Photovoltaic inverted grinding integrated accurate grinding wheel and preparation method thereof

By designing a grinding wheel containing artificial polycrystalline diamond and resin powder in the processing of photovoltaic silicon crystal rods, the problems of poor self-sharpness and low processing accuracy of traditional grinding wheels are solved, and higher processing accuracy and longer service life are achieved .

CN118977206AActive Publication Date: 2024-11-19NANJING SANCHAO ADVANCED MATERIALS

Patent Information

Application Number
CN202411267141.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-11
Publication Date
2024-11-19
Estimated Expiration
2044-09-11

AI Technical Summary

Technical Problem

In the processing of photovoltaic silicon crystal rods, traditional grinding wheels have problems such as poor self-sharpness, poor surface state, high processing load, low processing accuracy, poor impact resistance and low life. In addition, conventional resin grinding wheels are prone to produce sticky chips and the use of lubricating additives Ineffective enough, it affects the overall strength of the grinding wheel.

Method used

A photovoltaic backgrinding integrated fine grinding wheel is designed, including a substrate and abrasive layer. The abrasive layer consists of artificial polycrystalline diamond, auxiliary abrasives, lubricating additives, wear-resistant fibers and resin powders. Through specific mixing and forming processes, an arc is formed. The abrasive layer distributed in blocks combines the integrated production method of cold press forming and high-temperature curing to improve the sharpness and durability of the grinding wheel.

Benefits of technology

It improves the sharpness and impact resistance of the grinding wheel, reduces the grinding force during processing, extends the service life of the grinding wheel, ensures processing accuracy and surface quality, and avoids excessive loss of traditional grinding wheels and burns on the surface of the workpiece.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118977206A_ABST
    Figure CN118977206A_ABST
Patent Text Reader

Abstract

The invention discloses a photovoltaic reverse grinding integrated accurate grinding wheel and a preparation method thereof, and relates to the technical field of grinding wheel preparation, the photovoltaic reverse grinding integrated accurate grinding wheel comprises a base body and a grinding material layer located on the outer end face of the base body and distributed in the circumferential direction, and the grinding material layer comprises, by weight, 18-38 parts of artificial polycrystalline diamond; 19-22 parts of an auxiliary grinding material; 1.5-2 parts of a lubricating additive; 5 to 12.5 parts of wear-resistant fiber; according to the photovoltaic reverse grinding integrated accurate grinding wheel, the machining precision and the impact resistance of the grinding wheel are effectively improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of preparation of a grinding wheel, and more specifically to a grinding wheel for grinding and grinding photovoltaic silicon crystal rod wire post-processing and a preparation method thereof. Background Art

[0002] At present, with the rapid development of the photovoltaic industry, the surface condition requirements for photovoltaic silicon ingots are getting higher and higher. Under this condition, traditional grinding wheels are gradually unable to meet the growing quality requirements, showing problems such as poor self-sharpening, poor surface condition, high processing load, low processing accuracy, poor impact resistance of grinding wheels, and low life. Therefore, it is imperative to develop high-performance grinding and polishing tools and consumables for the photovoltaic industry.

[0003] There are many problems with the conventional resin grinding wheels currently used, such as easy to produce sticky chips, the surface processing accuracy of the workpiece does not meet the requirements, etc. At the same time, the grinding wheel is difficult to dress and the lubricating additives used in traditional grinding wheels are generally black graphite powder, MoS 2 Materials such as quartz have weak lubrication ability and need to be added in large quantities to play a lubricating role. However, excessive addition will significantly reduce the overall strength of the grinding wheel, causing excessive wear of the grinding wheel, making it difficult to ensure accuracy and surface quality. Summary of the invention

[0004] In view of the shortcomings of the prior art mentioned above, the purpose of the present invention is to provide a photovoltaic back-grinding integrated fine grinding wheel and a preparation method thereof, so as to effectively solve the problems of poor self-sharpening, poor surface condition, high processing load, low processing accuracy, poor impact resistance of grinding wheels, and short lifespan of other traditional grinding wheels.

