Production equipment and preparation method of polyamide resin

By designing polyamide resin production equipment for screw barrels and screw units, the existing high-temperature nylon preparation process is solved, and efficient and flexible polymerization processes are achieved, and the product performance and production efficiency are improved.

CN118977394AActive Publication Date: 2024-11-19CATHAY BIOTECH INC +1

Patent Information

Application Number
CN202310526095.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-10
Publication Date
2024-11-19
Estimated Expiration
2043-05-10

AI Technical Summary

Technical Problem

The existing high-temperature nylon preparation process is low efficiency, long time, and inflexible, making it difficult to adjust quickly.

Method used

A polyamide resin production equipment including a screw barrel and a screw unit is designed. The screw unit is composed of a mandrel, the first, second and third screw components. Through the special design and combination of the screw components, the rapid melting of materials is achieved. Polymerization and devolatility improve production efficiency.

Benefits of technology

The preparation efficiency of high-temperature nylon is significantly improved, and the polymerization process is rapidly adjusted, the melting point and relative viscosity of the product are improved, the molecular weight distribution is narrower, the yellow index is reduced, and the overall product quality and production efficiency are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118977394A_ABST
    Figure CN118977394A_ABST
Patent Text Reader

Abstract

The invention discloses production equipment and a preparation method of polyamide resin. The polyamide resin production equipment comprises a screw cylinder and a screw unit, the screw unit is arranged in the accommodating cavity of the screw cylinder; the screw unit comprises a mandrel and a screw assembly arranged on the mandrel in a sleeving mode. The screw assemblies comprise the first screw assembly, the second screw assembly and the third screw assembly which are sequentially arranged in the material conveying direction. Wherein the first screw assembly is used for conveying materials; the second screw assembly is used for performing melt polymerization and devolatilization on the materials; the second screw assembly is repeatedly arranged n times, and n is larger than or equal to 2; the third screw assembly is used for extruding to obtain the polyamide resin. According to the production equipment of the polyamide resin, the screw elements are specially designed and combined, so that thermal degradation is effectively reduced, the melting point and the relative viscosity of the obtained polyamide resin are higher, the yellow index of a resin slice is lower, the molecular weight distribution is narrower, the production efficiency is higher, and the overall quality of the obtained product is better.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polymers, and in particular to a production device for polyamide resin and a preparation method thereof. Background Art

[0002] Normally, in industry, high-temperature nylon is prepared by salifying diamines with dibasic acids, and then the obtained nylon salt is introduced into a subsequent reactor for pressure holding, prepolymerization, post-polymerization, and final granulation to obtain the corresponding product. However, whether intermittent or continuous polymerization is used, the entire polymerization process usually lasts for several or even dozens of hours, and in this process, the intermediate products of each stage need to be transferred back and forth to different polymerizers, involving long pipelines and large storage and reaction equipment; at the same time, due to the long polymerization process, it is often difficult to get timely feedback when adjusting the process. When the polymerization is unstable or problems occur, it usually takes a long time to obtain a stable product again. In summary, the existing high-temperature nylon preparation process is inefficient, takes a long time, and is relatively inflexible when adjusting the process.

[0003] Screw extruders are widely used in polymer modification and can quickly adjust the process. They have been widely used in polymer plasticization, reinforcement, and compounding. In recent years, many patents have been published on the use of screw extruders for polymerization. However, there are few patents and literature reports on the direct preparation of high-temperature nylon using screws. At the same time, due to the high melting point of high-temperature nylon, when using screw extrusion, it will face problems such as thermal degradation caused by excessive temperature. In addition, the type and combination of screw elements in the screw extruder have a significant impact on the mixing, polymerization, and devolatilization of the extruder, and directly affect the molecular weight and viscosity of the product. Therefore, in the preparation process of high-temperature nylon, there are high requirements for the configuration and combination of screw elements, devolatilization, and temperature control systems, and special designs are required. Overall, the direct preparation of high-temperature nylon using a screw extruder has high technical barriers.

[0004] In view of this, there is an urgent need to provide a screw device and preparation method that can not only ensure that the high-temperature nylon product obtained has better performance than the existing technology, but also greatly improve the efficiency of preparing high-temperature nylon. At the same time, it can realize timely and rapid adjustment of the polymerization process to better adapt to the production of high-temperature nylon. Summary of the invention

[0005] The present invention provides a polyamide resin production device and a preparation method thereof to solve the defects of long polymerization time, low efficiency and inflexible process in the preparation process of high-temperature nylon (ie, high-temperature resistant polyamide resin) in the prior art.

[0006] The present invention solves the above technical problems through the following technical solutions.

[0007] One of the technical solutions of the present invention is: a polyamide resin production device, which includes a screw barrel and a screw unit; the screw unit is arranged in the accommodating cavity of the screw barrel;

[0008] The screw unit comprises a core shaft and a screw assembly sleeved on the core shaft;

[0009] The screw assembly comprises a first screw assembly, a second screw assembly and a third screw assembly which are sequentially arranged along the material conveying direction;

[0010] Wherein, the first screw assembly is used for material transportation;

[0011] Wherein, the second screw assembly is used to melt-polymerize and devolatilize the material; the second screw assembly is repeated n times, n≥2;

[0012] The second screw assembly includes a first group of elements and a second group of elements arranged in sequence along the material conveying direction;

[0013] The first set of elements includes a forward thread element, an engagement block and a reverse thread element arranged in sequence, and is used to make the material undergo a polymerization reaction;

[0014] The second set of elements includes threaded elements for devolatilizing the polymer;

[0015] Wherein, the third screw assembly is used for extrusion to obtain polyamide resin.

[0016] In the present invention, the screw barrel can be conventional in the art, generally composed of several barrel sections connected in series; preferably including 6 to 30 barrel sections; more preferably including 6 to 16 barrel sections; for example, 10 barrel sections. According to the conventional art, each barrel can be equipped with an independent temperature control and heating system.

[0017] In the present invention, preferably, the polyamide resin production equipment comprises at least two screw units rotating in the same direction. More preferably, the mandrels of any two screw units and the screw assemblies sleeved on the mandrels are completely identical.

[0018] In the present invention, the aspect ratio of the mandrel may be (20-68):1; preferably (40-60):1; more preferably (45-55):1; and further preferably 48:1.

[0019] The diameter of the mandrel may be 20 to 95 mm, preferably 35 to 50 mm.

[0020] In the present invention, according to the conventional art, the core shaft can be fixedly connected to a screw assembly sleeved on the core shaft, so as to prevent any relative movement between the screw core shaft and the screw assembly.

[0021] In the present invention, the first screw assembly may include a forward thread element and a reverse thread element sequentially arranged along the material conveying direction.

