Preparation method and application of hydroxyapatite loaded silver phosphate hybrid material
By loading silver phosphate in situ on nano-natural hydroxyapatite, the problems of poor dispersion and reduced catalytic activity in water were solved, and an efficient water pollution treatment material was formed, using fish bone resources, and aquaculture was solved The problems of pollution and resource waste have achieved effective treatment of organic matter and heavy metals.
Patent Information
- Application Number
- CN202411052299.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-01
- Publication Date
- 2024-11-19
AI Technical Summary
The existing silver phosphate has poor dispersion in water, and its catalytic activity and antibacterial properties decrease with the reaction, making it difficult to widely use in water pollution treatment. Moreover, the pollution problems in the aquaculture industry are serious and it has failed to effectively utilize the fish bone resources in the fishery processing process.
By reacting hydroxyapatite with silver phosphate, silver phosphate is loaded in situ on the surface of nano-natural hydroxyapatite to improve its dispersion and photodegradation activity in water, and nano-natural hydroxyapatite is prepared by using salmon fish bones. , forming nano-natural hydroxyapatite in situ supported silver phosphate hybrid material.
It significantly improves the stability and photocatalytic activity of silver phosphate, enhances the adsorption capacity of organic matter and heavy metals, provides an efficient water pollution treatment material, reduces the environmental burden and realizes sustainable utilization of resources.
Smart Images

Figure CN118978135A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of new materials, and in particular relates to a preparation method and application of a novel hybrid material based on in-situ loading of silver phosphate on nano-natural hydroxyapatite. Background Art
[0002] With the rapid development of the aquaculture industry, the problem of aquaculture water pollution caused by aquaculture is becoming increasingly serious, causing huge economic losses to the aquaculture industry. Various metabolic organic substances in the aquaculture process and the excessive use of antibiotics have aggravated the pollution of aquaculture water. Photocatalytic technology is an emerging green and environmentally friendly purification technology, which has been deeply developed in the fields of energy development and environmental purification (photolysis of organic pollutants). Silver phosphate itself has high photocatalytic activity and high antibacterial ability, and is widely used in the fields of photocatalysis and antibacterial. Because the synthesized silver phosphate powder has poor dispersibility and is extremely difficult to dissolve in water, silver phosphate has not been widely used in the field of water pollution treatment so far. And as the catalytic reaction proceeds, the silver element on the surface of silver phosphate will increase, forming a black coating layer, which hinders the catalyst from absorbing light and reduces the active sites, which seriously reduces the photocatalytic activity and antibacterial properties of silver phosphate.
[0003] During the processing of salmon, many by-products that still have utilization value are produced, especially salmon bones, which are the waste produced during the initial processing to obtain edible fish meat. They account for about 50% of the total weight and are not fully utilized. Most of them are directly discarded as waste, which not only imposes a burden on the environment, but also causes a waste of high-value resources.
[0004] Hydroxyapatite is the main natural inorganic component in fish bones. It is non-toxic and has almost no pollution to the environment. At the same time, natural hydroxyapatite has a flexible structure, its surface is easily replaced by metals, and it has a high specific surface area after being prepared into nano-scale materials. Therefore, nano-scale natural hydroxyapatite is also a good catalyst carrier material. It has high ion exchange and adsorption capacity, which can not only retain the characteristics of the catalyst itself, but also improve its adsorption capacity for other metal ions. By reacting silver nitrate with nano-natural hydroxyapatite, silver ions react with phosphate ions contained in hydroxyapatite itself to form silver phosphate and load it on the surface in situ, obtaining a nano-natural hydroxyapatite silver phosphate hybrid material with unique properties and wide application. Summary of the invention
[0005] The present invention aims to provide a hybrid material based on nano-natural hydroxyapatite in-situ loaded silver phosphate (nHAP-Ag 3 PO 4) preparation method and use in aquaculture wastewater treatment, effectively utilizing nano-natural hydroxyapatite made from fish bone materials discarded in the fishery processing process, in-situ loading silver phosphate onto the surface of nano-natural hydroxyapatite through the reaction of hydroxyapatite and silver phosphate, effectively improving the dispersibility, stability and photodegradation activity of silver phosphate in water.
