Preparation method of melamine modified acrylic resin hard carbon material

Through the chemical bonding of melamine and acrylic resin and high-temperature carbonization treatment, melamine-modified acrylic resin hard carbon material with a porous structure is solved, and the problems of low first-term efficiency and poor circulation performance of phenolic resin hard carbon material are improved, and the sodium ion battery is improved. Capacity and cycling performance.

CN118978142AActive Publication Date: 2024-11-19SHENZHEN QINGYAN HAOLONG NEW ENERGY TECH CO LTD

Patent Information

Application Number
CN202411041586.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-19
Estimated Expiration
2044-07-31

AI Technical Summary

Technical Problem

The existing phenolic resin hard carbon as the negative electrode material of sodium ion battery has problems such as low first-term efficiency and poor circulation performance. The preparation process is complex and toxic, affecting the environment and human health.

Method used

Melamine is used to react chemically with acrylic resin with carboxyl functional groups to form a three-dimensional network structure, and melamine-modified acrylic resin hard carbon material with a sponge-like porous structure is generated by hydrothermal and high-temperature carbonization treatment.

Benefits of technology

It improves the structural stability and conductivity of the material, reduces pores and defects, increases the number of closed pores, improves the capacity and circulation performance of sodium ion batteries, and improves the chemical stability of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118978142A_ABST
    Figure CN118978142A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a melamine modified acrylic resin hard carbon material, chemical bond synthesis reaction is carried out by utilizing-NH2 of melamine and-COOH of acrylic resin, and amido bonds are generated by dehydration condensation to connect the melamine and the acrylic resin into a three-dimensional network structure, and the preparation method specifically comprises the following steps: step 1, element doping; 2, low-temperature curing; 3, high-temperature carbonization is carried out, and the loose porous spongy melamine modified acrylic resin hard carbon material can be obtained. The preparation method comprises the following steps: taking acrylic resin with carboxyl functional groups as a hard carbon precursor material, performing chemical bond synthesis reaction by utilizing-NH2 of melamine and-COOH of the acrylic resin, performing dehydration condensation to generate amido bonds, and connecting the amido bonds into a three-dimensional network structure; spongy amorphous carbon is generated through hydrothermal treatment, generation of pores and defects is reduced through low-temperature curing, and the first effect is greatly improved; the pores are changed from large pores to small pores through high-temperature carbonization, the number of closed pores is increased, the platform capacity of the sodium-ion battery is improved, and the cycle performance is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of negative electrode materials for sodium ion batteries, and in particular to a method for preparing a melamine-modified acrylic resin hard carbon material. Background Art

[0002] Most of the resin precursors of the hard carbon materials for the negative electrode of sodium-ion batteries are based on phenolic resins, but the preparation process of phenolic resins is too complicated. Formaldehyde and benzene need to be mixed in a certain proportion, and acid / alkaline solutions need to be added as catalysts. The polycondensation time needs to be strictly controlled. Secondly, formaldehyde monomer is toxic, and special attention should be paid to safety during the production and preparation process. Formaldehyde has a certain degree of harm to production workers and the environment. Finally, the resin will inevitably volatilize free phenol and free aldehyde gases during transportation in high temperature weather.

[0003] As the main negative electrode material of sodium-ion batteries, phenolic resin hard carbon has the basic problems of low initial efficiency and poor cycle performance. The main reason is that hard carbon has a short-range ordered and long-range disordered internal structure, which makes the potential barrier of sodium ions embedded large, the ion migration impedance large, and the thermodynamic performance unstable. In addition, the electronic state around the carbon atoms in hard carbon itself is not conducive to the embedding of sodium ions, which leads to its poor kinetic performance.

[0004] Acrylic resin is a type of thermoplastic resin made by polymerizing acrylic acid, methacrylic acid and its derivatives (esters, nitriles, amides), which can be repeatedly softened by heat and solidified by cooling. It is generally a linear polymer compound, which can be a homopolymer or a copolymer. It has excellent physical and mechanical properties, weather resistance, chemical resistance, water resistance, and high gloss and color retention. By modifying acrylic resin with melamine, part of the area in the cross-linked resin-based hard carbon material is graphitized, which increases the number of closed pores and improves the capacity of the cross-linked resin-based hard carbon material. Summary of the invention

[0005] The purpose of the present invention is to provide a method for preparing a melamine-modified acrylic resin hard carbon material, so as to solve the problems of low initial efficiency and poor cycle performance of the existing phenolic resin hard carbon as the main negative electrode material of sodium ion batteries.