[0022] The number of the forward thread elements may be conventional in the art, such as 1 to 10, preferably 2 to 8, and more preferably 3 to 6. The number of the reverse thread elements may be conventional in the art, such as 1 to 10, preferably 2 to 8, and more preferably 3 to 6.

[0023] Preferably, the first screw assembly is composed of more than one forward thread element and more than one reverse thread element. For example, the first screw assembly is composed of 4 forward thread elements and 4 reverse thread elements.

[0024] Wherein, the positive thread element may be a large-lead positive thread element. The lead of the positive thread element may be 1D to 2.5D. The lead of the reverse thread element may be 1D to 2D.

[0025] In the present invention, the first screw assembly and its corresponding plurality of barrel sections can be understood as a feeding and conveying system, and the feeding and conveying system is preferably used for rapid melting and conveying of raw materials.

[0026] The first screw assembly can generally correspond to more than 2 sections of the barrel.

[0027] Preferably, a main feeding port is provided at the upper end of the first cylinder of the feeding and conveying system, and is connected to the main feeding system through the main feeding port.

[0028] Preferably, an auxiliary feeding port is provided at the upper end of the second cylinder of the feeding and conveying system, and is connected to the auxiliary feeding system through the auxiliary feeding port.

[0029] When the feeding and conveying system includes more than three cylinders, optionally, an auxiliary agent feeding port is provided at the upper end of the third cylinder of the feeding and conveying system, and is connected to the auxiliary agent feeding system through the auxiliary agent feeding port.

[0030] In the present invention, in the first group of elements of the second screw assembly, the number of the forward thread elements and the reverse thread elements can be independently 1 to 5, preferably 2 to 4. The number of the meshing blocks is preferably 2 or more.

[0031] Preferably, the first group of elements of the second screw assembly includes two forward thread elements, two engaging blocks and two reverse thread elements which are sequentially arranged along the material conveying direction.

[0032] In the first group of elements of the second screw assembly, the positive thread element may be a small lead thread element. The lead of the positive thread element may be 0.1D to 0.5D, for example, 8 mm. The length of the positive thread element may be 4 to 60 mm, preferably 8 mm.

[0033] In the first group of elements of the second screw assembly, the lead of the reverse thread element may be 0.5D to 2D, preferably 0.57D to 1D, for example 20 mm. The length of the reverse thread element may be 10 to 120 mm, preferably 20 mm.

[0034] In the first group of elements of the second screw assembly, the meshing block can be conventional in the art, such as a forward meshing block or a reverse meshing block. When the number of the meshing blocks is 2, preferably one forward meshing block and one reverse meshing block are included.

[0035] The length of the engagement block may be 20 to 120 mm, preferably 56 mm.

[0036] The staggered angle between the adjacent end faces of the meshing blocks can be conventional in the art, generally referring to the angle of rotation between the adjacent end faces of the meshing blocks with the axis of the meshing disc element as the center, preferably 45°, 60° or 90°. The meshing disc element is a composite element composed of at least two separate meshing blocks.

[0037] In the present invention, the first group of elements of the second screw assembly and its corresponding barrel can be understood as a polymerization system, which is preferably used to fully polymerize the raw materials.

[0038] Preferably, the cylinder corresponding to the first group of elements of the second screw assembly is a closed cylinder for maintaining pressure.

[0039] In the present invention, the second group of elements of the second screw assembly may include a forward thread element. The forward thread element may be a conventional slotted thread element in the art, which is used to increase the material distribution area and facilitate devolatilization. Generally, the slotted thread element may have grooves of different shapes such as rectangular grooves on its thread.

[0040] The number of the forward thread elements may be 1 to 6, preferably 2 to 4.

[0041] Wherein, the lead of the forward thread element may be 1.5D to 2.5D.

[0042] In the present invention, the second group of elements of the second screw assembly and the corresponding barrel can be understood as a devolatilization system.

[0043] Preferably, a devolatilization port is provided at the upper end of the barrel corresponding to the second group of elements of the second screw assembly, which is used to discharge small molecular by-products, increase the molecular weight, and increase the viscosity of the polymer.

[0044] The devolatilization port can be directly connected to the atmosphere for natural devolatilization. Preferably, the devolatilization port can be provided with a vacuum device for vacuum devolatilization.

[0045] In the present invention, n is preferably 3 to 20, more preferably 3 to 8, further preferably 3 to 5, for example 3, for obtaining a polyamide resin with a suitable molecular weight and relative viscosity.

[0046] In the present invention, the third screw assembly may include a reverse thread element to establish a die head pressure to extrude the material smoothly.

[0047] The number of the reverse thread elements may be 5 to 15, preferably 6 to 12.

[0048] Wherein, the reverse thread element may be a small lead thread element. The lead of the reverse thread element may be 0.1D to 0.5D.

[0049] In the present invention, the third screw assembly and its corresponding plurality of barrel sections can be understood as an extrusion system.

[0050] In the present invention, the forward thread element can be a conventional element in the art that rotates in the direction of rotation of the conveying screw, and the shape of its screw groove can be rectangular; it is used for material conveying. It is generally selected from any one of a forward single-start thread element, a forward double-start thread element, a forward thread element transitioning from single-start to double-start, a forward thread element transitioning from double-start to single-start, and a forward three-start thread element, preferably a forward double-start thread element.

[0051] In the present invention, the reverse threaded element may be a conventional element in the art that rotates in the opposite direction of the conveying screw, and is similar in shape to the forward threaded element, and the spiral direction of the screw groove is opposite to that of the forward threaded element. It is generally selected from any one of a reverse single-start threaded element, a reverse double-start threaded element, a reverse threaded element transitioning from single-start to double-start, a reverse threaded element transitioning from double-start to single-start, and a reverse three-start threaded element, preferably a reverse double-start threaded element.

[0052] In the present invention, those skilled in the art may understand that D is the conventional major diameter (outer diameter) of the thread in the art.

[0053] Wherein, D can be independently 5 to 60 mm, preferably 10 to 40 mm.

[0054] In the present invention, the production equipment of the polyamide resin can generally be understood as a screw extruder, such as a twin-screw extruder. According to the conventional art, the production equipment of the polyamide resin can also include a drive motor, a coupling and a gear box connected in sequence at the front end of the screw extruder, and an extrusion pelletizing system arranged at the rear end of the screw extruder.

[0055] In the present invention, preferably, the temperature of the polyamide resin production equipment is set as follows: 120-300°C for the feeding and conveying system, 240-330°C for the polymerization system, 250-330°C for the devolatilization system, and 260-320°C for the extrusion system; this is used to prevent side reactions such as the inability to melt and convey materials due to too low a temperature and thermal degradation of materials during extrusion due to too high a temperature.

