Biochar material, preparation method and application thereof, gas transmission type electrode and gas lift liquid flow type electric ozone device
By modifying biochar materials, the catalytic activity and gas utilization rate of electroozone technology is improved, and the problem of low catalytic activity of traditional carbon black electrodes is solved, and the effect of efficient degradation of pollutants in water is achieved, reducing costs and promoting the expansion of technology. application.
Patent Information
- Application Number
- CN202411068491.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-06
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-08-06
AI Technical Summary
The carbon black electrode used in traditional electroozone technology has low catalytic activity, resulting in high cost and low gas utilization efficiency, and is unable to effectively degrade pollutants in water.
Using modified biochar material as a catalyst, a high catalytic activity biochar material is prepared by mixing biomass with transition metal salts, and applied to gas penetrating electrodes and gas-liquid flow-type electro-ozone devices to improve catalytic activity and Gas utilization.
It significantly improves catalytic activity and gas utilization rate, reduces production costs, achieves the effect of efficient degradation of pollutants in water, and promotes the expansion and application of electro-ozone technology.
Smart Images

Figure CN118978128A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of electric ozone, and specifically relates to a biochar material and a preparation method and application thereof, a gas-penetrating electrode and a gas-lift liquid-flow electric ozone device. Background Art
[0002] With the acceleration of industrialization and the rapid growth of population, water pollution is becoming increasingly serious. Traditional water treatment technologies, such as physical treatment technologies such as adsorption, coagulation, and filtration, can only change the physical state of pollutants, but cannot completely convert them into harmless substances. Biological treatment technologies, such as the activated sludge method, have limited treatment effects on certain difficult-to-degrade organic matter and micropollutants (such as environmental endocrine disruptors, pharmaceuticals, and personal care products), and it is difficult to achieve the expected purification effect. Therefore, it is imperative to find efficient, economical, and environmentally friendly water treatment technologies.
[0003] As a strong oxidant, ozone has attracted extensive attention in the field of water treatment because it can effectively degrade a variety of pollutants, and its decomposition products are oxygen, it does not produce toxic byproducts, and it can increase the dissolved oxygen in the water body. In addition to traditional ozone oxidation technology, many advanced oxidation technologies have been developed in recent years, including ozone catalytic oxidation, O3 / UV, O3 / H2O2, electro-ozone and other ozone coupling technologies. Among them, electro-ozone technology uses the two-electron oxygen reduction reaction to react hydrogen peroxide generated at the cathode with ozone to produce hydroxyl radicals (·OH). Hydroxyl radicals are active substances with strong oxidizing ability and can efficiently degrade a variety of organic pollutants. On the basis of achieving efficient degradation of pollutants, this technology avoids the step of adding additional hydrogen peroxide and the risk of explosion during the transportation of hydrogen peroxide. At the same time, it simplifies the treatment process and reduces operating costs. It is considered to be a promising water treatment technology.
[0004] The electro-ozone device includes an ozone generator and a reaction device, and the reaction device includes an immersed electrode (cathode and anode), an aeration device and a stirring device. The cathode of the traditional electro-ozone device adopts a carbon black-polytetrafluoroethylene electrode, and the conductive carbon black is expensive, which limits the application of this method. In addition, since carbon atoms are neutral, they are inert to the adsorption or activation of intermediates produced during O2 and the two-electron oxygen reduction reaction, which limits its activity in the two-electron oxygen reduction reaction, resulting in low catalytic activity of conductive carbon black. Summary of the invention
[0005] The object of the present invention is to provide a biochar material and a preparation method and application thereof, a gas-penetrating electrode and a gas-lift liquid flow electro-ozone device. The biochar material provided by the present invention has higher catalytic activity. The biochar material provided by the present invention is used as a catalyst to make a gas-penetrating electrode and applied to the electro-ozone technology. On the basis of obtaining excellent degradation effect, the production cost is reduced and the gas mass transfer efficiency is improved.
[0006] In order to achieve the above object, the present invention provides the following technical solutions:
[0007] The present invention provides a biochar material, comprising a biochar matrix and an active component loaded in the biochar matrix;
[0008] The active ingredients include metal elements and metal ions;
[0009] The metal element in the metal element and the metal ion is of the same type;
[0010] The metal element includes a transition metal element, and the transition metal element includes iron, manganese, copper, zinc, cobalt or nickel.
