Single-side repairing method for penetrability damage of composite sandwich structure in closed space
By using pneumatic grinding, patch production and curing steps in the enclosed space composite sandwich structure, one-sided repair of penetrating damage is achieved, solving the problem that traditional repair methods cannot repair internal panel damage, and ensuring the quality of repair and the material's stress balance.
Patent Information
- Application Number
- CN202411136679.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-19
- Publication Date
- 2024-11-19
AI Technical Summary
When the penetrating damages of the sandwich structure of the enclosed space composite material, traditional repair methods are difficult to repair internal panel damage, especially in restricted environments, traditional sandwich structure excavation and repair methods cannot be used.
A single-side repair method for penetrating damage of the sandwich structure of enclosed space composite material is adopted, including cleaning, pneumatic grinding, trimming, grinding, patch making, pasting, curing and other steps. By pasting precured patches on the inner panel and Combined with the traditional sandwich structure excavation and repair methods, damage repair of the inner and outer panels and core materials is achieved.
It effectively solves the problem that traditional repair methods in closed spaces cannot repair internal panel damage, and realizes the repair of damage to the inner and outer panels and core materials of the sandwich structure, ensuring the balance of repair quality and material stress.
Smart Images

Figure CN118977443A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of composite sandwich repair, in particular to a method for repairing penetrating damage on one side of a closed space composite sandwich structure. Background Art
[0002] Composite sandwich structures are widely used in the fields of aircraft, automobiles, ships, etc. due to their excellent designability and mechanical properties. Composite sandwich structures are usually composed of fiber-reinforced resin-based composite inner and outer panels and a core layer. The core layer can be made of NOMEX honeycomb, aluminum honeycomb, foam and other materials. During use, due to the influence of external loads, it is inevitable that the sandwich composite structure will be damaged, especially penetrating damage, that is, the damage penetrates from the outer panel to the inner panel, which must be repaired at this time. Then, for the purpose of protection design, some composite sandwich components are designed in a closed space, and in the actual repair process, they are usually affected by the field working environment, the spatial interference of other assemblies, etc., and the damaged inner panel cannot be repaired using the traditional sandwich structure patching repair method, which makes it difficult to repair penetrating damage to the closed space sandwich structure. Summary of the invention
[0003] In order to solve the above problems, the present invention proposes a method for unilaterally repairing penetrating damage of a closed space composite sandwich structure.
[0004] A method for repairing penetrating damage on one side of a closed space composite sandwich structure, the specific steps of which are as follows:
[0005] Step S1: Cleaning: Clean the damaged area with an organic solvent;
[0006] Step S2: pneumatic grinding: the outer composite material panel of the sandwich structure is bevel-grinded at a chamfer ratio of 1:20 by pneumatic grinding;
[0007] Step S3: trimming: first use a utility knife to preliminarily remove the honeycomb core layer, and then use a grinder to trim the periphery of the original honeycomb core material;
[0008] Step S4: polishing: polish the adhesive film below the removed honeycomb core layer, polish the damaged area of the inner panel to improve the surface roughness, and clean the surface of the inner panel after polishing;
[0009] Step S5: patch production: select a panel with the same material and thickness as the original inner panel, and according to the shape and size of the honeycomb core layer cut in step S3, use a machine tool or a tool to process the panel to the same shape and size as the cut honeycomb core layer for repair to form a patch;
[0010] Step S6: cutting the inner patch film: the size of the inner patch film is the same as the size of the patch, and the inner patch film is tightly attached around the damaged area of the inner panel. Meanwhile, the material system of the inner patch film should be the same as the film system used in the original structure;
[0011] Step S7: pasting: placing the prepared patch on the inner patch film, and allowing the patch and the inner patch film to stick tightly;
[0012] Step S8: cutting size: cutting the honeycomb bottom film, the size of the honeycomb bottom film is consistent with the size of the honeycomb, and the honeycomb bottom film should be the same as the inner patch film system;
[0013] Step S9: cutting a new honeycomb core layer and wrapping a foam glue 4 around the honeycomb core layer;
[0014] Step S10: Returning to position: placing the honeycomb core layer wrapped with foam glue on the honeycomb bottom glue film;
[0015] Step S11: cutting the outer layer of adhesive film: cutting the outer layer of adhesive film and pasting the outer layer of adhesive film on the upper end of the new honeycomb core layer;
[0016] Step S12: Repair: According to the repair needs, select pre-cured patch repair or prepreg paving repair to repair the outer panel:
[0017] a. If a pre-cured patch is used for repair, the patch must be made according to the material system, ply direction, and curing process of the original outer panel, and then the prepared patch is placed on the honeycomb top film;
[0018] b. If prepreg is used for repair, the prepreg shall be laid layer by layer according to the material system and laying direction of the original outer panel;
[0019] Step S13: Curing: Lay out the vacuum bag system, set the process curve according to the curing temperature, time and pressure of the adhesive film and prepreg, and perform heating and curing;
[0020] Step S14: Dismantling: After curing is completed, the vacuum system is dismantled and excess resin is removed;
[0021] Step S15: Inspection: Perform nondestructive inspection on the repair area to ensure the quality of the repair.