[0005] The present invention first provides a photovoltaic back-grinding integrated fine grinding wheel, which includes a base and an abrasive layer distributed circumferentially on the top of the outer end surface of the base, wherein the abrasive layer includes the following components in parts by weight: 18-38 parts of artificial polycrystalline diamond; 19-22 parts of auxiliary abrasive; 1.5-2 parts of lubricating additive; 5-12.5 parts of wear-resistant fiber; and 35-46 parts of resin powder.

[0006] The grinding wheel includes an abrasive layer and a substrate. A plurality of arc blocks are evenly distributed along the circumferential direction on the top of the outer end surface of the substrate. The arc blocks constitute the abrasive layer. There are gaps between the arc blocks. The width W of the gap is 2-4 mm. The thickness D of the arc blocks is 5-7 mm. The number of the arc blocks is 20-30.

[0007] Specifically, the substrate may be made of metal, and the substrate material includes any one of steel, aluminum alloy, titanium alloy, and the like.

[0008] Specifically, the artificial polycrystalline diamond has a particle size of 400-800#.

[0009] Specifically, the auxiliary abrasive is any one of SiC, iron oxide, aluminum oxide or chromium aluminum carbide or a combination of several of them.

[0010] Specifically, the lubricating additive is black graphite powder, MoS 2 Any one or a combination of two.

[0011] Specifically, the wear-resistant fiber is any one of reinforced glass fiber, carbon fiber, and calcium sulfate reinforced fiber, or a combination of several of them.

[0012] Specifically, the resin powder is any one of silicone, HDPE powder resin, polyvinyl butyral, phenolic resin powder or thermoplastic polyurethane powder, or a combination of several of them.

[0013] Specifically, the SiC is cubic green SiC, and the particle size of the auxiliary abrasive is 50-1200#.

[0014] Specifically, the black graphite powder and the MoS 2 The particle size of the chromium carbide aluminum is one particle size number lower than that of the artificial polycrystalline diamond, and the particle size of the chromium carbide aluminum is one particle size number coarser than that of the artificial polycrystalline diamond.

[0015] Specifically, the resin powder has a particle size of 5 to 100 μm.

[0016] The resin powder is any combination of two of silicone, HDPE powder resin, polyvinyl butyral ester, phenolic resin powder and thermoplastic polyurethane powder, and the mass ratio of the resin powders of any two combinations is 1:1-1:2.

[0017] Specifically, the wear-resistant fiber has an aspect ratio of no more than 20 and a length of less than 45 μm.

[0018] Another aspect of the present invention further provides a method for preparing a photovoltaic back-grinding integrated fine grinding wheel, the preparation method comprising the following steps: - S1: 18-38 parts of artificial polycrystalline diamond, 19-22 parts of auxiliary abrasive, 1.5-2 parts of lubricant, 5-12.5 parts of wear-resistant fiber and 35-46 parts of resin powder are mixed to obtain a mixture; - S2: forming and curing the mixed material to obtain an abrasive layer; - S3: Compounding the abrasive layer on a substrate to obtain the photovoltaic back-grinding integrated fine grinding wheel.

[0019] In step S1, the mixing includes a first mixing, a second mixing and a third mixing, and the mixing may include processes such as crushing, mixing, grinding, drying and screening.

[0020] In step S1, the first mixing may include mixing artificial polycrystalline diamond, auxiliary abrasive, lubricant and the wear-resistant fiber first, the first mixing includes adding an organic solvent, and the organic solvent is acetone or alcohol. The first mixing includes stirring in a centrifugal ultrasonic mixer, the ultrasonic time of the centrifugal ultrasonic mixer is 40-60 minutes, and the stirring time is not less than 1 hour. The first mixing also includes drying and screening, the drying temperature is 120-140°C, and the screening can be through a 50-200# sieve. After screening, the first mixture can be obtained; In step S1 , the second mixing includes mixing a plurality of resin powders.

[0021] In step S1, the second mixing includes processes such as crushing, grinding, drying and screening. Specifically, the crushing is performed by a pulverizer, the grinding is performed by a ball mill, and the drying is performed by an oven. The crushing and grinding can be performed at low temperatures to ensure the performance of the resin. The crushing and grinding temperatures can be -10°C-30°C, and the screening can be performed through a 100-200# sieve, so that the consistency of the particle size of the resin powder can be ensured. After the second mixing, a second mixed material is obtained.