[0006] To achieve the above object, the technical solution of the present invention is:
[0007] A method for preparing a hydroxyapatite-loaded silver phosphate hybrid material, the preparation method comprising the following steps:
[0008] (1) Thawing salmon bones in running water and mincing them into minced fish using a 3 mm perforated plate table meat grinder;
[0009] (2) Grinding the surimi in step (1) using a colloid mill (add 50 mL of deionized water to 1 g of surimi) and treating with a tissue homogenizer for 10 min;
[0010] (3) The protein homogenate in step (2) was titrated with HCl solution, placed in a 4°C refrigerator for 15 min, taken out and centrifuged at 11000 r / min for 20 min, the supernatant was discarded, and the precipitate was retained;
[0011] (4) mixing the precipitate in step (3) with deionized water in a volume ratio of 1:1, boiling at 100° C. for 2 h, drying in a 50° C. oven for 48 h, and then calcining in a muffle furnace at 700° C. for 4 h to obtain natural hydroxyapatite powder;
[0012] (5) The hydroxyapatite powder in step (4) was ground in a ball mill at 600 r / min for 10 h with a material-liquid ratio (natural hydroxyapatite powder (g): deionized water (mL)) of 1:20, using 5 mm grinding balls, and then ground again at the same speed for 10 h using 0.5 mm grinding balls to obtain nano-natural hydroxyapatite material;
[0013] (6) preparing 50 mM silver nitrate solution;
[0014] (7) Mix 10 mL of the silver nitrate solution in step (6) with 85 mg of the hydroxyapatite in step (5), react at room temperature in the dark for 6 h, centrifuge at 11000 r / min for 20 min, discard the supernatant, wash three times with deionized water, and dry in an oven at 50°C for 48 h.
[0015] The pH value of the HCl titration in step (3) is 2.0-5.0, preferably 2.0.
[0016] Preferably, the particle size of the prepared nano-natural hydroxyapatite in-situ loaded silver phosphate hybrid material is about 100 nm.
[0017] The nano-natural hydroxyapatite in-situ loaded silver phosphate hybrid material prepared according to the above preparation method also falls within the protection scope of the present invention.
[0018] Moreover, it has been verified through experiments that the nano-natural hydroxyapatite in-situ loaded silver phosphate hybrid material prepared by the present invention has excellent photocatalytic degradation of organic matter, adsorption of heavy metal pollutants, and killing of harmful bacteria in water bodies. Therefore, it can be applied to degradation of organic matter, adsorption of heavy metal pollutants, killing of harmful bacteria in water bodies, etc., and can be used as a wastewater treatment adsorbent, antibacterial agent, etc.
[0019] The present invention has the following advantages:
[0020] 1. The present invention uses salmon bones to make nano-natural hydroxyapatite, which is easy to obtain and can utilize waste. It not only effectively utilizes natural resources and reduces environmental burden, but can also be applied to the treatment of water pollution, and has the advantages of being green and sustainable.
[0021] 2. The present invention utilizes the characteristics of high surface area, flexible structure and easy metal substitution of nano-natural hydroxyapatite to load silver phosphate on the surface of nano-hydroxyapatite in situ, thereby effectively improving the stability and photodegradation activity of silver phosphate in water.
[0022] 3. This new material not only has good stability, but also has excellent ability to photocatalytically degrade organic matter, adsorb heavy metal pollutants, and kill harmful bacteria in water bodies.
[0023] 4. The present invention greatly improves the dispersibility of silver phosphate in water, and this method can not only improve the response efficiency of silver phosphate photocatalyst to visible light, but also reduce the photocorrosion phenomenon of silver phosphate, and finally improve the photocatalytic activity of silver phosphate. 3 PO 4 It has good photocatalytic degradation efficiency for organic dyes and tetracycline in aquaculture wastewater, and has high heavy metal adsorption capacity, providing a new type of nanomaterial for aquaculture wastewater treatment. Therefore, the nano-natural hydroxyapatite in-situ loaded silver phosphate hybrid material has important significance and great application value in the photocatalytic degradation of organic pollutants produced in aquaculture. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 A transmission electron microscope image of an embodiment;
[0025] Figure 2 A particle size distribution diagram of an embodiment;
[0026] Figure 3 The zeta potential diagram of the novel hybrid material, nano-natural hydroxyapatite and silver phosphate prepared in one embodiment;
[0027] Figure 4 The XRD spectrum of the novel hybrid material, nano-natural hydroxyapatite, prepared in one embodiment;
[0028] Figure 5 is a Fourier transform infrared spectrum of the novel hybrid material, nano-natural hydroxyapatite and silver phosphate prepared in an embodiment;
[0029] Figure 6 The figure is a UV-visible diffuse reflection absorption spectrum of the novel hybrid material, nano-natural hydroxyapatite and silver phosphate prepared in one embodiment;
[0030] Figure 7 This is a graph showing the thermogravimetric test results of a novel hybrid material prepared in an embodiment;
[0031] Figure 8 The experimental results of the photocatalytic degradation of organic dyes methylene blue (MB), methylene orange (MO) and rhodamine B (RhB), and antibiotic tetracycline (TC) by the prepared new hybrid material are shown in the figure. Figure 8 a. Figure 8 b. Figure 8 c. Figure 8 d are the experimental results of photocatalytic degradation of MB, MO, RhB and TC by the prepared new composite materials;
[0032] Fig. 9 This is a graph showing the experimental results of the cyclic stability analysis of the photocatalytic degradation of organic matter by the novel hybrid material prepared in one embodiment;
[0033] Fig.10 This is a diagram showing the results of a heavy metal adsorption experiment on a novel hybrid material prepared in an embodiment;
[0034] Fig.11 This is a graph showing the antibacterial test results of the novel hybrid material prepared in one embodiment. DETAILED DESCRIPTION
[0035] The present invention will be described in detail below through specific embodiments. These embodiments are provided to enable a more thorough understanding of the present invention and to fully convey the scope of the present invention to those skilled in the art.