[0006] To achieve the above object, the present invention provides the following technical solution: a method for preparing a melamine-modified acrylic resin hard carbon material, using -NH2 of melamine and -COOH of acrylic resin to carry out a chemical bond synthesis reaction, dehydration condensation to generate amide bonds to connect them into a three-dimensional network structure, specifically comprising the following steps:

[0007] Step 1, element doping: dissolving melamine in a mixed solution of ethanol and deionized water, then adding acrylic resin, stirring evenly and transferring to a hydrothermal reaction to form a sponge-like melamine-modified resin precursor;

[0008] Step 2, low temperature curing: placing the sponge-like melamine-modified resin precursor in a muffle furnace for heating to obtain a completely cured melamine-modified resin precursor;

[0009] Step 3, high temperature carbonization: The fully cured melamine modified resin precursor obtained in step 2 is subjected to two-stage heat treatment in a nitrogen atmosphere, the first stage is maintained at a constant temperature of 500°C for 10 hours, and the second stage is maintained at a constant temperature of 1400°C for 2 hours. After the second stage of heat treatment, a loose porous sponge-like melamine modified acrylic resin hard carbon material can be obtained.

[0010] Wherein, in step 1, the volume ratio of ethanol to deionized water in the mixed solution is 1:1-5.

[0011] Wherein, in step 1, the mass ratio of melamine to acrylic resin is 1:1-10.

[0012] Wherein, in step 1, the temperature of the hydrothermal reaction is 100-150° C., and the time is 1-10 h.

[0013] Wherein, in step 2, the specific conditions for heating in the muffle furnace are: a heating rate of 0.1-8°C / min, and a constant temperature of 100-300°C for 1-5h.

[0014] The protective gas introduced during the heating process is one or more of nitrogen, argon and helium, and the flow rate thereof is 4-400 mL / min.

[0015] Wherein, the ventilation flow rate of nitrogen in the high-temperature carbonization is 6-350 mL / min.

[0016] Wherein, the heating rate during the two-stage heat treatment process can be 0.5-10°C / min.

[0017] Compared with the prior art, the present invention has the following beneficial effects:

[0018] The present invention uses acrylic resin with carboxyl functional groups as a hard carbon precursor material, utilizes -NH2 of melamine and -COOH of acrylic resin to carry out chemical bond synthesis reaction, and dehydrates and condenses to generate amide bonds to connect them into a three-dimensional network structure; wherein melamine is both a cross-linking agent of acrylic resin and a dopant of N element, and the N element is added while improving the structural stability, thereby improving the conductivity of the overall material and the active sites for sodium storage; hydrothermal treatment generates sponge-like amorphous carbon, and low-temperature curing reduces the generation of pores and defects, thereby greatly improving the first efficiency; high-temperature carbonization converts the pores from large pores to small pores, thereby increasing the number of closed pores, improving the platform capacity of the sodium ion battery, and improving the cycle performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 This is a SEM image of the melamine-modified acrylic resin hard carbon material of the present invention. DETAILED DESCRIPTION

[0020] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0021] Example 1

[0022] A method for preparing a melamine-modified acrylic resin hard carbon material, which can be used as a negative electrode material for a sodium ion battery, uses -NH2 of melamine and -COOH of acrylic resin to carry out a chemical bond synthesis reaction, dehydration condensation generates amide bonds to connect them into a three-dimensional network structure, and specifically comprises the following steps:

[0023] Step 1, element doping: 4g of melamine was dissolved in a mixed solution of 100ml of ethanol and 200ml of deionized water, and then 20g of acrylic resin was added and stirred evenly, and then transferred to a hydrothermal reactor and kept at a constant temperature of 120°C for 5h to form a sponge-like melamine-modified resin precursor;

[0024] Step 2, low temperature curing: placing the sponge-like melamine-modified resin precursor in a muffle furnace in a nitrogen atmosphere and heating it, raising the temperature to 150° C. at 1° C. / min and maintaining it for 2 hours to obtain a fully cured melamine-modified resin precursor;

[0025] Step 3, high temperature carbonization: Grind the fully cured melamine-modified resin precursor obtained in step 2 into powder and perform two-stage heat treatment in a nitrogen atmosphere. The first stage is to heat up to 500°C at 2°C / min for low-temperature pre-carbonization heat treatment for 10 hours; the second stage is to heat up to 1400°C for high-temperature heat treatment for 3 hours. After the second stage of heat treatment, a loose porous sponge-like melamine-modified acrylic resin hard carbon material can be obtained.