[0022] The organic solvent in step S1 is acetone or ethanol.
[0023] The minimum diameter of the grinding in step S2 needs to be at least 25 mm larger than the damaged diameter of the inner panel.
[0024] In step S3, the diameter of the honeycomb core layer removed is at least 25 mm larger than the damaged diameter of the inner panel.
[0025] In step S5, the size of the patch is 25 mm larger than the damaged diameter of the inner panel.
[0026] In the step S9, the diameter of the new honeycomb core layer is 4 mm smaller than the diameter of the removed honeycomb core layer, and the height of the new honeycomb core layer is shorter than the height of the original honeycomb core by the thickness of an inner layer patch.
[0027] In the step S11, the size of the outer layer film is the same as the size of the honeycomb core layer, and the material system of the outer layer film should be the same as the film system used in the original structure.
[0028] In step S14, the excess resin on the surface of the honeycomb sandwich structure is removed by manual sandpaper polishing.
[0029] The beneficial effects of the present invention are: in order to address the problem of difficulty in repairing penetrating damage to composite sandwich structures in closed intervals, by pasting pre-cured patches on the inner panels and combining them with traditional sandwich structure patching and repair methods, damage repair of the inner and outer panels and core materials of the sandwich structure is achieved, solving the problem that traditional repair methods in closed spaces cannot repair damage to internal panels. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] The present invention is further described below in conjunction with the accompanying drawings and embodiments.
[0031] Figure 1 It is a structural schematic diagram of the present invention;
[0032] Figure numerals: 1, outer layer; 2, outer layer film; 3, honeycomb core layer; 4, foam glue; 5, outer layer panel; 6, original honeycomb core; 7, inner layer panel; 8, honeycomb bottom film; 9, patch; 10, film; 11, damaged area. DETAILED DESCRIPTION
[0033] In order to make the technical means, creative features, objectives and effects achieved by the present invention easy to understand, the present invention is further described below.
[0034] like Figure 1 As shown, a method for repairing penetrating damage on one side of a closed space composite sandwich structure, the specific steps of which are as follows:
[0035] Step S1: Cleaning: using an organic solvent to clean the damaged area 11;
[0036] Step S2: pneumatic grinding: the outer composite material panel of the sandwich structure is bevel-grinded at a chamfer ratio of 1:20 by pneumatic grinding;
[0037] Step S3: trimming: first use a utility knife to preliminarily remove the honeycomb core layer 3, and then use a grinder to trim the periphery of the original honeycomb core 6;
[0038] Step S4: polishing: polish the adhesive film 10 below the removed honeycomb core layer 3, and polish the damaged area 11 of the inner panel 7 to improve the surface roughness. After polishing, clean the surface of the inner panel 7 to ensure the cleanliness and roughness of each surface, thereby improving the bonding strength;
[0039] Step S5: patch production: select a panel with the same material and thickness as the original inner panel 7, and use a machine tool or a tool to process the panel to the same shape and size as the cut honeycomb core layer 3 according to the shape and size of the honeycomb core layer 3 cut in step S3 to form a patch 9, ensuring that it can be directly placed in the polished honeycomb space and accurately fit, without the need to use traditional prepreg paving, so as to achieve the purpose of repairing and filling the damaged panel in the closed space;
[0040] Step S6: cutting the inner patch film 10: the size of the inner patch film 10 is the same as that of the patch 9, and the film 10 is tightly attached around the damaged area 11 of the inner panel 7. At the same time, the material system of the inner patch film 10 should be the same as that of the original structure. The same material system can ensure that the internal force of the repaired material is balanced;
[0041] Step S7: pasting: placing the prepared patch 9 on the inner patch film 10, and closely pasting the patch 9 and the inner patch film 10, so as to achieve precise pasting of the patch 9 and the inner patch film 10, and avoid inadequate repair or excess material;
[0042] Step S8: cutting size: cutting the honeycomb bottom adhesive film 8, the size of the honeycomb bottom adhesive film 8 is consistent with the size of the honeycomb, and the honeycomb bottom adhesive film 8 should be the same as the inner patch adhesive film 10 system, so as to achieve accurate fitting of the honeycomb cornea and the honeycomb, avoiding inadequate repair or excess material;