[0036] As used throughout the specification and claims, "including" or "comprising" is an open term and should be interpreted as "including but not limited to". The specification subsequently describes the preferred embodiments of the present invention, but the description is for the purpose of the general principles of the specification and is not intended to limit the scope of the present invention. The scope of protection of the present invention shall be determined by the attached claims.
[0037] Unless otherwise specified, all methods used in the present invention are conventional methods, and all materials and reagents can be obtained through commercial channels.
[0038] Example 1 A method for preparing a hybrid material based on in-situ loading of silver phosphate on nano-natural hydroxyapatite comprises the following steps:
[0039] (1) Thaw salmon bones in running water and mince them into minced fish using a 3 mm perforated plate table meat grinder.
[0040] (2) Grind the minced fish in step (1) using a colloid mill (add 50 mL of deionized water to 1 g of minced fish) and process with a tissue homogenizer for 10 min.
[0041] (3) The protein homogenate in step (2) was titrated to pH = 2 with HCl solution, placed in a 4°C refrigerator for 15 min, taken out and centrifuged at 11000 r / min for 20 min, the supernatant was discarded, and the precipitate was retained.
[0042] (4) The precipitate in step (3) was mixed with deionized water in a volume ratio of 1:1, boiled at 100° C. for 2 h, dried in a 50° C. oven for 48 h, and then calcined in a muffle furnace at 700° C. for 4 h to obtain natural hydroxyapatite powder.
[0043] (5) The hydroxyapatite powder in step (4) was ground at a material-liquid ratio (natural hydroxyapatite powder (g): deionized water (mL)) of 1:20 using a 5 mm grinding ball and a ball mill at 600 r / min for 10 h; then, a 0.5 mm grinding ball was used and ground at the same speed for 10 h to obtain a nano-natural hydroxyapatite material.
[0044] (6) Prepare 50 mM silver nitrate solution.
[0045] (7) Mix 10 mL of the silver nitrate solution in step (6) with 85 mg of the hydroxyapatite in step (5), react at room temperature in the dark for 6 h, centrifuge at 11000 r / min for 20 min, discard the supernatant, wash three times with deionized water, and dry in an oven at 50°C for 48 h.
[0046] Example 2 A method for preparing a hybrid material based on in-situ loading of silver phosphate on nano-natural hydroxyapatite comprises the following steps:
[0047] (1) Thaw salmon bones in running water and mince them into minced fish using a 3 mm perforated plate table meat grinder.
[0048] (2) Grind the minced fish in step (1) using a colloid mill (add 50 mL of deionized water to 1 g of minced fish) and process with a tissue homogenizer for 10 min.
[0049] (3) The protein homogenate in step (2) was titrated to pH = 2 with HCl solution, placed in a 4°C refrigerator for 15 min, taken out and centrifuged at 11000 r / min for 20 min, the supernatant was discarded, and the precipitate was retained.
[0050] (4) The precipitate in step (3) was mixed with deionized water in a volume ratio of 1:1, boiled at 100° C. for 2 h, dried in a 50° C. oven for 48 h, and then calcined in a muffle furnace at 700° C. for 4 h to obtain natural hydroxyapatite powder.