[0026] Example 2

[0027] A method for preparing a melamine-modified acrylic resin hard carbon material, which can be used as a negative electrode material for a sodium ion battery, uses -NH2 of melamine and -COOH of acrylic resin to carry out a chemical bond synthesis reaction, dehydration condensation generates amide bonds to connect them into a three-dimensional network structure, and specifically comprises the following steps:

[0028] Step 1, element doping: 4g of melamine was dissolved in a mixed solution of 50ml of ethanol and 250ml of deionized water, and then 20g of acrylic resin was added and stirred evenly, and then transferred to a hydrothermal reactor and kept at a constant temperature of 120°C for 5h to form a sponge-like melamine-modified resin precursor;

[0029] Step 2, low temperature curing: placing the sponge-like melamine-modified resin precursor in a muffle furnace in a nitrogen atmosphere and heating it, raising the temperature to 150° C. at 1° C. / min and maintaining it for 2 hours to obtain a fully cured melamine-modified resin precursor;

[0030] Step 3, high temperature carbonization: Grind the fully cured melamine-modified resin precursor obtained in step 2 into powder and perform two-stage heat treatment in a nitrogen atmosphere. The first stage is to heat up to 500°C at 2°C / min for low-temperature pre-carbonization heat treatment for 10 hours; the second stage is to heat up to 1400°C for high-temperature heat treatment for 3 hours. After the second stage of heat treatment, a loose porous sponge-like melamine-modified acrylic resin hard carbon material can be obtained.

[0031] Example 3

[0032] A method for preparing a melamine-modified acrylic resin hard carbon material, which can be used as a negative electrode material for a sodium ion battery, uses -NH2 of melamine and -COOH of acrylic resin to carry out a chemical bond synthesis reaction, dehydration condensation generates amide bonds to connect them into a three-dimensional network structure, and specifically comprises the following steps:

[0033] Step 1, element doping: 2g of melamine was dissolved in a mixed solution of 100ml of ethanol and 200ml of deionized water, and then 20g of acrylic resin was added and stirred evenly, and then transferred to a hydrothermal reactor and kept at a constant temperature of 120°C for 5h to form a sponge-like melamine-modified resin precursor;

[0034] Step 2, low temperature curing: placing the sponge-like melamine-modified resin precursor in a muffle furnace in a nitrogen atmosphere and heating it, raising the temperature to 150° C. at 1° C. / min and maintaining it for 2 hours to obtain a fully cured melamine-modified resin precursor;

[0035] Step 3, high temperature carbonization: Grind the fully cured melamine-modified resin precursor obtained in step 2 into powder and perform two-stage heat treatment in a nitrogen atmosphere. The first stage is to heat up to 500°C at 2°C / min for low-temperature pre-carbonization heat treatment for 10 hours; the second stage is to heat up to 1400°C for high-temperature heat treatment for 3 hours. After the second stage of heat treatment, a loose porous sponge-like melamine-modified acrylic resin hard carbon material can be obtained.

[0036] Example 4

[0037] A method for preparing a melamine-modified acrylic resin hard carbon material, which can be used as a negative electrode material for a sodium ion battery, uses -NH2 of melamine and -COOH of acrylic resin to carry out a chemical bond synthesis reaction, dehydration condensation generates amide bonds to connect them into a three-dimensional network structure, and specifically comprises the following steps:

[0038] Step 1, element doping: 4g of melamine was dissolved in a mixed solution of 100ml of ethanol and 200ml of deionized water, and then 20g of acrylic resin was added and stirred evenly, and then transferred to a hydrothermal reactor and kept at a constant temperature of 120°C for 5h to form a sponge-like melamine-modified resin precursor;

[0039] Step 2, low temperature curing: placing the sponge-like melamine-modified resin precursor in a muffle furnace in a nitrogen atmosphere and heating it, raising the temperature to 300° C. at 1° C. / min and maintaining it for 2 hours to obtain a fully cured melamine-modified resin precursor;

[0040] Step 3, high temperature carbonization: Grind the fully cured melamine-modified resin precursor obtained in step 2 into powder and perform two-stage heat treatment in a nitrogen atmosphere. The first stage is to heat up to 500°C at 2°C / min for low-temperature pre-carbonization heat treatment for 10 hours; the second stage is to heat up to 1400°C for high-temperature heat treatment for 3 hours. After the second stage of heat treatment, a loose porous sponge-like melamine-modified acrylic resin hard carbon material can be obtained.