[0056] In the present invention, the screw speed of the polyamide resin production equipment can be 30-500rpm, preferably 60-500rpm, more preferably 60-200rpm. The residence time of the material in the polyamide resin production equipment can be 10s-30min, preferably 10s-15min, more preferably 1min-15min.

[0057] Preferably, the screw speed of the polyamide resin production equipment is 60 to 500 rpm, and the residence time of the material in the polyamide resin production equipment is 10 s to 15 min; this can effectively avoid the problem of low output when the screw speed is slow; and the problem that the material stays in the screw equipment for too long due to too slow a speed, which may cause thermal degradation at high temperatures.

[0058] More preferably, the screw speed of the polyamide resin production equipment is 60 to 200 rpm, and the residence time of the material in the polyamide resin production equipment is 1 min to 15 min; to avoid the problem that increasing the speed can increase the output per unit time, but the residence time of the material in the screw equipment is also greatly shortened, resulting in a lower viscosity of the final product.

[0059] The second technical solution of the present invention is: a method for preparing a polyamide resin, which adopts the production equipment of the polyamide resin as mentioned above.

[0060] In the present invention, the preparation method of the polyamide resin may include the following steps: adding diamine and dibasic acid, or nylon salt prepared from diamine and dibasic acid, into the production equipment of the polyamide resin, and after conveying, polymerizing and devolatilizing, extruding to obtain the polyamide resin; the number of polymerization and devolatilization is ≥2.

[0061] The diamine can be selected from diamines having 2 to 18 carbon atoms.

[0062] The dibasic acid may include dibasic acid A1 and dibasic acid A2; the dibasic acid A1 is selected from aromatic dicarboxylic acids and their derivatives, and the dibasic acid A2 is selected from aliphatic dicarboxylic acids having 2 to 18 carbon atoms.

[0063] In the present invention, the diamine includes one or more of 1,4-butanediamine, 1,5-pentanediamine, 1,6-hexanediamine, 1,8-octanediamine, 1,9-nonanediamine, 1,10-decanediamine, 1,11-undecanediamine, 1,12-dodecanediamine, 1,13-tridecanediamine and 1,14-tetradecanediamine; preferably 1,5-pentanediamine, or 1,5-pentanediamine and 1,10-decanediamine, or 1,5-pentanediamine and 1,12-diaminododecane.

[0064] In the present invention, the dibasic acid A1 includes terephthalic acid and its derivatives and / or isophthalic acid and its derivatives. Among them, the terephthalic acid and its derivatives preferably include terephthalic acid.

[0065] In the present invention, the dibasic acid A2 includes one or more of adipic acid, 1,8-octanedioic acid, 1,10-decanedioic acid, 1,11-undecanedioic acid, 1,12-dodecanedioic acid, 1,13-tridecanedioic acid, 1,14-tetradecanedioic acid and 1,16-hexadecanedioic acid, and preferably includes adipic acid. The adipic acid is preferably 1,6-hexanedioic acid.

[0066] In the present invention, preferably, the dibasic acid comprises terephthalic acid and / or 1,6-hexanedioic acid, preferably terephthalic acid and 1,6-hexanedioic acid.

[0067] In the present invention, the molar ratio of the dibasic acid to the diamine may be 1:(0.85-1.2), preferably 1:(0.95-1.15). Those skilled in the art will understand that the dibasic acid in the "molar ratio of the dibasic acid to the diamine" refers to dibasic acid A1 and dibasic acid A2.

[0068] In the present invention, the nylon salt may include nylon salt B1 and nylon salt B2.

[0069] The nylon salt B1 can be generally prepared from the diamine and the dibasic acid A1, for example, PA5T salt prepared from 1,5-pentanediamine and terephthalic acid or its derivatives, or PA10T salt prepared from 1,10-pentanediamine and terephthalic acid or its derivatives, or PA12T salt prepared from 1,12-dodecanediamine and terephthalic acid or its derivatives.

[0070] The nylon salt B2 can generally be prepared from a diamine and a dibasic acid A2, for example, a PA56 salt prepared from 1,5-pentanediamine and 1,6-hexanoic acid.

[0071] Preferably, the molar ratio of the nylon salt B1 to the nylon salt B2 is (30-90):(70-10).

[0072] In the present invention, the nylon salt preferably includes one or more of 5T salt, 56 salt, 10T salt and 12T salt; more preferably, 5T salt and 56 salt, or 10T salt and 56 salt, or 12T salt and 56 salt.

[0073] Wherein, when the nylon salt is 5T salt and 56 salt, the molar ratio of the 5T salt to the 56 salt may be (30-70):(70-30), preferably (40-70):(60-30), for example 51:49 or 56:44.

[0074] When the nylon salt is 10T salt and 56 salt, the molar ratio of the 10T salt to the 56 salt may be (90-50):(10-50), preferably (90-70):(10-30), and more preferably 86:14.

[0075] When the nylon salt is 12T salt and 56 salt, the molar ratio of the 12T salt to the 56 salt may be (90-60):(10-40), preferably (90-70):(10-30), and more preferably 82:18.

[0076] In the present invention, preferably, a catalyst and / or an antioxidant are added into the polyamide resin production equipment together with the "diamine and dibasic acid" or the "nylon salt prepared from diamine and dibasic acid".

[0077] Among them, the catalyst can be conventional in the art, such as phosphoric acid compounds, phosphoric acid metal salts, preferably one or more of phosphoric acid, phosphorous acid, hypophosphorous acid, phenyl hypophosphorous acid, phosphoric anhydride, tetrapolyphosphoric acid, pyrophosphoric acid, trimetaphosphoric acid, phosphorus pentachloride, triphenyl phosphite, ammonium hypophosphite, sodium hypophosphite, calcium hypophosphite, sodium hypophosphite, calcium hypophosphite and H10, preferably one or more of phosphoric anhydride, pyrophosphoric acid, triphenyl phosphite, ammonium hypophosphite, sodium hypophosphite, calcium hypophosphite, sodium hypophosphite, calcium hypophosphite and H10.

[0078] Among them, the antioxidant can be conventional in the art, such as one or more of N,N′-bis-(3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionyl)hexanediamine, tris[2,4-di-tert-butylphenyl]phosphite, tris[2,4-di-tert-butylphenyl]phosphite, pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate and β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate octadecyl alcohol ester.

[0079] The amount of the catalyst and / or the antioxidant added can be conventional in the art, for example, 10 to 10000 ppm, preferably 50 to 6000 ppm. The amount of the catalyst and / or the antioxidant added can be understood as the mass percentage of the amount of the catalyst and / or the antioxidant added to the "sum of the mass of all diamines and dibasic acids" or the "sum of the mass of all nylon salts". According to the convention in the art, the unit ppm can represent the mass percentage, 100 ppm = 0.01%.