[0051] (5) The hydroxyapatite powder in step (4) is ground at a material-liquid ratio (natural hydroxyapatite powder (g): deionized water (mL)) of 1:20, and ground with a ball mill at 600 r / min for 5 min; then ground with a ball mill at 0.5 min and at the same speed for 6 h to obtain a nano-natural hydroxyapatite material.
[0052] (6) Prepare 50 mM silver nitrate solution.
[0053] (7) Mix 10 mL of the silver nitrate solution in step (6) with 85 mg of the hydroxyapatite in step (5), react at room temperature in the dark for 6 h, centrifuge at 11000 r / min for 20 min, discard the supernatant, wash three times with deionized water, and dry in an oven at 50°C for 48 h.
[0054] Example 3 A method for preparing a hybrid material based on in-situ loading of silver phosphate on nano-natural hydroxyapatite comprises the following steps:
[0055] (1) Thaw salmon bones in running water and mince them into minced fish using a 3 mm perforated plate table meat grinder.
[0056] (2) Grind the minced fish in step (1) using a colloid mill (add 50 mL of deionized water to 1 g of minced fish) and process with a tissue homogenizer for 10 min.
[0057] (3) The protein homogenate in step (2) was titrated to pH = 2 with HCl solution, placed in a 4°C refrigerator for 15 min, taken out and centrifuged at 11000 r / min for 20 min, the supernatant was discarded, and the precipitate was retained.
[0058] (4) The precipitate in step (3) was mixed with deionized water in a volume ratio of 1:1, boiled at 100° C. for 2 h, dried in a 50° C. oven for 48 h, and then calcined in a muffle furnace at 700° C. for 4 h to obtain natural hydroxyapatite powder.
[0059] (5) The hydroxyapatite powder in step (4) was ground at a material-liquid ratio (natural hydroxyapatite powder (g): deionized water (mL)) of 1:20 using a 5 mm grinding ball and a ball mill at 600 r / min for 14 h; then, a 0.5 mm grinding ball was used and ground at the same speed for 14 h to obtain a nano-natural hydroxyapatite material.
[0060] (6) Prepare 50 mM silver nitrate solution.
[0061] (7) Mix 10 mL of the silver nitrate solution in step (6) with 85 mg of the hydroxyapatite in step (5), react at room temperature in the dark for 6 h, centrifuge at 11000 r / min for 20 min, discard the supernatant, wash three times with deionized water, and dry in an oven at 50°C for 48 h.
[0062] Example 4 A method for preparing a hybrid material based on in-situ loading of silver phosphate on nano-natural hydroxyapatite comprises the following steps:
[0063] (1) Thaw salmon bones in running water and mince them into minced fish using a 3 mm perforated plate table meat grinder.
[0064] (2) Grind the minced fish in step (1) using a colloid mill (add 50 mL of deionized water to 1 g of minced fish) and process with a tissue homogenizer for 10 min.
[0065] (3) The protein homogenate in step (2) was titrated to pH = 2 with HCl solution, placed in a 4°C refrigerator for 15 min, taken out and centrifuged at 11000 r / min for 20 min, the supernatant was discarded, and the precipitate was retained.
[0066] (4) The precipitate in step (3) was mixed with deionized water in a volume ratio of 1:1, boiled at 100° C. for 2 h, dried in a 50° C. oven for 48 h, and then calcined in a muffle furnace at 700° C. for 4 h to obtain natural hydroxyapatite powder.
[0067] (5) The hydroxyapatite powder in step (4) is ground at a material-liquid ratio (natural hydroxyapatite powder (g): deionized water (mL)) of 1:20 using a 5 mm grinding ball and a ball mill at 400 r / min for 10 h; then, a 0.5 mm grinding ball is used and ground at the same speed for 10 h to obtain a nano-natural hydroxyapatite material.
[0068] (6) Prepare 50 mM silver nitrate solution.
[0069] (7) Mix 10 ml of the silver nitrate solution in step (6) with 75 mg of the hydroxyapatite in step (5), react at room temperature in the dark for 6 h, centrifuge at 11000 r / min for 20 min, discard the supernatant, wash three times with deionized water, and dry in an oven at 50°C for 48 h.
[0070] Example 5 A method for preparing a hybrid material based on in-situ loading of silver phosphate on nano-natural hydroxyapatite comprises the following steps:
[0071] (1) Thaw salmon bones in running water and mince them into minced fish using a 3 mm perforated plate table meat grinder.
[0072] (2) Grind the minced fish in step (1) using a colloid mill (add 50 mL of deionized water to 1 g of minced fish) and process with a tissue homogenizer for 10 min.