[0043] Step S9: cutting a new honeycomb core layer 3, and wrapping a foam glue 4 around the honeycomb core layer 3, so that the newly filled honeycomb core layer can fully contact with the original honeycomb core layer, thereby improving the bonding strength;
[0044] Step S10: Returning to position: placing the honeycomb core layer 3 wrapped with the foam glue 4 on the honeycomb bottom glue film 8, so that the newly filled honeycomb core layer can fully contact with the original bottom panel to improve the bonding strength;
[0045] Step S11: cutting the outer layer adhesive film 2: cutting the outer layer adhesive film 2 and pasting the outer layer adhesive film 2 on the upper end of the new honeycomb core layer 3, so that the newly filled honeycomb core layer can fully contact with the subsequently added upper repair panel, thereby improving the bonding strength;
[0046] Step S12: Repair: According to the repair needs, the outer layer 1 patch 9 is selected for repair or the prepreg paving repair is performed on the outer layer panel 5 to ensure that the repaired outer layer material is consistent with the original panel to avoid unbalanced force caused by different material systems:
[0047] a. If the patch 9 is used for repair, the patch must be made according to the material system, ply direction, and curing process of the original outer panel 5, and then the made patch is placed on the honeycomb top film;
[0048] b. If prepreg is used for repair, the prepreg shall be laid layer by layer according to the material system and laying direction of the original outer panel 5;
[0049] Step S13: Curing: Lay out a vacuum bag system, set a process curve according to the curing temperature, time and pressure of the adhesive film and prepreg, and perform heating curing. After the adhesive film is cured, the bonding strength between the panel and the honeycomb can be improved;
[0050] Step S14: Dismantling: After curing is completed, the vacuum system is dismantled and excess resin is removed to keep the repaired surface flat and clean;
[0051] Step S15: Inspection: Perform nondestructive inspection on the repair area to ensure the repair quality and repair effect.
[0052] In view of the difficulty in repairing penetrating damage to composite sandwich structures in closed areas, the damage to the inner and outer panels and core materials of the sandwich structure can be repaired by pasting a patch 9 on the inner panel 7 and combining it with the traditional sandwich structure patching repair method, thus solving the problem that traditional repair methods in closed spaces cannot repair internal panel damage.
[0053] The organic solvent in step S1 is acetone or ethanol, which has strong cleaning ability, leaves no residue after cleaning, and does not damage the composite material panel.
[0054] The minimum diameter of the grinding in step S2 needs to be at least 25 mm larger than the damaged diameter of the inner panel 7. Miter grinding can increase the bonding area and enhance the bonding strength.
[0055] In the step S3, the removal diameter of the honeycomb core layer 3 is at least 25 mm larger than the damaged diameter of the inner panel 7. A tool is used for removal first, which is efficient, and then a grinder is used to improve the edge removal accuracy.
[0056] In step S5, the size of the patch is 25 mm larger than the damaged diameter of the inner panel 7.
[0057] As described in step 3-7, by increasing the honeycomb removal range, a patch 9 with the same material system and laying direction as the inner panel 7 of the composite sandwich structure is produced to achieve single-sided repair of penetrating damage to the closed space composite sandwich structure.
[0058] In the step S9, the diameter of the new honeycomb core layer 3 is 4 mm smaller than the diameter of the removed honeycomb core layer 3, and the height of the new honeycomb core layer 3 is shorter than the height of the original honeycomb core 6 by the thickness of an inner layer patch.
[0059] In the step S11, the size of the outer layer adhesive film 2 is the same as the size of the honeycomb core layer 3, and the material system of the outer layer adhesive film 2 should be the same as the adhesive film 10 system used in the original structure.
[0060] As described in step 13, during the implementation process, a repair method of curing the inner panel 7, the honeycomb interlayer, and the outer panel 5 at one time is adopted to simplify the repair process method.
[0061] In step S14, the excess resin on the surface of the honeycomb sandwich structure is removed by manual sandpaper polishing.
[0062] The above shows and describes the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments. The above embodiments and descriptions only describe the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, which fall within the scope of the present invention. The scope of protection of the present invention is defined by the attached claims and their equivalents.
