Automatic polishing method for welding leakage in weld joint of bent pipe of liquid rocket engine
Through the automated grinding method, the grinding amount is controlled by combining force feedback of the contour clamp and floating spindle, combined with line laser detection, and solved the problem of high manual operation skills and low pass rate in the welding process of bending pipe of liquid rocket engines. The problem has achieved precise polishing and quality improvement of welding leakage.
Patent Information
- Application Number
- CN202410973835.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-11-19
AI Technical Summary
The welding and grinding process of existing liquid rocket engine bending pipe welds relies on manual operation, with high skill requirements and low pass rate, which leads to high difficulty in welding and grinding and poor product quality and reliability.
Using automated grinding method, by adjusting the consistency of the bend pipe loading, determining the grinding starting point and trajectory, using the combined force feedback of the prototyping clamps and floating spindles to control the grinding amount, combined with line laser detection to achieve accurate grinding of welding leakage, ensuring grinding The results meet technical requirements.
The controllability and quality assurance of bending pipe leakage grinding is improved, ensuring that the welding leakage is not higher than 0.5mm relative to the base material, and the recess to the main material is not greater than 0.3mm, improving the production reliability and pass rate.
Smart Images

Figure CN118977144A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of processing internal weld leaks in bent pipe welds, and in particular relates to an automatic grinding method for internal weld leaks in bent pipe welds of liquid rocket engines. Background Art
[0002] The main pipeline of the liquid rocket engine system serves as the main supply channel for oxidizer and fuel. The reverse side of the elbow weld must have a smooth transition without droplet welds and sharp protrusions. Otherwise, it will be easily washed away by the high-pressure, high-speed liquid oxygen or fuel gas flowing through this cavity, producing excess matter and seriously affecting the working reliability of the engine.
[0003] The elbow, which is part of the main pipeline of the system, adopts the half-pipe welding process, which will produce a long outer diameter longitudinal weld and a short inner diameter longitudinal weld. After the longitudinal seam is welded, according to the technical requirements, the reverse side weld leakage needs to be polished, and the reverse side weld leakage is required to be no higher than 0.5mm, and the concavity to the main material is allowed to be no more than 0.3mm during polishing.
[0004] The longitudinal weld form of the bent pipe, such as Figure 1 shown.
[0005] The existing welding leak grinding process mainly relies on workers to use pneumatic grinding heads or files for manual grinding. Manual grinding requires high skill levels of operators, and it is difficult for the welding leak height to meet technical requirements, and the product quality and reliability are poor. There are often problems such as repeated grinding due to excessive height, or excessive grinding exceeding the lower limit of the height, which requires re-welding and re-grinding. Summary of the invention
[0006] The purpose of the present invention is to provide a method for automatically grinding weld leaks in the weld seam of a liquid rocket engine elbow pipe in view of the problems that the existing grinding process has high requirements on the skill level of the operator and the weld leak grinding pass rate is low.
[0007] The technical solution adopted by the present invention is as follows:
[0008] A method for automatically grinding internal weld leaks in a liquid rocket engine elbow weld, comprising:
[0009] (1) Adjust the consistency of elbow feeding;
[0010] Profiling clamps are made according to the bending angle, bending radius and bending diameter to ensure that all the bent pipes with qualified sizes can be accurately placed in the profiling clamps when loading; after the bent pipe is loaded, the end face of the bent pipe is aligned with the end face of the profiling clamp, and the curved surface of the bent pipe is not warped, and the bent pipe is pressed by a clamping mechanism;
[0011] (2) Determine the starting point of grinding;
[0012] By means of photographic measurement, the weld leak morphology is photographed to form a cross-sectional view of one end of the elbow. The highest point of the cross-sectional view is taken as the starting point for grinding, and the distance between the highest point and the outer edge of the pipe diameter is taken as the grinding amount. The grinding width is formed according to the width of the weld leak of the elbow.