[0011] Preferably, the atomic content of the metal element in the active ingredient is 10% to 20%;
[0012] The atomic content of active components in the biochar material is 0.5% to 2%.
[0013] Preferably, the biochar material is also doped with nitrogen; the atomic content of nitrogen in the biochar material is 2% to 10%.
[0014] The present invention also provides a method for preparing the biochar material described in the above technical solution, comprising:
[0015] Mixing the biomass raw material and the metal salt, and calcining them to obtain the biochar material;
[0016] The metal salt includes a transition metal salt, and the transition metal salt includes an iron salt, a manganese salt, a copper salt, a zinc salt, a cobalt salt or a nickel salt.
[0017] Preferably, the biomass raw material includes one or more of chitosan, sodium alginate, gelatin, plant residues, wood and bamboo; the plant residues include one or more of tea residues, olive residues, coffee residues, fruit peels, straw and fruit shells;
[0018] The calcination temperature is 800-900° C., and the heat preservation time is 40-90 minutes; the calcination is carried out under a protective atmosphere.
[0019] The present invention also provides the use of the biochar material described in the above technical solution or the biochar material prepared by the preparation method described in the above technical solution as a catalyst in preparing a cathode of an electric ozone device.
[0020] The present invention also provides a gas permeable electrode, comprising a porous gas permeable layer and a porous catalyst layer stacked in sequence;
[0021] The material of the porous catalyst layer includes a catalyst and a binder;
[0022] The catalyst is the biochar material described in the above technical solution or the biochar material prepared by the preparation method described in the above technical solution.
[0023] Preferably, the content of the catalyst in the gas permeable electrode is 0.5-5 mg / cm 2 .
[0024] The present invention also provides an airlift liquid flow type electric ozone device, comprising a reaction tower 12 and an ozone generating device connected to the bottom end of the reaction tower 12;
[0025] A cathode 6 is horizontally arranged at the lower part of the reaction tower 12. The cathode 6 is a gas-permeable electrode as described in the above technical solution. The porous gas-permeable layer of the gas-permeable electrode is arranged downward.
[0026] An anode 8 is horizontally disposed at the upper portion of the reaction tower 12 , and a closed reaction chamber 7 is formed between the cathode 6 , the anode 8 and the side wall of the reaction tower 12 .
[0027] Preferably, the anode 8 is a coated titanium electrode;
[0028] The bottom end of the reaction tower 12 is provided with an air inlet 5;
[0029] The ozone generating device comprises an oxygen cylinder 1 and an ozone generator 2 which are connected in sequence, and the ozone generator 2 is connected to the air inlet 5 .
[0030] The present invention provides a biochar material, including a biochar matrix and an active component loaded in the biochar matrix; the active component includes a metal element and a metal ion; the metal element in the metal element and the metal ion is of the same type; the metal element includes a transition metal element, and the transition metal element includes iron, manganese, copper, zinc, cobalt or nickel. The present invention can obtain a higher catalytic activity than conductive carbon black by modifying the biochar with metal elements and metal ions, and can be applied to the electro-ozone technology, which can further reduce the cost and promote the expanded application of the electro-ozone technology; at the same time, it can realize the re-value of biomass and is also of great significance for solid waste management.
[0031] The present invention also provides a gas-penetrating electrode, comprising a porous gas-permeable layer and a porous catalyst layer stacked in sequence; the material of the porous catalyst layer comprises a catalyst and a binder; the catalyst is the biochar material described in the above technical solution or the biochar material prepared by the preparation method described in the above technical solution. In the present invention, the gas-penetrating electrode has a significant advantage in increasing the gas utilization rate. Due to its structural limitations and the accessibility of gaseous substances, the traditional submerged electrode mainly relies on oxygen and ozone dissolved in water for reaction. However, the solubility of oxygen and ozone in water is relatively low, resulting in a large amount of gas escaping from the liquid surface into the air, thereby greatly reducing the gas utilization efficiency. In contrast, the gas-penetrating electrode can not only utilize dissolved oxygen and ozone, but also directly utilize gaseous oxygen and ozone. This is because in the gas-penetrating electrode, gaseous oxygen and ozone must first pass through the catalyst layer of the electrode before entering the solution. This process forms a three-phase reaction interface in the catalyst layer, namely, a gas-liquid-solid three-phase interface, at which an electrode reaction occurs. In this way, the gas-penetrating electrode can effectively utilize gaseous substances, thereby significantly improving the utilization rate of gas. Due to the improvement in gas utilization, the gas-penetrating electrode not only increases the reaction rate, but also reduces the overpotential and reduces energy input. In other words, the gas-penetrating electrode shows obvious advantages in catalytic efficiency, energy utilization and reaction effect. These advantages make the gas-penetrating electrode show good prospects in the application of electro-ozone.