[0022] In step S1, the third mixing may be mixing the second mixed material and the first mixed material. The third mixing includes mixing and sieving, the mixing is performed using a three-dimensional mixer, the mixing time is 40-60 minutes, and the third mixing also includes sieving through a 100-200# sieve, and the third mixed material can be obtained after sieving.

[0023] In step S2, the molding may be to put the third mixed material into a mold of a specified shape for molding, and the molding may be cold press molding. The temperature of the cold press molding is room temperature, that is, it can be satisfied without heating. The calculation method of the cold press molding pressure is: F = S (3-5), where F is the pressure and S is the cross-sectional area of ​​the arc block.

[0024] In step S2, the curing may be high temperature curing, and the curing may be achieved by using a double plate heating and pressurizing curing hot press. The curing temperature is 120-160°C, and the pressure of the hot press during curing may be 6-10 MPa. The high temperature curing pressure is calculated as follows: F = S (3-5), where F is the pressure and S is the cross-sectional area of ​​the arc block.

[0025] Specifically, in order to ensure the performance stability of the product, the curing process also includes exhaust and pressure relief during the continuous increase of the curing temperature. The exhaust and pressure relief can discharge the gas generated by the decomposition of the abrasive layer raw materials, such as the gas generated by the decomposition of the resin powder. The exhaust and pressure relief includes the process of discharging the gas in the mold cavity during the curing process. The heating rate of the curing temperature is 10-15°C / 5min. The exhaust and pressure relief includes 2-3 times of pressure relief when the curing temperature reaches 100°C. When the hot press is kept warm and pressurized for 20-60min under the condition of the curing temperature of 120-160°C, exhaust and pressure relief are performed again 4-5 times. A single exhaust and pressure relief takes 10 minutes, and the interval time is 5 minutes. After the curing is completed, the demolding post-processing can be carried out.

[0026] The abrasive layer is manufactured and cured using an integrated manufacturing method, that is, the cold pressing and high-temperature curing are performed in the same set of molds, so as to avoid foreign matter, dirt, and diamond contaminants on the surface of the product during the process of removing the molded blank. This method avoids possible contamination of the product during the manufacturing process, and this method avoids changes in product density caused by size differences between different molds. This method avoids possible contamination of the product during the manufacturing process and stabilizes the quality of the product.

[0027] In step S3, the compounding may be performed by a bonding process.

[0028] The present invention provides a photovoltaic back-grinding integrated fine grinding wheel and a preparation method thereof, which has the following beneficial effects: (1) Several arc blocks on the end face of the grinding wheel base are distributed along the ring, which is different from the circumferential distribution of traditional grinding wheels. The design of this product is conducive to the removal of debris and the smooth flow of coolant, reducing the grinding force during the processing process, which will indirectly improve the sharpness of the product and reduce scratches on the surface of the processed object.

[0029] The diamond design of this product is a sharp multi-edge shape, which is different from the traditional single crystal diamond. This is conducive to dispersing the heat and processing resistance generated by processing. This design improves the sharpness of the grinding wheel, effectively reduces the possibility of burns during processing, improves processing quality, and improves surface processing quality.

[0030] (2) This product is manufactured and cured using an integrated manufacturing method, that is, the cold pressing and high-temperature curing are carried out in the same set of molds. This method avoids possible contamination of the product during the manufacturing process and stabilizes the quality of the product.

[0031] (3) The abrasives used in the present invention are cubic SiC, iron oxide, aluminum oxide and chromium carbide aluminum, which act as abrasives during grinding and also serve as factors for sharpening the blade, thus promoting grinding. This will enable the grinding wheel to continuously sharpen itself during grinding, thus ensuring the sharpness of the grinding wheel and avoiding the situation in which the traditional grinding wheel is not sharp enough and may burn the processing object during grinding.

[0032] (4) The present invention uses black graphite powder, MoS 2 As a lubricating additive, a small amount can meet the lubrication performance requirements without affecting the overall strength of the grinding wheel. The performance of the product can effectively prevent burns on the workpiece surface.