[0080] In the present invention, the screw speed of the screw extruder may be 30 to 500 rpm, preferably 60 to 500 rpm, more preferably 120 to 200 rpm, further preferably 140 to 160 rpm, for example 150 rpm.

[0081] Preferably, the residence time of the diamine and dibasic acid, or the nylon salt prepared from the diamine and dibasic acid, in the screw is 10s to 30min, preferably 1min to 15min, more preferably 3min to 5min, for example 3min10s, 3min25s, 3min40s or 4min30s.

[0082] When the catalyst and / or the antioxidant are added into the screw extruder together with the "diamine and dibasic acid" or the "nylon salt made from diamine and dibasic acid", the residence time in the screw is as described above.

[0083] In the present invention, during the conveying process, the material melts; the melting temperature may be 120-350°C, preferably 200-330°C, more preferably 250-325°C, for example 260°C.

[0084] In the present invention, the polymerization temperature may be 200 to 350°C, preferably 240 to 330°C, more preferably 295 to 320°C, and further preferably 300 to 310°C.

[0085] In the present invention, the devolatilization temperature may be 220-350°C, preferably 250-330°C, more preferably 295-325°C, further preferably 298-320°C, for example 305-310°C.

[0086] In the present invention, the devolatilization may generally be vacuum devolatilization. The vacuum degree of the vacuum devolatilization may be -0.095 to 0 MPa, preferably -0.09 to 0 MPa, for example -0.09 MPa.

[0087] In the present invention, the extrusion temperature may be 220 to 350°C, preferably 240 to 320°C, more preferably 290 to 310°C, and further preferably 300 to 305°C.

[0088] In the present invention, after the extrusion, a pelletizing step is generally included.

[0089] In the present invention, the polyamide resin can be obtained by adopting the above-mentioned preparation method of the polyamide resin.

[0090] The melting point of the polyamide resin may be 260 to 330°C, preferably 280 to 320°C.

[0091] The relative viscosity of the polyamide resin may be 1.5 to 3.5, preferably 1.8 to 2.8.

[0092] The yellowness index (YI) of the polyamide resin may be 1 to 20, preferably 1 to 10, more preferably 1 to 5, and further preferably 1 to 2.5.

[0093] The molecular weight distribution (PDI) of the polyamide resin may be 1 to 3.2, preferably 1.5 to 2.6, and more preferably 1.5 to 2.

[0094] On the basis of being in accordance with the common sense in the art, the above-mentioned preferred conditions can be arbitrarily combined to obtain the preferred embodiments of the present invention.

[0095] The reagents and raw materials used in the present invention are commercially available.

[0096] The positive and progressive effects of the present invention are:

[0097] (1) The polyamide resin production equipment provided by the present invention effectively reduces the occurrence of thermal degradation through the special design and combination of screw elements. The obtained polyamide resin has a higher melting point and relative viscosity, a lower yellow index of resin chips, a narrower molecular weight distribution, higher production efficiency, and better product quality overall.

[0098] (2) The reaction process of the polyamide resin production method provided by the present invention can be better controlled, the reaction efficiency is higher, the yield is significantly increased, and the mechanical properties of the polyamide resin finally obtained are better than those of the polyamide resin product prepared by conventional processes. BRIEF DESCRIPTION OF THE DRAWINGS

[0099] Figure 1 Schematic diagram of the structure of the production equipment of polyamide resin in Examples 1 to 9.

[0100] Reference numerals:

[0101] First cylinder 1

[0102] Main feeding port 11

[0103] Second cylinder 2

[0104] Auxiliary feeding port 21

[0105] The third cylinder 3

[0106] Additive feeding port 31

[0107] First positive thread element 121

[0108] First reverse threaded element 122

[0109] Fourth cylinder 4

[0110] The second positive thread element 41

[0111] The first positive engagement block 42

[0112] First reverse engagement block 43

[0113] Second counter threaded element 44

[0114] Fifth cylinder 5

[0115] The third positive thread element 51

[0116] First devolatilization port 52

[0117] Sixth cylinder 6

[0118] Fourth positive thread element 61

[0119] The second positive engagement block 62

[0120] Second reverse engagement block 63

[0121] The third reverse threaded element 64

[0122] Seventh cylinder 7

[0123] Fifth positive thread element 71

[0124] Second devolatilization port 72

[0125] Eighth cylinder 8

[0126] Sixth positive thread element 81

[0127] The third positive engagement block 82

[0128] The third reverse engagement block 83

[0129] Fourth reverse threaded element 84

[0130] Ninth cylinder 9

[0131] Seventh positive thread element 91

[0132] The third devolatilization port 92

[0133] Tenth cylinder 10

[0134] Fifth reverse thread element 101 DETAILED DESCRIPTION

[0135] The present invention is further described below by way of examples, but the present invention is not limited to the scope of the examples. The experimental methods in the following examples without specifying specific conditions are carried out according to conventional methods and conditions, or selected according to the product specifications.

[0136] The diamines, dibasic acids, additives (catalysts and antioxidants) and the like in the following examples are all general products and can be purchased from the market.

[0137] In the following examples, the preparation method of nylon salt specifically includes the following steps: putting diamine, dibasic acid and deionized water into a 10L reactor, setting the reactor temperature, reacting for 3 hours under nitrogen protection, and then centrifuging, filtering and drying.

[0138] Nylon salt preparation method:

[0139] Preparation method of PA5T salt: 1287g of 1,5-pentanediamine, 2076g of terephthalic acid and 3400g of deionized water are put into a 10L reactor, the reactor temperature is set to 80°C, and the reaction is carried out under nitrogen protection for 3 hours, followed by centrifugal filtration and drying to obtain PA5T salt.

[0140] Preparation method of PA56 salt: put 1450g 1,5-pentanediamine, 2045g 1,6-adipic acid and 3500g deionized water into a 10L reactor, set the reactor temperature to 60°C, react for 3h under nitrogen protection, then centrifuge and filter to dry to obtain.

[0141] Preparation method of PA10T salt: put 1757g 1,10-decanediamine, 1694g terephthalic acid and 4500g deionized water into a 10L reactor, set the reactor temperature to 90°C, react for 3h under nitrogen protection, then centrifuge and filter to dry, and the product can be obtained.

[0142] Preparation method of PA12T salt: 1903g 1,12-dodecanediamine, 1578g terephthalic acid and 4700g deionized water are put into a 10L reactor, the reactor temperature is set to 90°C, react for 3h under nitrogen protection, and then centrifuge and filter to dry to obtain.