[0032] The present invention also provides a gas-lift liquid flow type electro-ozone device, comprising a reaction tower 12 and an ozone generating device connected to the air inlet 5 at the bottom of the reaction tower; the bottom of the reaction tower 12 comprises a horizontally arranged cathode 6, the cathode 6 is the gas-penetrating electrode described in the above technical solution, the porous gas-permeable layer of the gas-penetrating electrode is located above the air inlet 5 at the bottom of the reaction tower, and forms a closed space with the side wall of the reaction tower 12; the top of the reaction tower 12 comprises a horizontally arranged anode 8, and a reaction chamber 7 is formed between the cathode 6 and the anode 8. In the present invention, the gas-lift liquid flow type electro-ozone device can further improve the utilization rate of oxygen and ozone. The key to the device is to place the gas-penetrating electrode horizontally, and the gas passes through the electrode from bottom to top, and then rises by its own buoyancy. This design cleverly utilizes the internal pressure characteristics of the liquid and the diffusion characteristics of bubbles in the liquid, and significantly improves the reaction efficiency. After the gas passes through the gas-penetrating electrode, bubbles are formed, and the bubbles diffuse to the surface of the solution, and the liquid undergoes material transfer to generate dissolved oxygen and ozone. The contact time is determined by the diffusion path length of the bubbles. The longer the path, the more oxygen and ozone are dissolved. When the electrodes are placed vertically, the liquid pressure at the top is the lowest, and the gas can enter more easily from the top, forming short-path bubbles with less dissolved amount. When the electrodes are placed horizontally at the bottom of the reactor, the liquid pressure is uniform and maximum, and the gas passes through the electrodes from the bottom, extending the bubble path, increasing the contact time, maximizing the dissolved amount, and making the bubble distribution more uniform, which helps to further improve the reaction efficiency and reduce energy consumption without relying on additional stirring devices.
[0033] The gas-penetrating electrode and gas-lift liquid-flow electro-ozone device provided by the present invention optimize the electrode design and improve the gas dispersion system, thereby enhancing the mass transfer of ozone and oxygen to the electrode and increasing the utilization rate of ozone and oxygen, thereby achieving the effect of simultaneously improving the degradation efficiency and reducing energy consumption, and promoting the expanded application of electro-ozone degradation of pollutants. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] Figure 1 This is the SEM image of the biochar material obtained in Example 1;
[0035] Figure 2 This is the XRD pattern of the biochar material obtained in Example 1;
[0036] Figure 3 This is a physical picture of the hydrophobic carbon paper and the gas permeable electrode in Example 2;
[0037] Figure 4 It is a schematic diagram of the structure of the gas permeable electrode in the present invention;
[0038] Figure 5Schematic diagram of the structure of the gas-lift liquid flow type electric ozone device in Example 3 of the present invention, wherein 1 is an oxygen cylinder, 2 is an ozone generator, 3 is an ozone detector, 4 is a mass flow meter, 5 is an air inlet, 6 is a cathode, 7 is a reaction chamber, 8 is an anode, 9 is a tail gas chamber, 10 is a DC power supply, 11 is an ozone destruction chamber, 12 is a reaction tower, and 13 is an air outlet;
[0039] Figure 6 The LSV curves and H2O2 oxidation current test results of the two-electron oxygen reduction reaction of the biochar material obtained in Example 1 and commercially available conductive carbon black;
[0040] Figure 7 is the two-electron selectivity calculated from the LSV curve and H2O2 oxidation current;
[0041] Figure 8 This is a diagram showing the effect of ibuprofen degradation by the gas-lift liquid flow electro-ozone device, the traditional ozone oxidation device and the electrolysis device in Application Example 1;
[0042] Fig. 9 This is a diagram showing the effect of degrading ibuprofen at different current densities using the gas-lift liquid flow electro-ozone device in Application Example 2. DETAILED DESCRIPTION
[0043] The present invention provides a biochar material, comprising a biochar matrix and an active component loaded in the biochar matrix;
[0044] The active ingredients include metal elements and metal ions;
[0045] The metal element in the metal element and the metal ion is of the same type;
[0046] The metal element includes a transition metal element, and the transition metal element includes iron, manganese, copper, zinc, cobalt or nickel.