[0013] (3) Grinding with controlled grinding amount;
[0014] An arc is generated by the bending radius of the bent pipe, the center point of the profiling clamp and the bending angle of the pipe, and a grinding trajectory is formed by combining the grinding starting point and the grinding amount. The robot drives the rotating grinding head to grind according to the grinding trajectory, and the dust removal system is started simultaneously. When the robot is grinding, the grinding amount is controlled by the floating spindle in combination with force feedback. During grinding, it is determined whether the force feedback value meets the force feedback set value. If not, the original grinding starting point is used to continue grinding with force. If it meets the requirements, step (4) is entered; the center point of the profiling clamp coincides with the center point of the bent pipe.
[0015] (4) After grinding, perform welding leak detection;
[0016] The laser point cloud measurement of the weld leak and the ±5mm area on both sides is performed using a line laser to form a specific value of the weld leak relative to the base material height to determine whether the grinding is qualified.
[0017] Furthermore, when the contoured clamp is manufactured, the bending angle tolerance is ≤±1°, the bending radius tolerance is ≤0.5mm, and the bending diameter tolerance is ≤3mm.
[0018] Furthermore, the bent pipe material is made of 1Cr18Ni9Ti, S-03, S-06 or GH202 special steel.
[0019] Furthermore, the contoured clamp is made of resin material and completed through 3D printing to prevent aging and deformation.
[0020] Furthermore, an arc is generated by the bending radius of the elbow, the center point of the profiling clamp and the bending angle of the elbow, and a grinding trajectory is formed by combining the grinding starting point and the grinding amount, specifically:
[0021] Starting from the grinding starting point, an arc is generated along the bending radius of the elbow, the center point of the profiling clamp (coinciding with the center point of the elbow) and the bending angle. The grinding head starts grinding from the starting point of the arc to the end point of the arc. Then the grinding head is offset along the grinding width direction by a certain distance (this distance is related to the grinding feed amount and needs to be obtained through experiments based on the pipe material and the grinding head material) and then grinds in the reverse direction until the grinding area covers the grinding width.
[0022] Furthermore, the floating spindle is used to ensure the constancy of the grinding force, adapt to the deviation between the actual bending radius of the bent pipe and the theoretical bending radius, and the deviation between the actual wall thickness of the bent pipe and the theoretical wall thickness, so as to ensure that the grinding process does not damage the bent pipe base.
[0023] Furthermore, the force feedback, i.e. the feedback of the grinding force of the grinding head to the floating spindle, is a basic condition for the floating spindle to realize its function and ensures the constancy of the grinding force.
[0024] Furthermore, the force feedback setting value is obtained based on the previous test, is related to the material of the grinding head, the material of the bent pipe, and the feed rate, and is determined through experiments.
[0025] Furthermore, the preliminary test needs to calibrate the relative position relationship between the middle point of the outer edge of the grinding head and the fixed point of the end face of the profiling clamp, that is, put the grinding head and the bent pipe into the same coordinate system to ensure the accuracy of the grinding starting point and grinding trajectory.
[0026] Furthermore, the floating spindle is combined with force feedback to ensure that the weld leakage is no higher than 0.5mm relative to the parent material and the depression into the main material is no greater than 0.3mm.
[0027] The beneficial effects of the present invention are:
[0028] (1) The grinding process method formed by accurate measurement and calculation of the grinding starting point, bidirectional grinding trajectory, and grinding amount of the present invention replaces the traditional grinding method of manual grinding based on experience, improves the controllability of the welding leak grinding of the bent pipe, and improves the quality assurance of the bent pipe.
[0029] (2) The profiling clamp of the present invention collects key data of the bent pipe to form a support solution for the bent pipe with placement repeatability and consistency that can meet the grinding accuracy of -0.3 to +0.5 mm. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 This is a schematic diagram of the longitudinal weld form of the bent pipe;
[0031] Figure 2 It is a schematic diagram of the calculation of the grinding starting point and grinding amount of the present invention;
[0032] Figure 3 is a schematic diagram of the grinding width of the present invention;
[0033] Figure 4 The figure is a flow chart of the method of the present invention. DETAILED DESCRIPTION
[0034] The present invention designs an automatic grinding method for weld leaks in the weld seams of liquid rocket engines. The grinding process of weld leaks in the weld seams of the elbow pipes is changed from the traditional manual grinding using a pneumatic grinding wheel. The grinding starting point is accurately found through photographic measurement, and a manipulator grabs a rotating grinding head to achieve grinding. Closed-loop control is achieved through the combination of floating spindle + force feedback + line laser detection. The grinding amount of weld leaks in the elbow pipe can always be controlled within a precise range, so that the weld leak is no higher than 0.5mm relative to the parent material and is not more than 0.3mm recessed into the main material. The overall accuracy is 0.02mm.