[0143] Examples 1 to 9 use Figure 1 The polyamide resin production equipment shown is a twin-screw extruder, which includes: a barrel composed of 10 barrel sections and two screw units rotating in the same direction; the two screw units rotating in the same direction are both arranged in the containing cavity of the barrel;

[0144] The two screw units rotating in the same direction each independently include a core shaft, and a first screw assembly sleeved on the core shaft and arranged in sequence along the material conveying direction, a second screw assembly and a third screw assembly which are repeatedly arranged three times;

[0145] The core shaft has a diameter of 35 mm and a length-to-diameter ratio of 48:1, which can increase the residence time of the material in the screw, thereby increasing the vacuum time of the material in the screw and ultimately achieving a better overall viscosity-enhancing effect.

[0146] In the screw extruder, the feeding and conveying system comprises: a first screw assembly and its corresponding first barrel 1, second barrel 2 and third barrel 3;

[0147] Among them, the upper end of the first cylinder 1 is provided with a main feeding port 11, and is connected to the main feeding system through the main feeding port 11; the upper end of the second cylinder 2 is provided with an auxiliary feeding port 21, and is connected to the auxiliary feeding system through the auxiliary feeding port 21; the upper end of the third cylinder 3 is provided with an auxiliary agent feeding port 31, and is connected to the auxiliary agent feeding system through the auxiliary agent feeding port 31.

[0148] The first screw assembly is composed of a first forward thread element 121 and a first reverse thread element 122 in sequence, and is used for rapidly melting and conveying raw materials;

[0149] Among them, the first forward thread element 121 includes 4 forward thread elements (forward double-start thread elements); the lead of any forward thread element is 70mm (2D) and the length is 70mm; the first reverse thread element 122 includes 4 reverse thread elements (reverse double-start thread elements); the lead of any reverse thread element is 50mm (1.42D) and the length is 50mm.

[0150] In the screw extruder, the first polymerization system comprises: a first group of elements of the second screw assembly and its corresponding fourth barrel 4;

[0151] The first group of elements of the second screw assembly includes: a second forward thread element 41, a first forward meshing block 42, a first reverse meshing block 43 and a second reverse thread element 44, which are sequentially composed to enable the raw materials to be fully polymerized;

[0152] The second forward thread element 41 includes two forward thread elements (forward double-start thread elements); the lead of any one of the forward thread elements is 8 mm (0.23D) and the length is 8 mm; the staggered angle of adjacent engagement blocks is 60° and the length is 56 mm; the second reverse thread element 44 includes two reverse thread elements (reverse double-start thread elements); the lead of any one of the reverse thread elements is 20 mm (0.57D) and the length is 20 mm;

[0153] The fourth cylinder 4 is a closed cylinder to maintain pressure.

[0154] In the screw extruder, the first devolatilization system comprises: a second group of elements of the second screw assembly and a corresponding fifth barrel 5;

[0155] Wherein, the second group of elements of the second screw assembly includes: a third forward thread element 51;

[0156] The third positive thread element 51 is composed of two positive thread elements (slotted thread elements), which can be used to increase the material distribution area and facilitate the devolatilization; the lead of any positive thread element is 85 mm (2.43D) and the length is 85 mm;

[0157] The fifth cylinder 5 is provided with a first devolatilization port 52 , and the first devolatilization port 52 is provided with a vacuum device for vacuum devolatilization and discharge of small molecular by-products.

[0158] In the screw extruder, the second polymerization system comprises: a third set of elements of the second screw assembly and its corresponding sixth barrel 6;

[0159] The third group of elements of the second screw assembly includes: a fourth forward thread element 61, a second forward meshing block 62, a second reverse meshing block 63 and a third reverse thread element 64, which are sequentially composed to enable the raw material to be fully polymerized;

[0160] The fourth forward thread element 61 includes two forward thread elements (forward double-start thread elements); the lead of any one of the forward thread elements is 8 mm (0.23D) and the length is 8 mm; the staggered angle of adjacent meshing blocks is 60° and the length is 56 mm; the third reverse thread element 64 includes two reverse thread elements (reverse double-start thread elements); the lead of any one of the reverse thread elements is 20 mm (0.57D) and the length is 20 mm;

[0161] The sixth cylinder 6 is a closed cylinder to maintain pressure.

[0162] In the screw extruder, the second devolatilization system comprises: a fourth group of elements of the second screw assembly and a corresponding seventh barrel 7;

[0163] Wherein, the fourth group of elements of the second screw assembly includes: a fifth forward thread element 71;

[0164] The fifth positive thread element 71 is composed of two positive thread elements (slotted thread elements), which can be used to increase the material distribution area and facilitate the devolatilization; the lead of any positive thread element is 85mm (2.43D) and the length is 85mm;

[0165] The seventh cylinder 7 is provided with a second devolatilization port 72, and the second devolatilization port 72 is provided with a vacuum device for vacuum devolatilization and discharge of small molecular by-products.

[0166] In the screw extruder, the third polymerization system comprises: a fifth group of elements of the second screw assembly and its corresponding eighth barrel 8;

[0167] The fifth set of elements of the second screw assembly includes: a sixth forward thread element 81, a third forward meshing block 82, a third reverse meshing block 83 and a fourth reverse thread element 84, which are sequentially composed to enable the raw materials to be fully polymerized;

[0168] The sixth forward thread element 81 includes two forward thread elements (forward double-start thread elements); the lead of any one of the forward thread elements is 8 mm (0.23D) and the length is 8 mm; the staggered angle of adjacent meshing blocks is 60° and the length is 56 mm; the fourth reverse thread element 84 includes two reverse thread elements (reverse double-start thread elements); the lead of any one of the reverse thread elements is 20 mm (0.57D) and the length is 20 mm;

[0169] Among them, the eighth cylinder 8 is a closed cylinder to maintain pressure.

[0170] In the screw extruder, the third devolatilization system comprises: a sixth group of elements of the second screw assembly and a corresponding ninth barrel 9;

[0171] Wherein, the sixth group of elements of the second screw assembly includes: a seventh forward thread element 91;

[0172] The seventh positive thread element 91 is composed of two positive thread elements (slotted thread elements), which can be used to increase the material distribution area and facilitate the devolatilization; the lead of any positive thread element is 85mm (2.43D) and the length is 85mm;

[0173] The ninth cylinder 9 is provided with a third devolatilization port 92 , and the third devolatilization port 92 is provided with a vacuum device for vacuum devolatilization and discharge of small molecular by-products.