[0047] In the present invention, the atomic content of the metal element in the active ingredient is preferably 10% to 20%, and more preferably 15%. In the present invention, the atomic content of the active ingredient in the biochar material is preferably 0.5% to 2%, and more preferably 0.66% to 1.0%. In the present invention, the biochar material is also preferably doped with nitrogen; the atomic content of nitrogen in the biochar material is preferably 2% to 10%.
[0048] In the present invention, the biochar material has a porous structure, and by modifying the biochar with metal elements and metal ions, a catalytic activity higher than that of conductive carbon black can be obtained.
[0049] The present invention also provides a method for preparing the biochar material described in the above technical solution, comprising the following steps:
[0050] Mixing the biomass raw material and the metal salt, and calcining them to obtain the biochar material;
[0051] The metal salt includes a transition metal salt, and the transition metal salt includes an iron salt, a manganese salt, a copper salt, a zinc salt, a cobalt salt or a nickel salt.
[0052] In the present invention, unless otherwise specified, all preparation raw materials are commercially available products well known to those skilled in the art.
[0053] In the present invention, the biomass raw material preferably includes one or more of chitosan, sodium alginate, gelatin, plant residues, wood and bamboo; the plant residues preferably include one or more of tea residues, olive residues, coffee residues, peels, straw and fruit shells. In the present invention, the nickel salt is more preferably NiCl2·6H2O. In the present invention, the mass ratio of the biomass raw material to the transition metal salt is preferably 1 to 10:1, and more preferably 2:1.
[0054] In the present invention, the mixing is preferably carried out under the condition of heating and stirring, the temperature of the heating and stirring is preferably 120°C, and the time is preferably 8h. In the present invention, the temperature of the calcination is preferably 800-900°C, the holding time is preferably 40-90min, and more preferably 60min; the calcination is preferably carried out under a protective atmosphere, and the protective atmosphere is preferably nitrogen or an inert gas. In the present invention, the calcination is preferably carried out in a tubular furnace. In the present invention, during the calcination process, the biomass raw material is carbonized, part of the metal is anchored on the carbon material substrate to form MNC bonds (M represents metal, i.e., metal ions), and part of the metal undergoes thermal migration to form metal clusters (i.e., metal elements).
[0055] After the calcination, the present invention also preferably includes sequentially pickling, water washing, drying and ball milling the calcined product; the acid used for the pickling is preferably hydrochloric acid, and the molar concentration of the hydrochloric acid is preferably 1 mol / L; the temperature of the pickling is preferably 120°C, and the time is preferably 12h, and the excess impurities on the surface of the material can be removed by pickling; the water washing is preferably carried out with deionized water until the washing liquid is neutral. In the present invention, the drying temperature is preferably 80°C. In the present invention, the ball-to-material ratio of the ball milling is preferably 1:1, the rotation speed is preferably 600r / min, and the time is preferably 4h.
[0056] The present invention also provides the use of the biochar material described in the above technical solution or the biochar material prepared by the preparation method described in the above technical solution as a catalyst in preparing a cathode of an electric ozone device.
[0057] The present invention also provides a gas permeable electrode, comprising a porous gas permeable layer and a porous catalyst layer stacked in sequence;
[0058] The material of the porous catalyst layer includes a catalyst and a binder;
[0059] The catalyst is the biochar material described in the above technical solution or the biochar material prepared by the preparation method described in the above technical solution.
[0060] In the present invention, the porous air-permeable layer is preferably porous hydrophobic carbon paper, porous hydrophobic carbon felt or porous hydrophobic carbon cloth. In the present invention, the thickness of the porous air-permeable layer is preferably 0.1 to 0.3 mm, more preferably 0.19 mm.
[0061] In the present invention, the binder preferably includes polytetrafluoroethylene and / or perfluorosulfonic acid-polytetrafluoroethylene copolymer. In the present invention, the content of the catalyst in the gas permeable electrode is preferably 0.5-5 mg / cm 2 , more preferably 1 to 3 mg / cm 2 .
[0062] In the present invention, the gas-permeable electrode is preferably prepared by a spraying method; the spraying method preferably includes the following steps: mixing a catalyst, a binder solution and an organic solvent to obtain a slurry; placing the porous gas-permeable layer on a preheated substrate, spraying the slurry on one side of the porous gas-permeable layer, and obtaining the gas-permeable electrode after drying and heat treatment.