[0035] The key points of the automatic grinding method for welding leaks in the weld seam of the liquid rocket engine elbow pipe of the present invention are: ensuring the consistency and repeatability of the elbow feeding, finding the grinding starting point, accurately controlling the grinding amount and detecting welding leaks after the grinding is completed. Figure 4 As shown, the following steps are included:
[0036] (1) Ensure the consistency and repeatability of elbow feeding
[0037] The profiling clamp is made according to the bending angle, bending radius and bending diameter (bending angle tolerance ≤±1°, bending radius tolerance ≤0.5mm, bending diameter tolerance ≤3mm). The above three data are made according to the upper difference to ensure that all bent pipes with qualified dimensions can be accurately placed in the profiling clamp. The profiling clamp is made of resin material and completed by 3D printing to prevent aging and deformation.
[0038] After the bent pipe is loaded, the end face of the bent pipe is aligned with the end face of the clamping block, the curved surface of the bent pipe is free of warping, and the bent pipe is clamped using a clamping mechanism.
[0039] (2) Determine the starting point of grinding
[0040] like Figure 2 and Figure 3 As shown, by photographing the weld leak morphology, a cross-sectional view of one end of the elbow is formed, the highest point of the cross-sectional view is taken as the starting point for grinding, and the distance between the highest point and the outer edge of the pipe diameter is taken as the grinding amount; the grinding width is formed according to the width of the weld leak of the elbow;
[0041] (3) Control the grinding amount for grinding
[0042] An arc is generated by using the bending radius of the bend, the center point of the profiling clamp and the bending angle of the bend, and a grinding trajectory is formed by combining the grinding starting point and the grinding amount. The robot drives the rotating grinding head to grind according to the grinding trajectory, and the dust removal system is started simultaneously. When the robot is grinding, the grinding amount is controlled by the floating spindle combined with force feedback. During grinding, it is determined whether the force feedback value meets the force feedback set value. If not, the force grinding is continued at the original grinding starting point. If it is satisfied, the process proceeds to step (4).
[0043] The specific formation of the grinding trajectory is as follows: starting from the grinding starting point, an arc is generated along the bending radius of the elbow, the center point of the contour clamp (coinciding with the center point of the elbow) and the bending angle of the elbow, and the grinding head starts grinding from the starting point of the arc to the end point of the arc, and then the grinding head is offset along the grinding width direction by a certain distance (this distance is related to the grinding feed amount, and needs to be obtained through experiments based on the pipe material and the grinding head material) and then grinds in the reverse direction until the grinding area covers the grinding width.
[0044] In the present invention, the center point of the contoured clamp coincides with the center point of the curved pipe;
[0045] In the present invention, the floating spindle + force feedback is used to ensure that the weld leakage is no higher than 0.5 mm relative to the parent material and the depression into the parent material is no greater than 0.3 mm.
[0046] The floating spindle is used to ensure the constant grinding force, adapt to the deviation between the actual bending radius and the theoretical bending radius of the bent pipe, and the deviation between the actual wall thickness and the theoretical wall thickness of the bent pipe, so as to ensure that the bent pipe base is not damaged during the grinding process. The force feedback is the feedback of the grinding force of the grinding head to the floating spindle, which is the basic condition for the floating spindle to realize its function and ensure the constant grinding force.
[0047] The force feedback setting value is obtained according to the preliminary test, and is related to the material of the grinding head, the material of the bent pipe, and the feed rate. The grinding head speed, the feed rate along the grinding track, and the bidirectional feed rate along the pipe diameter direction are found out through preliminary tests.