[0174] In the screw extruder, the extrusion system comprises: a third screw assembly and its corresponding tenth barrel 10;

[0175] Among them, the third screw assembly includes the fifth reverse thread element 101, which is composed of 10 reverse thread elements (reverse double-head thread elements) and can be used to establish the head pressure to extrude the material smoothly; the lead of any reverse thread element is 14mm (0.4D) and the length is 14mm.

[0176] Example 1

[0177] 2624 g of 5T salt, 2526 g of 56 salt (5T / 56 molar ratio 51 / 49), 1.5 g of sodium hypophosphite, and 5 g of tris[2,4-di-tert-butylphenyl]phosphite were added to a twin-screw extruder, and the temperatures of the feeding and conveying section, the polymerization section, the devolatilization section, and the extrusion section were set to 250°C, 310°C, 310°C, and 305°C, and the extruder speed was set to 140 rpm, the vacuum degree of the devolatilization section was set to -0.09 MPa, the residence time was 3 min 40 s, and the extrudate was extruded through a die, pulled, cooled, and pelletized to obtain the corresponding product.

[0178] Example 2

[0179] The same twin-screw equipment, feed ratio and process as those in Example 1 were used, except that a dibasic acid and a diamine combination were used for preparation. The feed conditions were as follows: 1972 g of 1,5-pentanediamine, 1624 g of terephthalic acid, and 1369 g of 1,6-hexanediol, wherein the molar ratio of the dibasic acid to the diamine was 1:1.009.

[0180] Example 3

[0181] The same twin-screw equipment, vacuum degree of the devolatilization section and granulation method as in Example 1 were used, except that the 5T / 56 molar ratio was 56:44, and the feeding conditions were as follows: 2871 g of 5T salt, 2079 g of 56 salt, 1.5 g of sodium hypophosphite, 7.5 g of tris[2,4-di-tert-butylphenyl]phosphite, the temperature of the extruder feeding and conveying section was 250°C, the polymerization section was 320°C, the devolatilization section was 320°C, the extrusion section was 310°C, the rotation speed was 160 rpm, and the residence time was 3 min 10 s.

[0182] Example 4

[0183] The same twin-screw equipment, feed ratio and process as those in Example 3 were used, except that a dibasic acid and a diamine combination were used for preparation. The feed conditions were as follows: 1960 g of 1,5-pentanediamine, 1777 g of terephthalic acid, and 1223 g of adipic acid, wherein the molar ratio of the dibasic acid to the diamine was 1:1.007.

[0184] Example 5

[0185] The same twin-screw equipment as in Example 1 was used, except that the 10T / 56 molar ratio was 86:14, and the feeding conditions were as follows: 4455 g of 10T salt, 495 g of 56 salt, 3 g of sodium hypophosphite, 7.5 g of N,N′-bis-(3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionyl)hexanediamine, the temperature of the extruder feeding and conveying section was 260°C, the polymerization section was 300°C, the devolatilization section was 305°C, the extrusion section was 305°C, the rotation speed was 150 rpm, and the residence time was 3 min 25 s.

[0186] Example 6

[0187] The same twin-screw equipment, feed ratio and process as those in Example 5 were used, except that a dibasic acid and a diamine composition were used for preparation. The feed conditions were as follows: 214 g of 1,5-pentanediamine, 2278 g of 1,10-decanediamine, 2187 g of terephthalic acid, and 291 g of 1,6-hexanediamine, wherein the molar ratio of the dibasic acid to the diamine was 1:1.01.

[0188] Example 7

[0189] The same twin-screw equipment as in Example 1 was used, except that the 12T / 56 molar ratio was 82:18, and the feeding conditions were as follows: 4356 g of 12T salt, 594 g of 56 salt, 2.75 g of sodium hypophosphite, 9 g of (3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionyl)hexanediamine, the temperature of the extruder feeding and conveying section was 250°C, the polymerization section was 295°C, the devolatilization section was 298°C, the extrusion section was 290°C, the rotation speed was 120 rpm, and the residence time was 4 min 30 s.

[0190] Example 8

[0191] The same twin-screw equipment, feed ratio and process as those in Example 7 were used, except that a dibasic acid and a diamine composition were used for preparation. The feed conditions were as follows: 252 g of 1,5-pentanediamine, 2531 g of 1,12-diaminododecane, 1825 g of terephthalic acid, and 278 g of 1,6-hexanodioic acid, wherein the molar ratio of the dibasic acid to the diamine was 1:1.17.

[0192] Example 9

[0193] The same twin-screw equipment as in Example 1 was used, with the addition amount of additives, rotation speed and residence time, except that the feed ratio and temperature setting were different. Specifically, the 5T / 56 molar ratio was 7.5 / 92.5, the feed conditions were as follows: 396 g of 5T salt, 4554 g of 56 salt, the temperature of the extruder feeding and conveying section was 250°C, the polymerization section was 270°C, the devolatilization section was 265°C, and the extrusion section was 265°C.

[0194] Comparative Example 1

[0195] (1) Add the raw materials (same as in Example 1) into a twin-screw extruder;

[0196] Compared with the screw extruder in Example 1, the first group of elements, the third group of elements and the fifth group of elements of the second screw assembly in the screw extruder are all composed of three meshing blocks, excluding forward thread elements and reverse thread elements, and the three meshing blocks are forward meshing blocks, reverse meshing blocks and forward meshing blocks in sequence, and the staggered angle of adjacent meshing blocks is 90° and the length is 60 mm; the rest is the same as in Example 1;

[0197] (2) Same as Example 1;

[0198] (3) Same as Example 1.

[0199] Comparative Example 2

[0200] (1) Add the raw materials (same as in Example 1) into a twin-screw extruder;

[0201] Compared with the screw extruder in Example 1, the screw extruder is sequentially arranged with a first screw assembly and its corresponding barrels 1-3 (i.e., a feeding and conveying system), a first group of elements of a second screw assembly and its corresponding barrel 4 (i.e., a first polymerization system), a second group of elements of a second screw assembly and its corresponding barrel 5 (i.e., a first devolatilization system), a first screw assembly and its corresponding barrels 6-9 (i.e., a feeding and conveying system); and a third screw assembly and its corresponding barrel 10 (extrusion system); the rest are the same as in Example 1;

[0202] (2) Same as Example 1;

[0203] (3) Same as Example 1.

[0204] Comparative Example 3

[0205] (1) 2624 g of 5T salt, 2526 g of 56 salt and 4950 g of deionized water were added into a 20 L polymerization reactor, wherein the molar ratio of 5T salt to 56 salt was 51:49;

[0206] (2) After maintaining the pressure at 2 MPa for 50 minutes, releasing the pressure for 60 minutes to normal pressure, and evacuating the pressure (-0.09 MPa) for 30 minutes, the material is discharged to obtain a polyamide resin.