[0063] In the present invention, the organic solvent preferably includes anhydrous ethanol. In the present invention, the mass concentration of the binder solution is preferably 60%; the volume of the binder solution is preferably 0.166% of the volume of the organic solvent. In the present invention, the mass concentration of the catalyst in the slurry is preferably 4.536g / L. In the present invention, the mixing is preferably carried out under ultrasonic conditions. In the present invention, the preheating temperature is preferably 110°C. The present invention has no special limitation on the spraying process, and it can be adopted by those skilled in the art. In the present invention, the temperature of the heat treatment is preferably 330°C, and the insulation time is preferably 30min.
[0064] The present invention also provides an airlift liquid flow type electric ozone device, comprising a reaction tower 12 and an ozone generating device connected to the bottom end of the reaction tower 12;
[0065] A cathode 6 is horizontally arranged at the lower part of the reaction tower 12. The cathode 6 is a gas-permeable electrode as described in the above technical solution. The porous gas-permeable layer of the gas-permeable electrode is arranged downward.
[0066] An anode 8 is horizontally disposed at the upper portion of the reaction tower 12 , and a closed reaction chamber 7 is formed between the cathode 6 , the anode 8 and the side wall of the reaction tower 12 .
[0067] In one embodiment of the present invention, the bottom end of the reaction tower 12 is provided with an air inlet 5 .
[0068] In one embodiment of the present invention, the ozone generating device comprises an oxygen cylinder 1 and an ozone generator 2 which are connected in sequence, and the ozone generator 2 is connected to the air inlet 5 .
[0069] In one embodiment of the present invention, an ozone detector 3 and a mass flow meter 4 are further provided between the ozone generator 2 and the air inlet 5 .
[0070] In the present invention, in a specific application process, the reaction chamber is filled with a solution to be treated, one side of the porous catalyst layer of the gas-penetrating electrode is in contact with the liquid, and gaseous oxygen and ozone must first pass through the porous catalyst layer of the cathode before entering the reaction chamber. This process forms a three-phase reaction interface in the porous catalyst layer, namely, a gas-liquid-solid three-phase interface, on which an electrode reaction occurs. In this way, the gas-penetrating electrode can effectively utilize gaseous substances, thereby significantly improving the utilization rate of the gas. Due to the improvement in gas utilization, the gas-penetrating electrode not only improves the reaction rate, but also reduces the overpotential and reduces energy input.
[0071] In one embodiment of the present invention, the anode 8 is preferably a coated titanium electrode. In the present invention, the coated titanium electrode preferably comprises a titanium substrate and a tantalum-iridium coating on the surface of the titanium substrate; the thickness of the coated titanium electrode is preferably 1 mm, and the thickness of the tantalum-iridium coating is preferably 4-6 μm.
[0072] In one embodiment of the present invention, the cathode 6 and the anode 8 are preferably connected via a DC power supply 10 .
[0073] In one embodiment of the present invention, a gas outlet 13 is provided at the top of the reaction tower 12, and a tail gas chamber 9 is formed between the anode 8 and the gas outlet 13. In one embodiment of the present invention, the gas outlet 13 is connected to an ozone destroyer 11.
[0074] In an embodiment of the present invention, the schematic diagram of the gas-lift liquid flow type electro-ozone device is as follows: Figure 5 As shown, 1 is an oxygen cylinder, 2 is an ozone generator, 3 is an ozone detector, 4 is a mass flow meter, 5 is an air inlet, 6 is a cathode, 7 is a reaction chamber, 8 is an anode, 9 is an exhaust chamber, 10 is a DC power supply, 11 is an ozone destruction chamber, 12 is a reaction tower, and 13 is an air outlet.