[0033] (5) When processing silicon single crystals, traditional grinding wheels have a high wear ratio and a fast change in the grinding wheel profile. This change will cause uneven texture on the processed surface of the silicon single crystal rod and may also cause low processing dimensional accuracy. The addition of reinforced fiber reinforcement increases the retention of the product, so that the grinding wheel will not experience a rapid decrease in life due to processing and grinding, thereby affecting the processing size of the workpiece.

[0034] In summary, the Brinell hardness of the grinding wheel prepared by the present invention is HRB (50-60), and the elastic modulus of the grinding layer is (0.003-0.025) 10 5 MPa, the product is relatively brittle and at the same time low hardness and self-lubricating. This physical property is conducive to the processing of photovoltaic silicon crystal rod and wire materials, and can cope with complex grinding scenarios with high surface quality requirements. It can effectively solve the problems of poor self-sharpening of traditional grinding wheels, easy burning of workpieces, low processing accuracy, poor impact resistance of grinding wheels, and short life. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 Shown is a top view of the photovoltaic back-grinding integrated fine grinding wheel of the present invention.

[0036] Figure 2 Shown is a cross-sectional view of the photovoltaic back-grinding integrated fine grinding wheel of the present invention.

[0037] Figure 3 Shown is a cross-sectional view of the conventional grinding wheel structure in Comparative Example 1.

[0038] Figure 4 Shown is the SEM image of the abrasive layer prepared in Example 1.

[0039] Figure 5 Shown is a SEM image of the artificial polycrystalline diamond in the examples.

[0040] Figure 6 Shown is a SEM image of the wear-resistant calcium sulfate fiber in the examples.

[0041] Figure 7 The photo shows the photovoltaic silicon ingot being processed. DETAILED DESCRIPTION

[0042] See also Figures 1 to 7 .

[0043] like Figure 1 As shown, the grinding wheel includes an abrasive layer 1 and a base 2. The end surface of the base 2 is evenly distributed with a plurality of arc blocks along a ring shape. The arc blocks constitute the abrasive layer 1. The specific embodiments are as follows: like Figure 1 and Figure 2 As shown, the grinding wheel in the following embodiment includes an abrasive layer 1 and a base 2, a plurality of arc blocks are evenly distributed along the circumference of the top of one end surface of the base 2, and gaps 11 are formed between the arc blocks. A through hole 3 is opened in the middle of the base 2, and the arc blocks constitute the abrasive layer 1. The thickness D of the arc blocks is 6 mm, the number of the arc blocks is 24, and the width W of the gap 11 is 3 mm.

[0044] The specific embodiments are as follows:

[0045] Embodiment 1: The abrasive layer of this embodiment includes the following raw materials in parts by weight: 18 parts of artificial polycrystalline diamond (TOMEI diamond IRV-400#), 19 parts of cubic green SiC (Electro-Sensors SIC-600#), 1.5 parts of black graphite powder (Showa Denko Materials G-600#), 3 parts of chromium carbide aluminum (Alcoa C2Cr3-300#), 12.5 parts of carbon fiber (Toray T700: 5-10um), 23 parts of thermoplastic polyurethane powder (BAYER 9370A: 15-55um), and 23 parts of phenolic resin powder (DIALOK 939P: 80-100um).

[0046] That is, 18 parts of artificial polycrystalline diamond; 22 parts of auxiliary abrasive; 1.5 parts of lubricating additive; 12.5 parts of wear-resistant fiber; 46 parts of resin powder; The preparation steps of the above-mentioned grinding wheel are as follows: (1) Pour the artificial polycrystalline diamond, cubic green SiC, black graphite powder, chromium carbide aluminum, and carbon fiber in the formula into acetone or alcohol or other organic solution, stir evenly, centrifuge and ultrasonicate for 60 minutes, and dry at 140°C to obtain a mixture A; (2) The thermoplastic polyurethane powder and the phenolic resin powder are crushed with liquid nitrogen, ball-milled, dried at 123° C., and passed through a 120# sieve to obtain a mixture B; (3) Mixture A and mixture B are mixed using a three-dimensional mixer at a speed of 60 Hz for 25 min until they are evenly mixed to obtain mixture C; (4) Mixture C is placed in a cold pressing and high-temperature curing integrated mold for production. The cold pressing pressure is 4.5 MPa and the temperature is cold pressing at room temperature. During curing, the hot press pressure is 6 MPa and the temperature is raised to 100°C. The exhaust and pressure relief are performed twice, each time for 10 minutes. Then the curing is continued. The hot press is kept warm and pressurized at 140°C for 60 minutes. During the high-temperature curing process at 140°C, the exhaust and pressure relief are performed four times, each time for 10 minutes, and the interval time is 5 minutes. Finally, the arc block is removed from the mold.