[0073] (3) The protein homogenate in step (2) was titrated to pH = 2 with HCl solution, placed in a 4°C refrigerator for 15 min, taken out and centrifuged at 11000 r / min for 20 min, the supernatant was discarded, and the precipitate was retained.
[0074] (4) The precipitate in step (3) was mixed with deionized water in a volume ratio of 1:1, boiled at 100° C. for 2 h, dried in a 50° C. oven for 48 h, and then calcined in a muffle furnace at 700° C. for 4 h to obtain natural hydroxyapatite powder.
[0075] (5) The hydroxyapatite powder in step (4) was ground at a material-liquid ratio (natural hydroxyapatite powder (g): deionized water (mL)) of 1:20 using a 5 mm grinding ball and a ball mill at 800 r / min for 10 h; then, a 0.5 mm grinding ball was used and ground at the same speed for 10 h to obtain a nano-natural hydroxyapatite material.
[0076] (6) Prepare 50 mM silver nitrate solution.
[0077] (7) Mix 10 mL of the silver nitrate solution in step (6) with 25 mg of the hydroxyapatite in step (5), react at room temperature in the dark for 6 h, centrifuge at 11000 r / min for 20 min, discard the supernatant, wash three times with deionized water, and dry in an oven at 50°C for 48 h.
[0078] Example 6 A method for preparing a hybrid material based on in-situ loading of silver phosphate on nano-natural hydroxyapatite comprises the following steps:
[0079] (1) Thaw salmon bones in running water and mince them into minced fish using a 3 mm perforated plate table meat grinder.
[0080] (2) Grind the minced fish in step (1) using a colloid mill (add 50 mL of deionized water to 1 g of minced fish) and process with a tissue homogenizer for 10 min.
[0081] (3) The protein homogenate in step (2) was titrated to pH = 2 with HCl solution, placed in a 4°C refrigerator for 15 min, taken out and centrifuged at 11000 r / min for 20 min, the supernatant was discarded, and the precipitate was retained.
[0082] (4) The precipitate in step (3) was mixed with deionized water in a volume ratio of 1:1, boiled at 100° C. for 2 h, dried in a 50° C. oven for 48 h, and then calcined in a muffle furnace at 700° C. for 4 h to obtain natural hydroxyapatite powder.
[0083] (5) The hydroxyapatite powder in step (4) is ground at a material-liquid ratio (natural hydroxyapatite powder (g): deionized water (mL)) of 1:20 using a 5 mm grinding ball and a ball mill at 1000 r / min for 10 h; then, a 0.5 mm grinding ball is used and ground at the same speed for 10 h to obtain a nano-natural hydroxyapatite material.
[0084] (6) Prepare 100 mM silver nitrate solution.
[0085] (7) Mix 10 mL of the silver nitrate solution in step (6) with 50 mg of the hydroxyapatite in step (5), react at room temperature in the dark for 6 h, centrifuge at 11000 r / min for 20 min, discard the supernatant, wash three times with deionized water, and dry in an oven at 50°C for 48 h.
[0086] Example 7 A method for preparing a hybrid material based on in-situ loading of silver phosphate on nano-natural hydroxyapatite comprises the following steps:
[0087] (1) Thaw salmon bones in running water and mince them into minced fish using a 3 mm perforated plate table meat grinder.
[0088] (2) Grind the minced fish in step (1) using a colloid mill (add 50 mL of deionized water to 1 g of minced fish) and process with a tissue homogenizer for 10 min.
[0089] (3) The protein homogenate in step (2) was titrated to pH = 2 with HCl solution, placed in a 4°C refrigerator for 15 min, taken out and centrifuged at 11000 r / min for 20 min, the supernatant was discarded, and the precipitate was retained.
[0090] (4) The precipitate in step (3) was mixed with deionized water in a volume ratio of 1:1, boiled at 100° C. for 2 h, dried in a 50° C. oven for 48 h, and then calcined in a muffle furnace at 700° C. for 4 h to obtain natural hydroxyapatite powder.
[0091] (5) The hydroxyapatite powder in step (4) was ground at a material-liquid ratio (natural hydroxyapatite powder (g): deionized water (mL)) of 1:20 using a 10 mm grinding ball and a ball mill at 600 r / min for 10 h; then ground at the same speed for 10 h using a 1 mm grinding ball to obtain a nano-natural hydroxyapatite material.
[0092] (6) Prepare 200 mM silver nitrate solution.