[0048] The preliminary test requires calibrating the relative position relationship between the middle point of the outer edge of the grinding head and the fixed point of the end face of the profiling clamp, that is, placing the grinding head and the bent pipe in the same coordinate system to ensure the accuracy of the grinding starting point and grinding trajectory.
[0049] The grinding width is determined according to the width of the elbow weld, generally ≤10mm.
[0050] During the grinding process, pay attention to dust collection, noise isolation, and physical isolation of the grinding mechanism.
[0051] (4) After grinding, perform welding leak detection;
[0052] The laser point cloud measurement of the weld leak and the ±5mm area on both sides is performed using a line laser to form a specific value of the weld leak relative to the base material height to determine whether the grinding is qualified.
[0053] Example:
[0054] This embodiment provides a method for automatically grinding the internal weld leak of a liquid rocket engine elbow weld, provided that the deviations of the three key basic data must satisfy the elbow angle tolerance ≤±1°, the bending radius tolerance ≤0.5mm, and the elbow diameter tolerance ≤3mm. A cross-sectional view of one end of the elbow is formed by photographic measurement, and the highest point of the cross-sectional view is taken as the starting point for grinding, and the distance between the highest point and the outer edge of the pipe diameter is taken as the grinding amount. A grinding trajectory is formed according to the bending radius of the elbow and the center point of the contoured clamp. A grinding width is formed according to the width size of the weld leak of the elbow. A grinding trajectory is formed on the grinding width according to the inner diameter of the elbow.
[0055] The bending materials include special steels such as 1Cr18Ni9Ti, S-03, S-06, GH202, etc. The equipment includes grinding head, turntable, fixture, robot control system, visual recognition system, dust removal system and sound insulation system. The profiling clamp block is made of resin material and completed by 3D printing to prevent aging and deformation.
[0056] The relative position relationship between the middle point of the outer edge of the grinding head and the fixed point of the end face of the profiling clamp is calibrated to establish a unified coordinate system. Through experiments, the grinding head speed, feed along the grinding width, and feed along the pipe diameter direction (related to the grinding force of the floating spindle) for different material bends are explored. The grinding actuator grinds the weld leak in the same way as the rotary file. During the grinding process, attention should be paid to dust collection, noise isolation, and physical isolation of the grinding mechanism.
[0057] At the loading station, the staff places the product on the contour clamp, the clamping cylinder clamps the product, the scanning camera scans and locates the product weld, finds the starting point of grinding, and after the scanning is completed, the turntable with the fixture and the product rotates to the soundproof room, the grinding robot drives the grinding head to grind along the weld, and the dust removal system is started at the same time. After the grinding is completed, the turntable with the fixture and the product rotates out of the soundproof room, and the next elbow to be polished enters the soundproof room for grinding. The staff removes the polished product and puts the next workpiece on, and the cycle continues.
[0058] By means of the process method formed by the present invention, the weld leaks in the weld seams of the bent pipes of liquid rocket engines are automatically polished, so that the quality and diameter of the inner wall of the liquid rocket engine conduit meet the use requirements, the weld leak polishing work is controllable, the production bottleneck problem is solved, and the production qualification rate is improved.
[0059] Parts of the present invention that are not described in detail belong to common knowledge among those skilled in the art.
Claims
1. A method for automatically grinding internal weld leaks in a liquid rocket engine elbow weld, characterized in that include: (1) Adjust the consistency of elbow feeding; Profiling clamps are made according to the bending angle, bending radius and bending diameter to ensure that all the bent pipes with qualified sizes can be accurately placed in the profiling clamps when loading; after the bent pipe is loaded, the end face of the bent pipe is aligned with the end face of the profiling clamp, and the curved surface of the bent pipe is not warped, and the bent pipe is pressed by a clamping mechanism; (2) Determine the starting point of grinding; By means of photographic measurement, the weld leak morphology is photographed to form a cross-sectional view of one end of the elbow. The highest point of the cross-sectional view is taken as the starting point for grinding, and the distance between the highest point and the outer edge of the pipe diameter is taken as the grinding amount. The grinding width is formed according to the width of the weld leak of the elbow. (3) Grinding with controlled grinding amount; An arc is generated by the bending radius of the bent pipe, the center point of the profiling clamp and the bending angle of the pipe, and a grinding trajectory is formed by combining the grinding starting point and the grinding amount. The robot drives the rotating grinding head to grind according to the grinding trajectory, and the dust removal system is started simultaneously. When the robot is grinding, the grinding amount is controlled by the floating spindle in combination with force feedback. During grinding, it is determined whether the force feedback value meets the force feedback set value. If not, the original grinding starting point is used to continue grinding with force. If it meets the requirements, step (4) is entered; the center point of the profiling clamp coincides with the center point of the bent pipe. (4) After grinding, perform welding leak detection; The laser point cloud measurement of the weld leak and the ±5mm area on both sides is performed using a line laser to form a specific value of the weld leak relative to the base material height to determine whether the grinding is qualified.