[0047] (5) The arc block is subjected to sandblasting, bonding (bonding to the substrate), rough turning of the substrate, fine turning of the substrate, and fine grinding of the arc block. Finally, the finished grinding wheel is obtained after the quality inspection is passed.

[0048] The processing parameters and effects of the grinding wheel in this embodiment are shown in Table 1.

[0049] Table 1 Performance evaluation table of Example 1

[0050] Example 2: The abrasive layer of this example includes the following raw materials in parts by weight: 24 parts of artificial polycrystalline diamond (TOMEIdiamond IRV-600#), 14 parts of alumina (Alcoa AL2O3-800#), and 14 parts of MoS 2 (olibdenos y MetalesMOS-800#) 1.8 parts, SiC (Electro-Sensors SIC-800#) 5 parts, calcium sulfate fiber (BAYER CaSO4: 5-10um) 11 parts, HDPE powder resin (Dow HDPE: 20-45um) 19.2 parts, phenolic resin powder (DIALOK 939p: 80-100um) 25 parts.

[0051] That is, 24 parts of artificial polycrystalline diamond; 19 parts of auxiliary abrasive; 1.8 parts of lubricating additive; 11 parts of wear-resistant fiber; 44.2 parts of resin powder; The preparation steps of the above-mentioned grinding wheel are as follows: (1) Diamond, alumina, MoS 2 , SiC, and calcium sulfate fibers are poured into acetone, alcohol, or other organic solutions and stirred evenly, centrifuged and ultrasonicated for 60 minutes, and dried at 140°C to obtain a mixture A; (2) HDPE powder resin and phenolic resin powder are crushed with liquid nitrogen, ball-milled, dried at 100°C, and passed through a 200# sieve to obtain a mixture B; (3) Mixture A and mixture B are mixed using a three-dimensional mixer at a speed of 60 Hz for 1 hour until they are evenly mixed to obtain mixture C; (4) Mixture C is placed in a mold for cold pressing and high-temperature curing. The cold pressing pressure is 4.5 MPa and the temperature is cold pressing at room temperature. During high-temperature curing, the hot press gives a pressure of 8 MPa and exhausts and depressurizes twice when the temperature rises to 100°C. The single time is 10 minutes. Then continue to cure. The hot press is kept warm and pressurized at 130°C for 60 minutes. Exhaust and depressurize four times. The single exhaust and depressurization takes 10 minutes. The interval time is 5 minutes. Finally, the arc block is removed from the mold.

[0052] (5) The arc block is subjected to sandblasting, bonding (bonding to the substrate), rough turning of the substrate, fine turning of the substrate, and fine grinding of the arc block. Finally, the finished grinding wheel is obtained after the quality inspection is passed.

[0053] The photovoltaic silicon crystal rod was ground using the grinding wheel of this embodiment, and the processing parameters and effects are shown in Table 2.

[0054] Table 2 Performance evaluation table of Example 2

[0055] Embodiment 3: The abrasive layer of this embodiment includes the following raw materials in parts by weight: 38 parts of artificial polycrystalline diamond (TOMEI diamond IRV-800#), 12 parts of alumina (Alcoa AL2O3-1000#), and 12 parts of MoS 2 (olibdenos y Metales SA MOS-1000#) 2 parts, SiC (Electro-Sensors SIC-1000#) 8 parts, calcium sulfate fiber (Neelkanth Chemicals CaSO4: 3-10um) 5 parts, silicone (Dow SI: 20-45um) 20 parts, polyvinyl butyral (Butvar B76: 50-100um) 15 parts.