[0075] In the present invention, when the gaslift liquid flow type electro-ozone device is used to degrade organic pollutants, the specific process of the degradation is preferably:
[0076] Step 1: After the oxygen flows out of the oxygen cylinder, it reaches the ozone generator, where part of the oxygen is converted into ozone to obtain an ozone / oxygen mixed gas;
[0077] Step 2: The ozone / oxygen mixed gas passes through an ozone detector (to detect ozone concentration) and a mass flow meter (to control gas flow) in sequence, and then enters the reaction tower through the air inlet at the bottom of the reaction tower;
[0078] Step 3: The ozone / oxygen mixed gas passes through the gas permeable electrode (cathode), and a chemical reaction occurs at the cathode: oxygen undergoes a two-electron oxygen reduction reaction at the cathode to generate hydrogen peroxide, and at the same time, part of the ozone is directly reduced by the cathode to generate hydroxyl radicals; subsequently, the hydrogen peroxide and hydroxyl radicals diffuse into the solution in the reaction chamber;
[0079] Generate hydrogen peroxide: O2+2H + +2e - →H2O2
[0080] Ozone reduction generates hydroxyl radicals:
[0081]
[0082]
[0083] ·HO3→O2+·OH
[0084] Step 4: The remaining unreacted mixed gas diffuses into the solution to form bubbles, which rise under the action of buoyancy. During the rising process, oxygen and ozone continuously contact with the solution and diffuse into the solution to form dissolved oxygen and ozone.
[0085] Step 5: The dissolved oxygen and ozone return to the cathode to react as described in step 3, and the dissolved ozone and hydrogen peroxide react to generate hydroxyl radicals, which react with the pollutants to degrade them;
[0086] 2O3+H2O2→2·OH+3O2
[0087] Step 6: The gas escaping from the solution enters the tail gas chamber and is then discharged after being treated by the ozone destructor.
[0088] The technical solutions in the present invention will be described clearly and completely below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0089] Example 1
[0090] Chitosan and NiCl2·6H2O were mixed in a mass ratio of 2:1 and stirred at 120°C for 8 h until dry; the mixture was then placed in a tubular furnace, heated to 800°C in a nitrogen atmosphere, and kept warm for 60 min for calcination; the calcined product was acid-washed with 1 mol / L HCl at 120°C for 12 h, and washed with deionized water several times until the washing liquid was neutral, and the product was dried at 80°C in a vacuum oven, and ball milled (ball-to-material ratio of 1:1, rotation speed of 600 r / min, time of 4 h) to obtain biochar material.
[0091] Figure 1 The SEM image of the biochar material obtained is Figure 1 It can be seen that the obtained biochar material is an agglomerate formed by irregular blocks or spherical particles, and has a porous structure on the surface;
[0092] The element contents in the obtained biochar material were tested, where C, H and O were tested by XPS, and Ni was tested by ICP-OES. The test results are shown in Table 1:
[0093] Table 1 Element content of biochar material obtained in Example 1
[0094] Material C (atom%) N (atom%) O(atom%) Ni(atom%) Ni@NC-0.50 87.25% 2.73% 9.35% 0.66%
[0095] Among them, through XPS Ni fine spectrum peak analysis, it can be known that the atomic content of nickel in the nickel element is 13%.
[0096] Figure 2 The XRD pattern of the obtained biochar material is Figure 2 It can be seen that the obtained biochar material contains Ni nanoparticles, and the carbon material is atypical amorphous carbon material with a certain degree of graphitization.
[0097] The catalytic performance of biochar materials and commercially available conductive carbon black (model XFI15) for the two-electron oxygen reduction reaction was tested;
[0098] The test method is: accurately weigh 5 mg of catalyst and add it to 2 mL of ethanol and 20 μL of Nafion solution, and use an ultrasonic probe to work at 100 W for 10 minutes to obtain a uniformly dispersed catalyst ink. Drop 10 μL of catalyst ink on a glassy carbon disk (area 0.2475 cm) twice. 2, collection efficiency 36%), and after the film is formed, it is installed in the RRDE instrument for testing. RRDE measurement is carried out in a five-port electrolytic cell using a constant potentiostat (PINE, USA). The glassy carbon electrode coated with a catalyst is the working electrode, the Hg / HgO electrode is the reference electrode, the stone mill rod electrode is the counter electrode, and the electrolyte is 50mL, 100mM KOH solution. In the test, N2 is first introduced for 10 minutes to exhaust other gases in the solution, and then the working potential is 100mV·s -1 The electrode was activated by scanning the cyclic voltammetry curve, and this was repeated 20 times until a stable CV curve was obtained. -1 O2 was introduced for 5 minutes to saturate the solution with dissolved oxygen, and the speed of the RRDE device was set to 1600 r / min. The H2O2 oxidation current curve was obtained by scanning the It curve at a constant potential (1.2 V vs. RHE). Based on the obtained disk current and ring current, the 2e of the material can be calculated. - ORR selectivity is calculated as follows:
[0099]
[0100] Among them, I R is the ring current, I D is the disk current, and N is the collection efficiency of the electrode (calibrated to be 36%).