[0093] (7) Mix 10 mL of the silver nitrate solution in step (6) with 100 mg of the hydroxyapatite in step (5), react at room temperature in the dark for 6 h, centrifuge at 11000 r / min for 20 min, discard the supernatant, wash three times with deionized water, and dry in an oven at 50°C for 48 h.
[0094] After multiple control experiments, it was concluded that nHAP-Ag prepared in an ultrapure water reaction system with a mass ratio of 1:1 between nano-natural hydroxyapatite and silver nitrate under the conditions of pH 2.0 titration and room temperature 3 PO 4 The composite material is the best synthesis method for this investigation. nHAP-Ag was observed by transmission electron microscopy 3 PO 4 The hybrid material is an irregular ellipsoid or rod-shaped material of about 82 nm. Figure 1 ). nHAP-Ag measured by laser particle size analyzer 3 PO 4 The average hydrated particle size of the hybrid material is around 158.64 nm ( Figure 2 ). Zeta potential measurement found that the surface of nHAP carries a negative charge with an absolute potential of 2.65mV; Ag 3 PO 4 The surface carries a positive charge, and the absolute value of the potential is 92.36mV; nHAP-Ag 3 PO 4 Carrying positive charge, the absolute value of potential is 19.58mV ( Figure 3 ), it can be seen that the surface of nHAP should be successfully loaded with Ag 3 PO 4 .
[0095] nHAP and nHAP-Ag 3 PO 4 The XRD spectrum of Figure 4 As shown. The diffraction peak angles corresponding to nHAP are 30°, 32.1°, 34.9° and 41.2°, respectively, which correspond to the nHAP standard spectrum (200), (211), (300) and (310); nHAP-Ag 3 PO 4 The corresponding diffraction peak angles are 29.6°, 33.2° and 36.5°, which are consistent with the known literature. 3 PO 4 The corresponding diffraction peak angles of 30°, 33° and 36° are basically consistent, and are also consistent with Ag 3 PO 4 The standard spectra (200), (210) and (211) correspond to each other. + With PO 43- Reaction to generate Ag 3 PO 4 And successfully loaded on the surface of nHAP.
[0096] Fourier transform infrared spectroscopy was used to characterize nHAP-Ag 3 PO 4 The structure of the hybrid material was characterized ( Figure 5 ). Comparison of nHAP, Ag3PO4 and nHAP-Ag 3 PO 4 The infrared spectrum shows that the wave number is 674.99-688.49cm- 1 The absorption peak is generated by CH bending vibration; wave number 912.20-1091.55cm- 1 and 1880.60cm- 1 The absorption peaks on the left and right correspond to the stretching and bending vibrations of O=PO and POP; wave number 1496.54-1646.97cm -1 The absorption peak is generated by the asymmetric stretching vibration of C=O; 3137.43-3405.79cm -1 The absorption peak is caused by the stretching vibration of OH. 3 PO 4 Simultaneously with nHAP and Ag 3 PO 4 The infrared absorption peaks are basically consistent, which indicates that Ag + With PO 4 3- Ag generated by the reaction 3 PO 4 Successfully loaded on the surface of nHAP.
[0097] Comparison with Ag 3 PO 4 、nHAP、nHAP-Ag 3 PO 4 UV-Vis diffuse reflectance spectrum ( Figure 6 ) Display: Ag 3 PO 4 Strong absorption occurs in the range of 300-550nm, nHAP has lower absorbance in the range of 300-600nm, and nHAP-Ag 3 PO 4 Strong absorption appears at 378-600nm. This is probably due to the presence of Ag on the surface of nHAP. 3 PO 4 This led to a change in the spectrum. In particular, compared with nHAP, a new absorption peak at 475nm appeared in the nHAP-Ag3PO4 spectrum, which is consistent with the Ag 3 PO 4The characteristic absorption peak of Ag 3 PO 4 Successfully loaded onto the nHAP surface.
[0098] The synthesized nHAP-Ag 3 PO 4 Thermogravimetric analysis of the hybrid material was performed to investigate the effect of ambient temperature on its stability. Figure 7 ) It can be seen that when the temperature reaches 40℃, nHAP-Ag 3 PO 4 The weight loss rate was 4.62% at 40-160℃, and the weight loss rate reached a peak at 115.17℃, which may be due to the evaporation of water in the sample. The weight loss was 11.36% at 160-500℃, and the weight loss rate reached a peak at 213.17℃, 263.5℃ and 413℃, which may be due to the decomposition of organic matter in the sample nHAP or Ag. When the temperature exceeded 500℃, nHAP-Ag 3 PO 4 The thermal decomposition rate gradually decreases to no loss. At 40-800℃, nHAP-Ag 3 PO 4 The weight loss of the composite material was about 16.18%, which indicated that nHAP-Ag 3 PO 4 The thermal stability is relatively high.