[0056] That is, 38 parts of artificial polycrystalline diamond; 20 parts of auxiliary abrasive; 2 parts of lubricating additive; 5 parts of wear-resistant fiber; 35 parts of resin powder; The preparation steps of the above-mentioned grinding wheel are as follows: (1) Diamond, alumina, MoS 2 , SiC, and calcium sulfate fibers are poured into alcohol and stirred evenly, centrifuged and ultrasonicated for 60 minutes, and dried at 140°C to obtain a mixture A; (2) crushing the organosilicon powder and polyvinyl butyral with liquid nitrogen, drying at 120°C, and passing through a 200# sieve to obtain a mixture B; (3) Mixture A and mixture B are mixed using a three-dimensional mixer at a speed of 60 Hz for 40 min until they are evenly mixed to obtain mixture C; (4) Mixture C is placed in a cold pressing and high-temperature curing integrated mold for production. The cold pressing pressure is 6 MPa and the temperature is cold pressing at room temperature. During high-temperature curing, the hot press gives a pressure of 10 MPa and exhausts the pressure twice when the temperature rises to 100°C for 10 minutes. Then continue to cure. The hot press is kept warm and pressurized at 130°C for 60 minutes. During the high-temperature curing process, exhaust and pressure relief are performed 4 times, of which a single exhaust and pressure relief takes 10 minutes, with an interval of 5 minutes. Finally, the arc block is removed from the mold.

[0057] (5) The arc block is subjected to sandblasting, bonding (bonding to the substrate), rough turning of the substrate, fine turning of the substrate, and fine grinding of the arc block. Finally, the finished grinding wheel is obtained after the quality inspection is passed.

[0058] The grinding wheel of this embodiment is used to grind photovoltaic silicon crystal rods on a vertical grinder. The processing parameters and effects are shown in Table 3.

[0059] Table 3 Performance evaluation table of Example 3

[0060] Comparative Example 1: like Figure 3 As shown, a conventional abrasive layer 1 is used to surround the outer circumference of the substrate and is distributed circumferentially in the grinding wheel structure. The abrasive layer ratio is the same as that in Example 1, the mixing method is the same as that in Example 1, and the same processing parameters are used to process photovoltaic silicon crystal rods.

[0061] Comparative Example 2: In comparative example 2, the base structure adopts end face arc blocks distributed along a ring shape, the abrasive layer ratio is the same as that in example 1, the abrasive layer is prepared by normal molding and curing method, and the exhaust pressure relief process is not used. The remaining process methods and abrasive treatment methods are the same as those in example 1.

[0062] Comparative Example 3: The base structure of Comparative Example 3 adopts end face arc blocks distributed along a ring shape, and the abrasive layer ratio is the same as that of Example 1, wherein 23 parts of thermoplastic polyurethane are replaced by phenolic resin powder, and the rest of the preparation method is the same as that of Example 1.

[0063] Table 4 Performance comparison table of comparative examples 1-3 and embodiment 1

[0064] The above results show that the use of evenly spaced arc blocks on the end face of the substrate is beneficial to improving the surface quality of the grinding wheel and reducing the occurrence of scratches and wear marks. The abrasive layer of the grinding wheel in Example 1 is distributed in a ring shape on the end face of the substrate by arranging a number of arc blocks, which can enhance the removal of debris and the smooth flow of coolant, reduce the grinding force during the processing process, indirectly improve the sharpness of the product and reduce the phenomenon of scratches on the surface of the processing object.

[0065] During the high-temperature curing process, an exhaust and pressure relief process is adopted. The physical properties of the product meet the requirements of the present invention. At the same time, the effect of the use of thermoplastic polyurethane can also be seen, which has a beneficial effect on increasing the life of the grinding wheel, improving the surface quality of the grinding wheel, and reducing the occurrence of scratches and wear marks.

[0066] Comparative Example 4: The processing substrate structure, abrasive layer ratio, and mixing method of Comparative Example 4 are the same as those of Example 2, wherein the artificial polycrystalline diamond is replaced by the common single crystal diamond, the particle size remains unchanged, and the processing technology is the same as that of Example 2.