[0101] The test results obtained are as follows Figure 6 and Figure 7 As shown, Figure 6 The LSV curves and H2O2 oxidation current test results of the two-electron oxygen reduction reaction of biochar materials and commercially available conductive carbon black; Figure 7 is the two-electron selectivity calculated from the LSV curve and H2O2 oxidation current;
[0102] Depend on Figure 6 and Figure 7 It can be seen that the biochar material obtained by the present invention has a higher hydrogen peroxide oxidation current and selectivity than commercially available conductive carbon black, indicating that the biochar material provided by the present invention has a higher catalytic activity. Therefore, the electrode provided by the present invention can significantly reduce costs and promote the expanded application of electro-ozone on the basis of improving catalytic activity.
[0103] Example 2
[0104] The biochar material obtained in Example 1 was used to prepare a gas permeation electrode;
[0105] Under the assistance of ultrasound, a 60% mass concentration of PTFE solution and biochar material are evenly dispersed in anhydrous ethanol (the volume of PTFE solution is 0.166% of the volume of ethanol; the concentration of biochar material is 4.536g / L) to obtain a slurry. The porous hydrophobic carbon paper is placed on a heating plate at 110°C, and the slurry is evenly sprayed on one side of the hydrophobic carbon paper using a spray pen device. After it is dried, it is heat treated at 330°C in a muffle furnace for 30 minutes to obtain a gas-penetrating electrode, wherein the content of biochar material in the gas-penetrating electrode is 1mg / cm 2 .
[0106] Among them, the actual picture of porous hydrophobic carbon paper is as follows Figure 3 As shown in (a), the thickness is 0.19 mm; the physical picture of the gas permeable electrode is as follows Figure 3 (b) is shown; the structural diagram is shown Figure 4 As shown, 1 is a porous hydrophobic carbon paper and 2 is a porous catalyst layer.
[0107] Example 3
[0108] The gas-penetrating electrode obtained in Example 2 was used as the cathode to assemble a gas-lift liquid flow electro-ozone device (the schematic diagram of the device is shown in FIG. Figure 5 shown);
[0109] The anode is a coated titanium electrode (the substrate is a titanium substrate, and the thickness of the titanium coating is a tantalum-iridium coating of 5 μm);
[0110] The cathode and the anode are horizontally arranged at the lower part and the upper part of the reaction tower respectively, wherein the porous gas permeable layer of the gas permeable electrode is arranged downward; the cathode and the anode form a closed reaction chamber with the side wall of the reaction tower; the cathode and the anode are connected through a DC power supply;
[0111] A tail gas chamber is formed between the anode and the gas outlet of the reaction tower; the gas outlet of the reaction tower is connected to an ozone destroyer;
[0112] The air inlet of the reaction tower is connected in sequence with a mass flow meter, an ozone detector, an ozone generator and an oxygen cylinder.
[0113] Application Example 1
[0114] The airlift liquid flow electro-ozone device of Example 3 was used to degrade ibuprofen;
[0115] The initial ibuprofen concentration was 20 mg / L, the solution was 0.05 M Na2SO4 solution, the gas flow rate was 40 mL / min, the ozone concentration was 70 mg / L, and the current density was 4 mA / cm 2 .
[0116] A conventional ozone oxidation device and an electrolysis device with the same gas flow rate and ozone concentration were used as comparative examples; the ozone oxidation device was operated under the same conditions as the gas-lift liquid flow type electro-ozone device of the present invention except that no current was applied. The electrolysis device was operated under the same conditions as the gas-lift liquid flow type electro-ozone device of the present invention except that the ozone generator was not turned on.
[0117] Test results such as Figure 8 As shown, ibuprofen at high concentration can be completely removed within 15 minutes using the gas-lift liquid flow electro-ozone device provided by the present invention, and the required current is only 28 mA, with extremely low energy consumption. In the comparative example, the degradation rate of the ozone oxidation device at 20 minutes was 95%, which could not achieve complete removal. The degradation rate of the electrolysis device at 20 minutes was 15%. This result fully illustrates the excellent performance of the gas-lift liquid flow electro-ozone device provided by the present invention in degrading difficult-to-degrade pollutants, indicating that the device has broad application prospects and high practical value in the fields of environmental protection and industrial wastewater treatment.