[0041] Example 5

[0042] A method for preparing a melamine-modified acrylic resin hard carbon material, which can be used as a negative electrode material for a sodium ion battery, uses -NH2 of melamine and -COOH of acrylic resin to carry out a chemical bond synthesis reaction, dehydration condensation generates amide bonds to connect them into a three-dimensional network structure, and specifically comprises the following steps:

[0043] Step 1, element doping: 4g of melamine was dissolved in a mixed solution of 100ml of ethanol and 200ml of deionized water, and then 20g of acrylic resin was added and stirred evenly, and then transferred to a hydrothermal reactor and kept at a constant temperature of 120°C for 5h to form a sponge-like melamine-modified resin precursor;

[0044] Step 2, low temperature curing: placing the sponge-like melamine-modified resin precursor in a muffle furnace in a nitrogen atmosphere and heating it, raising the temperature to 150° C. at 2° C. / min and maintaining it for 2 h to obtain a fully cured melamine-modified resin precursor;

[0045] Step 3, high temperature carbonization: Grind the fully cured melamine-modified resin precursor obtained in step 2 into powder and perform two-stage heat treatment in a nitrogen atmosphere. The first stage is to heat up to 500°C at 2°C / min for low-temperature pre-carbonization heat treatment for 10 hours; the second stage is to heat up to 1400°C for high-temperature heat treatment for 3 hours. After the second stage of heat treatment, a loose porous sponge-like melamine-modified acrylic resin hard carbon material can be obtained.

[0046] Comparative Example 1

[0047] A method for preparing an N-doped acrylic resin hard carbon material, the resin hard carbon material can be used as a negative electrode material for a sodium ion battery, and the specific preparation method is as follows:

[0048] Step 1: Evenly mix 4 g of melamine and 20 g of acrylic resin to obtain a mixed resin precursor;

[0049] Step 2: Place the mixed resin precursor obtained above in a muffle furnace with an argon atmosphere, heat it to 500°C at 2°C / min and keep it for 10 hours; then heat it to 1400°C at the same heating rate and perform high-temperature heat treatment for 3 hours to obtain a melamine mixed acrylic resin hard carbon material.

[0050] Comparative Example 2

[0051] A method for preparing an acrylic resin hard carbon material, the resin hard carbon material can be used as a negative electrode material for a sodium ion battery, and the specific preparation method is as follows:

[0052] Step 1: Disperse 4 g of aqueous ammonia in a mixed solution of 100 ml of ethanol and 200 ml of deionized water, then add 20 g of acrylic resin and mix evenly, then transfer to a hydrothermal reactor and keep the temperature at 120° C. for 5 hours to obtain a sponge-like melamine-modified resin precursor;

[0053] Step 2: placing the melamine-modified resin precursor obtained above in a muffle furnace in a nitrogen atmosphere, heating it to 150° C. at 1° C. / min and maintaining it for 2 h to obtain a fully cured N-doped resin precursor;

[0054] Step 3: Grind the fully cured resin into powder, heat it to 500°C at 2°C / min in an argon atmosphere, and perform low-temperature pre-carbonization heat treatment for 10 hours; then heat it to 1400°C and perform high-temperature heat treatment for 3 hours to obtain melamine-modified acrylic resin hard carbon material.

[0055] Experimental Example 1

[0056] SEM test: The loose porous sponge-like melamine-modified acrylic resin hard carbon material prepared in Example 1 was subjected to SEM test. The results are as follows: Figure 1 As shown. Figure 1 It can be seen that the loose porous sponge-like melamine-modified acrylic resin hard carbon material presents a porous sponge-like structure with a large number of pore structures on the surface, and the particle size is between 20-30 μm.

