on the new alloy substrate are significantly reduced compared with the control group (pure copper substrate). Figure 3 The tool electrodes with certain shapes and sizes were used in electrochemical discharge assisted grinding and drilling of aluminum-based silicon carbide composite materials. The results showed that the loss of the new alloy diamond tool electrode was significantly reduced compared with the pure Cu binder diamond tool electrode, while the average material removal rate was greatly improved. Figure 4 As shown. In summary, the obtained new alloy diamond tool electrode has high wear resistance, electrical corrosion resistance and processing efficiency.
[0040] Comparative Example 1
[0041] The difference between Comparative Example 1 and Example 1 is that the same weight fraction of Cu powder is used to replace the new alloy powder;
[0042] Comparative Example 2
[0043] The difference between Comparative Example 2 and Example 2 is that the same weight fraction of Cu powder is used to replace the abrasive;
[0044] Comparative Example 3
[0045] The only difference between Comparative Example 3 and Example 1 is that the particle size of the new alloy powder is 180 μm;
[0046] Comparative Example 4
[0047] The difference between Comparative Example 4 and Example 1 is only that the particle size of the abrasive is 650 μm;
[0048] Comparative Example 5
[0049] The only difference between Comparative Example 5 and Example 2 is that the particle size of the new alloy powder is 180 μm;
[0050] Comparative Example 6
[0051] The only difference between Comparative Example 6 and Example 1 is that the particle size of the abrasive is 650 μm;
[0052] Comparative Example 7
[0053] The difference between Comparative Example 7 and Example 1 is that the same weight proportions of Mo, Ta, and Cr powders are used to replace W, Nb, Mo, Ta, and Cr powders;
[0054] Comparative Example 8
[0055] The difference between Comparative Example 8 and Example 1 is that the same weight proportions of W, Nb, and Mo powders are used to replace W, Nb, Mo, Ta, and Cr powders;
[0056] Comparative Example 9
[0057] The difference between Comparative Example 9 and Example 2 is that the same weight proportions of W, Nb, and Mo powders are used to replace W, Nb, Mo, Ta, and V powders;
[0058] Comparative Example 10
[0059] The difference between Comparative Example 10 and Example 2 is that the same weight proportions of Mo, Ta, and V powders are used to replace W, Nb, Mo, Ta, and V powders;
[0060] The above test data are recorded in Table 1.
[0061] Table 1
[0062]
[0063] It can be seen from Table 1 that the particle size and composition of the new alloy powder and the abrasive particle size also have a certain influence on the electro-etching results, electrode loss and material removal rate. Among them, the change of the composition of the new alloy powder has a relatively large influence on these effects. Compared with the electrodes in Comparative Examples 1-2, the tool electrode of the present invention has a very good performance.
[0064] The above content is the best specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily thought of by any technician familiar with the technical field within the technical scope disclosed by the present invention should be covered within the protection scope of the present invention.
Claims
1. A new alloy tool electrode for electric discharge machining, characterized in that: The novel alloy tool electrode is composed of the following components in parts by weight: 20-150 parts of novel alloy powder, 1-100 parts of copper or copper alloy powder, and 5-30 parts of abrasive; The novel alloy powder is prepared by mixing more than four elements of W, Nb, Mo, Ta, Zr, V, Ti and Hf in a molar ratio of (0.5-1.5):(0.5-1.5), and has a particle size of 5-150 μm. The abrasive is one of uncoated diamond, W-coated diamond and Ti-coated diamond, and has a particle size of 5-600 μm.
2. A new alloy tool electrode for electric discharge machining as claimed in claim 1, characterized in that: The novel alloy tool electrode is composed of the following components in parts by weight: 30-120 parts of novel alloy powder, 5-80 parts of copper or copper alloy powder, and 10-25 parts of abrasive; The novel alloy powder is prepared by mixing more than four elements of W, Nb, Mo, Ta, Zr, V, Ti and Hf in a molar ratio of (0.5-1.5):(0.5-1.5), and has a particle size of 5-120 μm. The abrasive is one of uncoated diamond, W-coated diamond and Ti-coated diamond, and has a particle size of 5-500 μm.
3. A new alloy tool electrode for electric discharge machining as claimed in claim 2, characterized in that: The novel alloy tool electrode is composed of the following components in parts by weight: 30-100 parts of novel alloy powder, 5-70 parts of copper or copper alloy powder, and 10-20 parts of abrasive; The novel alloy powder is prepared by mixing more than four elements of W, Nb, Mo, Ta, Zr, V, Ti and Hf in a molar ratio of (0.5-1.5):(0.5-1.5), and has a particle size of 5-100 μm. The abrasive is one of uncoated diamond, W-coated diamond and Ti-coated diamond, and has a particle size of 5-400 μm.
4. A method for preparing a new alloy tool electrode for electric discharge machining according to any one of claims 1 to 3, characterized in that: The method for preparing the novel alloy tool electrode comprises the following steps: (1) Weighing the new alloy powder according to the required weight, and ball milling the new alloy powder in an argon / nitrogen atmosphere for 5-50 hours, with a ball-to-powder ratio of (10-30):1 and a rotation speed of 200-500 rpm; (2) Weighing copper or copper alloy powder and abrasive according to the required weight proportions, mixing with the novel alloy powder obtained in step (1) and ball milling, wherein the ball mill speed is 100-250 r / min, the ball milling time is 1-10 h, the protective atmosphere is argon or nitrogen, and the total volume of the raw materials does not exceed 2 / 3 of the volume of the ball mill; (3) placing the mixed material obtained in step (2) into a cold pressing mold for cold pressing to obtain a green body, wherein the green body has a green body density of 40 to 60% and a cold pressing pressure of 100 to 250 MPa; (4) hot pressing and sintering the green body obtained above, heating to 750-1450°C at a heating rate of 40-100°C / min, keeping the temperature for 5-40min, the sintering pressure in the heating stage is 20-100MPa, the protective atmosphere is argon or nitrogen, and cooling to room temperature with the furnace to obtain the novel alloy tool electrode.
Citation Information
Patent Citations
Combined electric spark grinding machining tool, tool manufacturing method and machining method
CN112351862A
Active electrode material
CN114868278A
Method and device for discharge surface treatment
CN1329531A
Electrode material
CN1873876A
Discharge surface treatment method, and treatment device
JP1998225824A