[0118] Application Example 2
[0119] The gas-lift liquid flow ozone device in Example 3 was used to degrade ibuprofen at different current densities. The initial ibuprofen concentration was 20 mg / L, the solution was 0.05 M Na2SO4 solution, the gas flow rate was 40 mL / min, and the ozone concentration was 70 mg / L. The test results are as follows: Fig. 9 As shown in Table 2;
[0120] Table 2 Degradation effect of ibuprofen at different current densities
[0121]
[0122] It can be seen from Table 2 that the degradation efficiency of the airlift liquid flow ozone device provided by the present invention is superior to that of the traditional ozone oxidation method at different current densities.
[0123] Although the above embodiment describes the present invention in detail, it is only a part of the embodiments of the present invention, not all of the embodiments. Other embodiments can be obtained based on this embodiment without creativity, and these embodiments all fall within the protection scope of the present invention.
Claims
1. A biochar material, characterized in that: It includes a biochar matrix and an active component loaded in the biochar matrix; The active ingredients include metal elements and metal ions; The metal element in the metal element and the metal ion is of the same type; The metal element includes a transition metal element, and the transition metal element includes iron, manganese, copper, zinc, cobalt or nickel.
2. The biochar material according to claim 1, characterized in that: The atomic content of the metal element in the active ingredient is 10% to 20%; The atomic content of active components in the biochar material is 0.5% to 2%.
3. The biochar material according to claim 1 or 2, characterized in that: The biochar material is also doped with nitrogen; the atomic content of nitrogen in the biochar material is 2% to 10%.
4. The method for preparing the biochar material according to any one of claims 1 to 3, characterized in that: include: Mixing the biomass raw material and the metal salt, and calcining them to obtain the biochar material; The metal salt includes a transition metal salt, and the transition metal salt includes an iron salt, a manganese salt, a copper salt, a zinc salt, a cobalt salt or a nickel salt.
5. The preparation method according to claim 4, characterized in that: The biomass raw material includes one or more of chitosan, sodium alginate, gelatin, plant residues, wood and bamboo; the plant residues include one or more of tea residues, olive residues, coffee residues, fruit peels, straw and fruit shells; The calcination temperature is 800-900° C., and the heat preservation time is 40-90 minutes; the calcination is carried out under a protective atmosphere.
6. Use of the biochar material according to any one of claims 1 to 3 or the biochar material prepared by the preparation method according to claim 4 or 5 as a catalyst in preparing a cathode of an electric ozone device.
7. A gas permeable electrode, characterized in that: It includes a porous gas-permeable layer and a porous catalyst layer stacked in sequence; The material of the porous catalyst layer includes a catalyst and a binder; The catalyst is the biochar material according to any one of claims 1 to 3 or the biochar material prepared by the preparation method according to claim 4 or 5.
8. The gas permeable electrode according to claim 7, characterized in that: The content of the catalyst in the gas permeable electrode is 0.5-5 mg / cm 2 .
9. An airlift liquid flow type electric ozone device, characterized in that: It comprises a reaction tower (12) and an ozone generating device connected to the bottom end of the reaction tower (12); A cathode (6) is horizontally arranged at the lower part of the reaction tower (12), wherein the cathode (6) is a gas-permeable electrode according to claim 7 or 8, and the porous gas-permeable layer of the gas-permeable electrode is arranged downward; An anode (8) is horizontally arranged at the upper part of the reaction tower (12), and a closed reaction chamber (7) is formed between the cathode (6) and the anode (8) and the side wall of the reaction tower (12).
10. The airlift liquid flow type electric ozone device according to claim 9, characterized in that: The anode (8) is a coated titanium electrode; The bottom end of the reaction tower (12) is provided with an air inlet (5); The ozone generating device comprises an oxygen cylinder (1) and an ozone generator (2) which are connected in sequence, and the ozone generator (2) is connected to the air inlet (5).
Citation Information
Patent Citations
Method for anode and cathode synergistic oxidized electro-catalysis-ozonation
CN106335998A
Preparation method and application of novel biomass-based functional nano material
CN108620075A
Preparation method of charcoal-loaded zero-valent iron catalytic material
CN109225221A
Circulating overflow type electric assisted ozone water treatment equipment as well as method for treating water thereby
CN110642340A
Preparation method and application of zero-valent iron-loaded biochar material
CN112354532A
Cited By
Gas-liquid mixed electrochemical oxidation device
CN120841662A