[0099] MB, MO, RhB and TC were used as simulated pollutants to investigate the 3 PO 4 Photocatalytic activity. Figure 8 middle, Figure 8 a is the MB concentration (C / C 0 ) with different irradiation time. After 20 minutes of visible light irradiation, Ag 3 PO 4 The photocatalytic degradation efficiency of MB is about 99.82%; the photocatalytic degradation efficiency of nHAP for MB is only 13.54%; and the photocatalytic degradation efficiency of nHAP-Ag is only 13.54%. 3 PO 4 The degradation efficiency of the hybrid material was 97.81%, which was 84.27% higher than that of nHAP. 3 PO 4 The photocatalytic degradation effect of the hybrid material on MB is significantly better than that of nHAP, which indicates that nHAP-Ag 3 PO 4 It is an efficient photocatalyst for MB degradation. Figure 8 b is the MO concentration (C / C 0) with different irradiation time. After 20 minutes of visible light irradiation, Ag 3 PO 4 The photocatalytic degradation efficiency of MO is about 96.69%; the photocatalytic degradation efficiency of MO by nHAP is only 11.42%; and the photocatalytic degradation efficiency of MO by nHAP-Ag is about 96.69%. 3 PO 4 The degradation efficiency of the hybrid material was 94.49%, which was 83.07% higher than that of nHAP. 3 PO 4 The photocatalytic degradation effect of the hybrid material on MB is significantly better than that of nHAP, which indicates that nHAP-Ag 3 PO 4 It is a highly efficient photocatalyst for the degradation of MO. Figure 8 c is the RhB concentration (C / C 0 ) with different irradiation time. After 20 minutes of visible light irradiation, Ag 3 PO 4 The photocatalytic degradation efficiency of RhB was about 97.34%, while the photocatalytic degradation efficiency of nHAP for MB was only 8.57%. 3 PO 4 The degradation efficiency of the hybrid material was 96.51%, which was 87.94% higher than that of nHAP. 3 PO 4 The photocatalytic degradation effect of the hybrid material on RhB is significantly better than that of nHAP, which indicates that nHAP-Ag 3 PO 4 It is an efficient photocatalyst for the degradation of RhB. Figure 8 d is the curve of TC concentration (C / C0) changing with different irradiation time. After 20 minutes of visible light irradiation, Ag 3 PO 4 The photocatalytic degradation efficiency of TC is about 91.26%; the photocatalytic degradation efficiency of TC by nHAP is only 7.14%; and the photocatalytic degradation efficiency of nHAP-Ag is only 7.14%. 3 PO 4 The degradation efficiency of the hybrid material was 94.68%, which was 87.54% higher than that of nHAP. 3 PO 4 The photocatalytic degradation effect of the hybrid material on MB is significantly better than that of nHAP, which indicates that nHAP-Ag 3 PO 4 It is an efficient photocatalyst for TC degradation. 3 PO 4The separation of electrons and holes occurs on the surface of the hybrid material. Electrons are reducing and can reduce oxygen to superoxide radicals, while holes are oxidizing and can oxidize water to hydroxyl radicals. Holes, superoxide radicals, and hydroxyl radicals can all oxidize organic matter in the water, thereby degrading the dyes in the water. Fig. 9 It can be seen that after three cycles, the efficiency of photocatalyst in degrading dyes decreased by only about 8.21%, and the efficiency of degrading TC decreased by only 9.36%, and the degradation efficiency was still above 83%, which shows that nHAP-Ag 3 PO 4 The hybrid material has relatively high photochemical stability.
[0100] We selected Pb(II) as the target pollutant to explore the prepared nHAP-Ag 3 PO 4 The adsorption capacity of hybrid materials for heavy metals. Fig.10 Shown: nHAP and nHAP-Ag 3 PO 4 The hybrid materials have a certain adsorption capacity for Pb(II). Under the same dosage and conditions, the adsorption capacity of the two materials for Pb(II) increased significantly before 50 minutes. After 50 minutes, the adsorption capacity of nHAP for Pb(II) decreased significantly, and basically stopped reaching saturation at 90 minutes, with a maximum adsorption capacity of about 60 mg / g. 3 PO 4 After 50 minutes, the adsorption capacity of Pb(II) was still strong, and it did not stop until 100 minutes. The maximum adsorption capacity was 180 mg / g, which was three times that of pure HAP. 3 PO 4 The results of Pb(II) adsorption indicated that it is a promising heavy metal adsorbent.