[0207] The total polymerization time of the above production process is at least 140 minutes, which is much longer than the direct preparation of polyamide resin by a twin-screw extruder in Examples 1 to 9 (time of about 3 to 5 minutes), and the efficiency is relatively low.

[0208] Effect Example 1

[0209] The polyamide resins prepared in the above Examples 1 to 9 and Comparative Examples 1 to 3 were tested as follows:

[0210] (1) Relative viscosity ηr

[0211] Test instrument: Ubbelohde viscometer AVS600, purchased from Shanghai Luwen Scientific Instrument Co., Ltd.

[0212] Test method: Ubbelohde viscometer concentrated sulfuric acid method, accurately weigh 0.5±0.0002g of dried polyamide resin material sample, add 50mL concentrated sulfuric acid (96%) to dissolve, measure and record the concentrated sulfuric acid flow time t0 and the polyamide resin material solution flow time t in a 25℃ constant temperature water bath. Relative viscosity calculation formula: relative viscosity ηr=t / t0; where: t: solution flow time; t0: solvent flow time.

[0213] (2) Melting point

[0214] Test instrument: Differential Scanning Calorimeter DSC Q20, purchased from TA Instruments, USA.

[0215] Test method: Weigh 5-8 mg of sample and place it in an aluminum crucible, use an empty crucible as a comparison, and under nitrogen protection (air flow rate of 50 mL / min), heat up to 300°C at 20°C / min, stay for 3 minutes to eliminate thermal history, then cool down to 30°C at 20°C / min, and then heat up to 300°C at 20°C / min, and record the change in thermal enthalpy during the temperature scan.

[0216] (3) Yellowness index

[0217] Testing instrument: Yellowness index meter

[0218] Test method: The test method refers to HG / T3862-2006.

[0219] (4) Molecular weight

[0220] Testing instrument: Gel permeation chromatography

[0221] Test method: The test was conducted by gel permeation chromatography (GPC), with PMMA as the standard substance and trifluoroethanol + 0.05% potassium trifluoroacetate as the solvent. After complete dissolution, the solution was filtered through a PTFE membrane and analyzed at 40°C to obtain the molecular weight and distribution relative to PMMA.

[0222] (5) Yield:

[0223] Yield = output of polyamide resin / total amount of input

[0224] The total amount of feed is the sum of the masses of the diamine and the dibasic acid, or the sum of the masses of different types of nylon salts.

[0225] The results are shown in Table 1.

[0226] Table 1

[0227] Yield (%) Melting point(℃) Relative viscosity Yellow Index YI Molecular weight distribution PDI Example 1 90 297.7 2.33 1.68 1.89 Example 2 88 296.3 2.45 1.73 1.81 Example 3 92 303.5 2.39 1.58 1.94 Example 4 86 304.1 2.40 1.66 1.71 Example 5 89 291.7 2.38 1.99 2.04 Example 6 87 292.2 2.31 1.87 1.90 Example 7 90 284.7 2.49 2.28 1.78 Example 8 88 284.2 2.36 2.20 1.86 Example 9 85 252.7 2.33 2.03 1.98 Comparative Example 1 87 278.2 1.71 11.8 3.25 Comparative Example 2 85 283.5 1.75 5.89 4.56 Comparative Example 3 72 296.6 2.44 36.4 2.78

[0228] It can be seen from Table 1 that the production equipment of polyamide resin in the present invention has a significantly improved yield compared with conventional production equipment by specially designing the screw elements; and the polyamide resin produced under the same production conditions has the excellent effects of high melting point and high relative viscosity, a lower yellow index of resin chips, a narrower molecular weight distribution, and a higher chemical reaction efficiency.

[0229] Those skilled in the art know that PDI (Polymer dispersity index) is a polymer dispersity index used to describe the molecular weight distribution of polymers, and its value is also = M(w) / M(n), and its value is greater than 1. The larger the PDI, the wider the molecular weight distribution, and the smaller the PDI, the more uniform the molecular weight distribution.

[0230] Effect Example 2

[0231] Resin mechanical properties test

[0232] Test equipment: Electronic universal testing machine UTM4304, impact strength tester PTM1000, both purchased from Shenzhen Sansi Zongheng Technology Co., Ltd.

[0233] Test method: The polyamide resin slices are dried to a moisture content of less than 1000ppm, and injection molding is performed using an injection molding machine (the injection molding machine can be a conventional device in the art). The determination method of the tensile strength (MPa) and elongation at break (%) of the resin is determined by referring to the method of GB / T14344-2008 (tensile test specimen specification: 170*20*4mm, dumbbell-shaped); the determination method of the flexural strength (MPa) of the resin is determined by referring to the method of ISO527-2 (flexural test specimen specification: 80*10*4mm); the notched cantilever beam impact strength (kJ·m -2 ) is determined by referring to ISO 197 / leA method (impact test specimen specification: 80*10*4mm, with a notch on one side).

[0234] The performance of the resin materials prepared in Examples 1 to 9 and Comparative Examples 1 to 3 was tested, and the results are shown in Table 2 below.

[0235] Table 2

[0236]

[0237] It can be seen from Table 2 that the polyamide resin production equipment in Examples 1 to 9 selects a specific extruder for conveying, polymerization, devolatilization and extrusion, and the mechanical properties of the produced resin material are better, while the performance of the resin produced by conventional equipment is obviously inferior to that of Examples 1 to 9.

Claims

1. A polyamide resin production equipment, characterized in that, It comprises a screw barrel and a screw unit; the screw unit is arranged in the accommodating cavity of the screw barrel; The screw unit comprises a core shaft and a screw assembly sleeved on the core shaft; The screw assembly comprises a first screw assembly, a second screw assembly and a third screw assembly which are sequentially arranged along the material conveying direction; Wherein, the first screw assembly is used for material transportation; Wherein, the second screw assembly is used to melt-polymerize and devolatilize the material; the second screw assembly is repeated n times, n≥2; The second screw assembly includes a first group of elements and a second group of elements arranged in sequence along the material conveying direction; The first set of elements includes a forward thread element, an engagement block and a reverse thread element arranged in sequence, and is used to make the material undergo a polymerization reaction; The second set of elements includes threaded elements for devolatilizing the polymer; Wherein, the third screw assembly is used for extrusion to obtain polyamide resin.

2. The production equipment of polyamide resin according to claim 1, characterized in that, The polyamide resin production equipment meets one or more of the following conditions I to IV: I. The screw barrel comprises 6 to 30 barrel sections, preferably 6 to 16 barrel sections; II. The polyamide resin production equipment comprises at least two screw units rotating in the same direction; preferably, the mandrels of any two screw units and the screw assemblies sleeved on the mandrels are completely identical; III. The aspect ratio of the mandrel is (20-68):1; preferably (40-60):1; more preferably (45-55):1; IV. The diameter of the mandrel is 20 to 95 mm, preferably 35 to 50 mm; Preferably, the polyamide resin production equipment satisfies the above conditions I to IV at the same time.