[0067] Comparative Example 5: In Comparative Example 5, the processing substrate structure, abrasive layer ratio, and mixing method are the same as those in Example 2, wherein aluminum oxide is replaced by natural white corundum, the particle size remains unchanged, and the processing technology is the same as that in Example 2.

[0068] The natural white corundum model used in this comparative example is: Alcoa-natural white corundum W14.

[0069] Table 5 Performance comparison table of comparative examples 4-5 and embodiment 2

[0070] The above results show that the use of artificial polycrystalline diamond and alumina has a beneficial effect on improving the roughness of the grinding wheel and reducing the scratch rate and wear mark rate.

[0071] Comparative Example 6: Comparative Example 6 The processing substrate structure, abrasive layer ratio, and mixing method are the same as those in Example 3, wherein 2 parts of MoS 2 Replaced with chromium carbide aluminum, the processing technology is the same as Example 3.

[0072] Comparative Example 7: In Comparative Example 7, the processing substrate structure, abrasive layer ratio, and mixing method are the same as those in Example 3, wherein 5 parts of calcium sulfate fibers are removed, the grinding wheel density remains unchanged, and the processing technology is the same as that in Example 3.

[0073] Comparative Example 8: In Comparative Example 8, the processing substrate structure, abrasive layer ratio, and mixing method are the same as those in Example 3, wherein 5 parts of calcium sulfate fiber and 12 parts of aluminum oxide are removed, the grinding wheel density remains unchanged, and the processing technology is the same as that in Example 3.

[0074] Comparative Example 9: The processing substrate structure, abrasive layer ratio, and mixing method of Comparative Example 9 are the same as those of Example 3, wherein the molding and high-temperature curing method is changed to a split-type production method: different molds are used for cold pressing and high-temperature curing.

[0075] Table 6 Performance comparison table of comparative examples 6-9 and embodiment 3

[0076] The above results show that MoS 2 The addition of is beneficial to reduce the scratch and wear rate. This is because it has a relatively dense layer and has good anti-oxidation and self-lubricating properties when added in a small proportion, which can significantly reduce the friction coefficient and friction wear of the product during processing.

[0077] The addition of calcium sulfate fiber can greatly improve the shape retention and life of the grinding wheel, improve the impact resistance of the grinding wheel, and reduce the occurrence of scratches and wear marks caused by uneven grinding lines due to excessive consumption of the grinding wheel surface.

[0078] The molding and curing are made in one piece, that is, the cold pressing and high-temperature curing are carried out in the same set of molds, so as to avoid foreign matter, dirt and diamond contaminants on the surface of the product during the process of removing the molded blank. This method avoids possible contamination of the product during the manufacturing process; and this method avoids the change of product density caused by the size difference between different molds, so the density is more stable, and the quality of the product is stabilized.

[0079] The above embodiments are only illustrative of the principles and effects of the present invention, and are not intended to limit the present invention. When the embodiments give a numerical range, it should be understood that, unless otherwise specified in the present invention, the two endpoints of each numerical range and any numerical value between the two endpoints can be selected. Unless otherwise defined, all technical and scientific terms used in the present invention have the same meaning as those commonly understood by those skilled in the art. In addition to the specific methods, equipment, and materials used in the embodiments, according to the technical personnel of the present art's grasp of the prior art and the records of the present invention, any methods, equipment, and materials of the prior art similar or equivalent to the methods, equipment, and materials described in the embodiments of the present invention can also be used to implement the present invention. Anyone familiar with this technology can modify or change the above embodiments without violating the spirit and scope of the present invention. Therefore, all equivalent modifications or changes completed by those with ordinary knowledge in the art without departing from the spirit and technical ideas disclosed in the present invention should still be covered by the claims of the present invention.