[0101] The agar diffusion method was used to detect nHAP-Ag using Vibrio harveyi, a common pathogenic bacteria in aquatic products. 3 PO 4 The antibacterial effect of hybrid materials. Fig.11 As shown, nHAP-Ag 3 PO 4 The hybrid material can effectively inhibit the growth of aquatic pathogens and produce a significant inhibition zone on the pathogens; while hydroxyapatite has no inhibitory effect on the pathogens, indicating that it is not hydroxyapatite but the silver phosphate in it that has the inhibitory effect. Finally, the two-fold dilution method was used to determine the nHAP-Ag 3 PO 4 The minimum inhibitory concentration (MIC) of the hybrid material was 5 mg / mL, and the minimum bactericidal concentration (MBC) was 10 mg / mL.
[0102] All of the above indicate that this new material has excellent ability to photocatalytically degrade organic matter, adsorb heavy metal pollutants, and kill harmful bacteria in water bodies.
[0103] Although the present invention has been described in detail above by general description and specific embodiments, it is obvious to those skilled in the art that some modifications or improvements can be made to the present invention. Therefore, these modifications or improvements made without departing from the spirit of the present invention all belong to the scope of protection claimed by the present invention.
Claims
1. A method for preparing a hydroxyapatite-loaded silver phosphate hybrid material, characterized in that: The preparation method comprises the following steps: (1) Thaw salmon bones and mince into minced fish; (2) further processing the minced fish in step (1) by a colloid mill and a tissue homogenizer to obtain a protein homogenate; (3) titrating the protein homogenate in step (2) with HCl solution, and centrifuging to retain the precipitate; (4) mixing the precipitate in step (3) with deionized water in a volume ratio of 1:1, boiling at 100° C. for 2 h, drying in a 50° C. oven for 48 h, and then calcining in a muffle furnace at 700° C. for 4 h to obtain hydroxyapatite powder; (5) grinding the hydroxyapatite powder in step (4) at a material-liquid ratio of 1:20 with 5 mm grinding balls in a ball mill at 600 r / min for 10 h, and then grinding again at the same speed for 10 h with 0.5 mm grinding balls to obtain nano-hydroxyapatite material; the material-liquid ratio of 1:20 means that hydroxyapatite powder: deionized water = 1 g: 20 mL; (6) preparing 50 mM silver nitrate solution; (7) 10 mL of the silver nitrate solution in step (6) was mixed with 85 mg of the hydroxyapatite in step (5), reacted at room temperature in the dark for 6 h, centrifuged at 11000 r / min for 20 min, the supernatant was discarded, washed with deionized water three times, and dried in an oven at 50° C. for 48 h to obtain a nano-hydroxyapatite-loaded silver phosphate hybrid material.
2. The preparation method according to claim 1, characterized in that: The treatment method in step (2) is to add 50 mL of deionized water per 1 g of fish paste and treat it with a tissue homogenizer for 10 minutes.
3. The preparation method according to claim 1, characterized in that: Step (3) titrate to a pH value of 2.0-5.
0.
4. The preparation method according to claim 1, characterized in that: The pH value is 2.
0.
5. The preparation method according to claim 1, characterized in that: After titration with HCl solution in step (3), place in a 4°C refrigerator for 15 min, take out and centrifuge at 11000 r / min for 20 min, then discard the supernatant and keep the precipitate.
6. The preparation method according to claim 1, characterized in that: The particle size of the hydroxyapatite-loaded silver phosphate hybrid material is 100 nm.
7. The preparation method according to claim 1, characterized in that: The room temperature in step (7) is 20-25°C.
8. The hydroxyapatite-loaded silver phosphate hybrid material prepared according to the preparation method according to any one of claims 1 to 7.
9. Use of the hydroxyapatite-loaded silver phosphate hybrid material according to claim 8 in photocatalytic degradation of organic matter, adsorption of heavy metal pollutants, and killing of harmful bacteria in water bodies.
Citation Information
Patent Citations
Nano-Ag3PO4 / hydroxyapatite photocatalyst, and preparation method and application thereof
CN110152695A
Development of characterization and synthesis of natural fish bone activated carbon and hydroxyapatite through heat treatment
WO2016080825A1