3. The production equipment of polyamide resin according to claim 1, characterized in that, The polyamide resin production equipment meets the following conditions i and / or ii: i. The first screw assembly includes a forward thread element and a reverse thread element arranged in sequence along the material conveying direction; The number of the forward thread elements is preferably 1 to 10, more preferably 2 to 8, and further preferably 3 to 6; the number of the reverse thread elements is preferably 1 to 10, more preferably 2 to 8, and further preferably 3 to 6; Preferably, the first screw assembly is composed of more than one forward thread element and more than one reverse thread element; Wherein, the lead of the forward thread element is preferably 1D to 2.5D; the lead of the reverse thread element is preferably 1D to 2D; ii. The first screw assembly preferably corresponds to more than 2 sections of the barrel; The upper end of the first cylinder is provided with a main feeding port, and is connected to the main feeding system through the main feeding port; the upper end of the second cylinder is provided with an auxiliary feeding port, and is connected to the auxiliary feeding system through the auxiliary feeding port; When the first screw assembly corresponds to more than 3 sections of the barrel, optionally, an additive feeding port is provided at the upper end of the third barrel, and is connected to the additive feeding system through the additive feeding port.

4. The production equipment of polyamide resin according to claim 1, characterized in that: The polyamide resin production equipment meets one or more of the following conditions a to h: a. In the first group of elements of the second screw assembly, the number of the forward thread elements and the reverse thread elements are independently 1 to 5, preferably 2 to 4; the number of the meshing blocks is preferably more than 2; b. In the first group of elements of the second screw assembly, the lead of the forward thread element is 0.1D to 0.5D; c. In the first group of elements of the second screw assembly, the length of the forward thread element is 4 to 60 mm; d. In the first group of elements of the second screw assembly, the lead of the reverse thread element is 0.5D to 2D, preferably 0.57D to 1D; e. In the first group of elements of the second screw assembly, the length of the reverse thread element is 10 to 120 mm; f. In the first group of elements of the second screw assembly, the meshing block is a forward meshing block or a reverse meshing block; g. In the first group of elements of the second screw assembly, the length of the engagement block is 20 to 120 mm; h. In the first group of elements of the second screw assembly, the staggered angle between the connecting end faces of adjacent meshing blocks is 45°, 60° or 90°; Preferably, the polyamide resin production equipment satisfies the above conditions a to h at the same time.

5. The production equipment of polyamide resin according to claim 1, characterized in that: The polyamide resin production equipment meets one or more of the following conditions ① to ③: ①, the second group of elements of the second screw assembly includes forward thread elements; Wherein, the number of the positive thread elements is preferably 1 to 6, more preferably 2 to 4; Wherein, the lead of the forward thread element is preferably 1.5D to 2.5D; ②, a devolatilization port is provided at the upper end of the barrel corresponding to the second group of elements of the second screw assembly; Preferably, the devolatilization port is provided with a vacuum device; ③, n is 3 to 20, preferably 3 to 8, more preferably 3 to 5; Preferably, the polyamide resin production equipment satisfies the above conditions ① to ③ at the same time.

6. The production equipment of polyamide resin according to any one of claims 1 to 5, characterized in that: The production equipment of the polyamide resin meets the following conditions ④ and / or ⑤: ④. The third screw assembly includes a reverse thread element; Wherein, the number of the reverse thread elements is preferably 5 to 15, more preferably 6 to 12; Wherein, the reverse thread element is preferably a small lead thread element, and the lead of the reverse thread element is preferably 0.1D to 0.5D; ⑤. The D is the major diameter of the thread; D is independently preferably 5 to 60 mm, more preferably 10 to 40 mm.

7. The production equipment of polyamide resin according to claim 1, characterized in that: The polyamide resin production equipment meets one or more of the following conditions ⑥ to ⑧: ⑥. The temperature settings of the polyamide resin production equipment are: 120-300°C for the feeding and conveying system, 240-330°C for the polymerization system, 250-330°C for the devolatilization system, and 260-320°C for the extrusion system; ⑦. The screw speed of the polyamide resin production equipment is 30 to 500 rpm, preferably 60 to 500 rpm, more preferably 60 to 200 rpm; ⑧. The residence time of the material in the polyamide resin production equipment is 10s to 30min, preferably 10s to 15min, more preferably 1min to 15min; Preferably, the polyamide resin production equipment satisfies the above conditions ⑥ to ⑧ at the same time.

8. A method for preparing a polyamide resin, characterized in that: The polyamide resin production device is adopted as claimed in any one of claims 1 to 7.

9. The method for preparing a polyamide resin according to claim 8, wherein: The preparation method of the polyamide resin comprises the following steps: adding diamine and dibasic acid, or nylon salt prepared from diamine and dibasic acid, into the production equipment of the polyamide resin, and after conveying, polymerizing and devolatilizing, extruding to obtain the polyamide resin; the number of polymerization and devolatilization is ≥2.

10. The method for preparing a polyamide resin according to claim 9, wherein The preparation method of the polyamide resin satisfies one or more of the following conditions A to E: A. During the conveying process, the material melts; the melting temperature is 120-350°C, preferably 200-330°C, and more preferably 250-325°C; B. The polymerization temperature is 200-350°C, preferably 240-330°C, more preferably 295-320°C, and further preferably 300-310°C; C. The devolatilization temperature is 220-350°C, preferably 250-330°C, more preferably 295-325°C, further preferably 298-320°C, for example 305-310°C; D. The devolatilization is vacuum devolatilization; the vacuum degree of the vacuum devolatilization is preferably -0.095 to 0 MPa, more preferably -0.09 to 0 MPa; E. The extrusion temperature is 220-350°C, preferably 240-320°C, more preferably 290-310°C, and further preferably 300-305°C; Preferably, the method for preparing the polyamide resin satisfies the above conditions A to E simultaneously.

Citation Information

Patent Citations

  • Method for dewatering a polymer and the polymer made therefrom

    CN107849260A

  • Double-screw assembly for extrusion molding processing of nylon and glass fiber, and processing method thereof

    CN109291404A

  • Phosphonate flame-retardant system polyamide material and preparation method thereof

    CN113969057A

  • Nylon master batch with high lubricant content and preparation method of nylon master batch

    CN115582935A

  • A twin -screw for polystyrene regeneration pelleting

    CN207758094U

Cited By