Claims
1. A method for repairing penetrating damage on one side of a closed space composite sandwich structure, characterized by: The specific steps are as follows: Step S1: Cleaning: using an organic solvent to clean the damaged area (11); Step S2: pneumatic grinding: the outer composite material panel of the sandwich structure is bevel-grinded at a chamfer ratio of 1:20 by pneumatic grinding; Step S3: trimming: first use a utility knife to preliminarily remove the honeycomb core layer (3), and then use a grinder to trim the periphery of the original honeycomb core (6) material; Step S4: polishing: polishing the adhesive film (10) below the removed honeycomb core layer (3) and polishing the damaged area (11) of the inner panel (7), and cleaning the surface of the inner panel (7) after polishing; Step S5: patch production: a panel with the same material and thickness as the original inner panel (7) is selected, and the panel is processed by a machine tool or a tool to the same shape and size as the cut honeycomb core layer (3) according to the shape and size of the cut honeycomb core layer (3) in step S3, so as to form a patch (9); Step S6: cutting the inner patch film (10): the size of the inner patch film (10) is the same as the size of the patch (9), and the film (10) is tightly adhered around the damaged area (11) of the inner panel (7). At the same time, the material system of the inner patch film (10) should be the same as the inner patch film (10) system used in the original structure; Step S7: pasting: placing the prepared patch (9) on the adhesive film (10), and allowing the patch (9) and the adhesive film (10) to be closely pasted; Step S8: cutting size: cutting the honeycomb bottom adhesive film (8), the size of the bottom honeycomb bottom adhesive film (8) is consistent with the size of the honeycomb, and the honeycomb bottom adhesive film (8) should be the same as the material system of the inner patch adhesive film (10); Step S9: cutting a new honeycomb core layer (3), and wrapping a foam glue (4) around the honeycomb core layer (3); Step S10: Returning to position: placing the honeycomb core layer (3) wrapped with the foam glue (4) on the honeycomb bottom glue film (8); Step S11: cutting the outer layer of adhesive film (2): cutting the outer layer of adhesive film (2) and pasting the outer layer of adhesive film (2) on the upper end of the new honeycomb core layer (3); Step S12: Repair: According to the repair requirements, the outer layer (1) pre-cured patch (9) is selected for repair or the outer layer panel (5) is repaired by prepreg paving: a. If a pre-cured patch (9) is used for repair, the patch must be made according to the material system, ply direction, and curing process of the original outer panel (5), and then the made patch is placed on the honeycomb top film; b. If prepreg is used for repair, the prepreg shall be laid layer by layer according to the material system and laying direction of the original outer panel (5); Step S13: Curing: Lay out a vacuum bag system, set a process curve according to the inner patch film (10) and the prepreg curing temperature, time, and pressure, and perform heating curing; Step S14: Dismantling: After curing is completed, the vacuum system is dismantled and excess resin is removed; Step S15: Inspection: Perform nondestructive inspection on the repair area.
2. The method for repairing penetrating damage to a closed space composite sandwich structure according to claim 1, characterized in that: The organic solvent of the outer panel (5) in step S1 is acetone or ethanol.
3. The method for repairing penetrating damage to a closed space composite sandwich structure according to claim 1, characterized in that: The minimum diameter of the grinding in step S2 needs to be at least 25 mm larger than the damaged diameter of the inner panel (7).
4. The method for repairing penetrating damage to a closed space composite sandwich structure according to claim 1, characterized in that: In the step S3, the diameter of the honeycomb core layer (3) removed is 25 mm larger than the diameter of the damaged inner layer panel (7).
5. The method for repairing penetrating damage to a closed space composite sandwich structure according to claim 1, characterized in that: In step S5, the size of the patch is 25 mm larger than the damaged diameter of the inner panel (7).
6. The method for repairing penetrating damage to a closed space composite sandwich structure according to claim 1, characterized in that: In the step S9, the diameter of the new honeycomb core layer (3) is 4 mm smaller than the diameter of the removed honeycomb core layer (3), and the height of the new honeycomb core layer (3) is shorter than the height of the original honeycomb core (6) by the thickness of an inner layer patch.
7. The method for repairing penetrating damage to a closed space composite sandwich structure according to claim 1, characterized in that: In the step S11, the size of the outer layer adhesive film (2) is the same as the size of the honeycomb core layer (3), and the material system of the outer layer adhesive film (2) should be the same as the adhesive film system used in the original structure.
8. The method for repairing penetrating damage to a closed space composite sandwich structure according to claim 1, characterized in that: In step S14, the excess resin on the surface of the honeycomb sandwich structure is removed by manual sandpaper polishing.
Citation Information
Cited By
Composite material repairing method based on circular truncated cone
CN120287001A
Repair method of reverse pushing baffle door bending structure
CN122539694A