Claims

1. A photovoltaic back-grinding integrated fine grinding wheel, characterized in that: The grinding wheel comprises a base body and an abrasive layer located on the top of the outer end surface of the base body and distributed in the circumferential direction. The abrasive layer is a plurality of arc-shaped blocks arranged at intervals. The abrasive layer comprises the following components in parts by weight: 18-38 parts of artificial polycrystalline diamond; Auxiliary abrasive 19-22 parts; 1.5-2 parts of lubricating additive; 5-12.5 parts of wear-resistant fiber; 35-46 parts of resin powder.

2. The photovoltaic back-grinding integrated fine grinding wheel according to claim 1, characterized in that: The artificial polycrystalline diamond has a particle size of 400-800#.

3. The photovoltaic back-grinding integrated fine grinding wheel according to claim 1, characterized in that: The auxiliary abrasive is any one or a combination of SiC, iron oxide, aluminum oxide or chromium aluminum carbide; And / or, the lubricating additive is any one of black graphite powder and MoS2 or a combination of both; And / or, the wear-resistant fiber is any one of reinforcing glass fiber, carbon fiber, and calcium sulfate reinforcing fiber, or a combination of several thereof; And / or, the resin powder is any one of or a combination of silicone, HDPE powder resin, polyvinyl butyral ester, phenolic resin powder or thermoplastic polyurethane powder.

4. The photovoltaic back-grinding integrated fine grinding wheel according to claim 3 is characterized in that: The SiC is cubic green SiC, and the particle size of the auxiliary abrasive is 50-1200#.

5. The photovoltaic back-grinding integrated fine grinding wheel according to claim 3, characterized in that: The particle size of the black graphite powder and the MoS2 is one particle size number lower than that of the artificial polycrystalline diamond, and the particle size of the chromium carbide aluminum is one particle size number coarser than that of the artificial polycrystalline diamond.

6. The photovoltaic back-grinding integrated fine grinding wheel according to claim 3, characterized in that: The resin powder has a particle size of 5-100 μm, and the resin powder is any combination of silicone, HDPE powder resin, polyvinyl butyral, phenolic resin powder and thermoplastic polyurethane powder, and the mass ratio of any two combinations of resin powders is 1:1-1:

2.

7. A method for preparing a photovoltaic back-grinding integrated fine grinding wheel, characterized in that: The preparation method comprises the following steps: - S1: 18-38 parts of artificial polycrystalline diamond, 19-22 parts of auxiliary abrasive, 1.5-2 parts of lubricant, 5-12.5 parts of wear-resistant fiber and 35-46 parts of resin powder are mixed to obtain a mixture; - S2: forming and curing the mixed material to obtain an abrasive layer; - S3: Compounding the abrasive layer on a substrate to obtain the photovoltaic back-grinding integrated fine grinding wheel; Wherein, the abrasive layer is distributed along the circumferential direction on the top of the outer end surface of the substrate, and the abrasive layer is a plurality of arc-shaped blocks arranged at intervals.

8. The method according to claim 7, characterized in that: The curing is performed by a hot press, and the curing includes: the hot press is kept warm and pressurized for 20-60 minutes under the conditions of a pressure of 6-10 MPa and a temperature of 120-160° C.

9. The method according to claim 8, characterized in that: The curing further includes exhausting and relieving pressure during the process of continuously rising curing temperature, wherein the exhausting and relieving pressure is to discharge the gas in the mold cavity.

10. The method according to claim 9, characterized in that: The heating rate of the curing temperature is 10-15°C / 5min. When the curing temperature reaches 100°C, the exhaust and pressure relief are performed 2-3 times. When the curing temperature is 120-160°C, the exhaust and pressure relief are performed again 4-5 times. The single exhaust and pressure relief time is 10min, and the exhaust and pressure relief interval time is 5min.

Citation Information

Patent Citations

  • Carbon fiber reinforced resin grinding wheel and preparation method thereof

    CN108621038A

  • Grinding element, grinding wheel and manufacturing method of semiconductor package using the same

    CN109262447A

  • Wafer Grinding Wheel

    CN111347344A

  • Ultra-precision grinding wheel and preparation method and application thereof

    CN112536733A

  • High-self-sharpening diamond grinding wheel and preparation method thereof

    CN116810662A

Cited By

  • Beta-SiC flat-top honing oilstone as well as preparation method and application thereof

    CN120116132A