2. The method for automatically grinding internal weld leaks in a liquid rocket engine elbow weld according to claim 1, characterized in that: When making the contour clamp, the bending angle tolerance is ≤±1°, the bending radius tolerance is ≤0.5mm, and the bending diameter tolerance is ≤3mm.
3. The method for automatically grinding internal weld leaks in a liquid rocket engine elbow weld according to claim 1, characterized in that: The bending pipe material is 1Cr18Ni9Ti, S-03, S-06 or GH202 special steel.
4. The method for automatically grinding internal weld leaks in a liquid rocket engine elbow weld according to claim 2, characterized in that: The contoured clamp is made of resin material and completed through 3D printing to prevent aging and deformation.
5. The method for automatically grinding internal weld leaks in a liquid rocket engine elbow weld according to claim 1, characterized in that: An arc is generated based on the bending radius of the elbow, the center point of the profiling clamp and the bending angle of the elbow. The grinding trajectory is formed by combining the grinding starting point and the grinding amount. Specifically: Starting from the grinding starting point, an arc is generated along the bending radius of the elbow, the center point of the profiling clamp and the bending angle of the elbow. The grinding head starts grinding from the starting point of the arc to the end point of the arc. Then the grinding head is offset a certain distance along the grinding width direction and then grinds in the reverse direction until the grinding area covers the grinding width.
6. The method for automatically grinding internal weld leaks in a liquid rocket engine elbow weld according to claim 5, characterized in that: The floating spindle is used to ensure constant grinding force, adapt to the deviation between the actual bending radius of the bent pipe and the theoretical bending radius, and the deviation between the actual wall thickness of the bent pipe and the theoretical wall thickness, so as to ensure that the bent pipe base is not damaged during the grinding process.
7. The method for automatically grinding internal weld leaks in a liquid rocket engine elbow weld according to claim 5, characterized in that: The force feedback, i.e. the feedback of the grinding force of the grinding head to the floating spindle, is the basic condition for the floating spindle to realize its function and ensures the constancy of the grinding force.
8. The method for automatically grinding internal weld leaks in a liquid rocket engine elbow weld according to claim 6, characterized in that: The force feedback setting value is obtained based on the previous test, is related to the material of the grinding head, the material of the bending pipe, and the feed rate, and is determined through experiments.
9. The method for automatically grinding internal weld leaks in a liquid rocket engine elbow weld according to claim 8, characterized in that: The preliminary test requires calibrating the relative position relationship between the middle point of the outer edge of the grinding head and the fixed point of the end face of the profiling clamp, that is, placing the grinding head and the bent pipe in the same coordinate system to ensure the accuracy of the grinding starting point and grinding trajectory.
10. The method for automatically grinding internal weld leaks in a liquid rocket engine elbow weld according to claim 8, characterized in that: The floating spindle combined with force feedback ensures that the weld leakage is no higher than 0.5mm relative to the parent material and the depression into the main material is no more than 0.3mm.
Citation Information
Patent Citations
Welding line polishing robot
CN107116561A
System and method for grinding part weld joint based on vision guide robot
CN110253373A
Equipment and method for automatically polishing vehicle body side wall skin welding seam through robot
CN114800171A
Automatic grinding decision planning device and method for intelligent grinding robot
CN115805503A
Elbow welding seam polishing device and method based on machine vision and force control
CN117207008A