[0057] Example 2

[0058] The method for testing the gram capacity and cycle number of the negative electrode material of the sodium ion battery is as follows: the hard carbon material in Examples 1-5 and Comparative Examples 1-2 is used as the negative electrode, the metal sodium sheet is used as the positive electrode, and 1.0 mol / L LiPF6 / EC (ethylene carbonate) + DMC (dimethyl carbonate) + FEC (fluoroethylene carbonate) (EC, DMC and FEC volume ratio 4.5:4.5:1) is used as the electrolyte, and CR2032 button batteries are assembled in an argon glove box. The constant current charge and discharge are tested in the 0-2V voltage window using the LAND battery test system. The test conditions and results are shown in Table 1 below:

[0059] Table 1

[0060]

[0061] As can be seen from Table 1, the button battery was subjected to constant current charge and discharge test at a current density of 500mA / g, a voltage range of 0-2V, and 100 cycles. The button half-cells of melamine-modified resin hard carbon materials prepared in Examples 1-5 all had good cycle retention rates (greater than 90%), showing excellent cycle stability. However, the capacity retention rates of Comparative Examples 1 and 2 were only about 60%. Specific values ​​are shown in Table 2 (Capacity retention rates of button half-cells of electrode materials prepared in Examples 1-5 and Comparative Examples 1-2 after 100 cycles.)

[0062] Table 2

[0063] Current density 500mA / g 100 cycles capacity retention rate (%) Example 1 99.7 Example 2 98.7 Example 3 92.3 Example 4 94.2 Example 5 97.6 Comparative Example 1 62.7 Comparative Example 2 50.4

[0064] In summary, the present invention uses acrylic resin with carboxyl functional groups as a hard carbon precursor material, utilizes -NH2 of melamine and -COOH of acrylic resin to carry out chemical bond synthesis reaction, and dehydration condensation generates amide bonds to connect them into a three-dimensional network structure; wherein melamine is both a cross-linking agent of acrylic resin and a dopant of N element, and the N element is incorporated while improving the structural stability, thereby improving the conductivity of the overall material and the active sites for sodium storage; hydrothermal treatment generates sponge-like amorphous carbon, and low-temperature curing reduces the formation of pores and defects, greatly improving the first effect; high-temperature carbonization converts the pores from large pores to small pores, increases the number of closed pores, improves the platform capacity of the sodium ion battery, and improves the cycle performance.

[0065] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A method for preparing a melamine-modified acrylic resin hard carbon material, characterized in that: The -NH2 of melamine and the -COOH of acrylic resin are used for chemical bond synthesis reaction, and dehydration condensation generates amide bonds to connect them into a three-dimensional network structure, which specifically includes the following steps: Step 1, element doping: dissolving melamine in a mixed solution of ethanol and deionized water, then adding acrylic resin, stirring evenly and transferring to a hydrothermal reaction to form a sponge-like melamine-modified resin precursor; Step 2, low temperature curing: placing the sponge-like melamine-modified resin precursor in a muffle furnace for heating to obtain a completely cured melamine-modified resin precursor; Step 3, high temperature carbonization: The fully cured melamine modified resin precursor obtained in step 2 is subjected to two-stage heat treatment in a nitrogen atmosphere, the first stage is maintained at a constant temperature of 500°C for 10 hours, and the second stage is maintained at a constant temperature of 1400°C for 2 hours. After the second stage of heat treatment, a loose porous sponge-like melamine modified acrylic resin hard carbon material can be obtained.

2. The method for preparing a melamine-modified acrylic resin hard carbon material according to claim 1, characterized in that: In step 1, the volume ratio of ethanol to deionized water in the mixed solution is 1:1-5.

3. The method for preparing a melamine-modified acrylic resin hard carbon material according to claim 1, characterized in that: In step 1, the mass ratio of melamine to acrylic resin is 1:1-10.

4. The method for preparing a melamine-modified acrylic resin hard carbon material according to claim 1, characterized in that: In step 1, the temperature of the hydrothermal reaction is 100-150° C., and the time is 1-10 h.

5. The method for preparing a melamine-modified acrylic resin hard carbon material according to claim 1, characterized in that: In step 2, the specific conditions for heating in the muffle furnace are: a heating rate of 0.1-8°C / min, and a constant temperature of 100-300°C for 1-5h.

6. The method for preparing a melamine-modified acrylic resin hard carbon material according to claim 5, characterized in that: The protective gas introduced during the heating process is one or more of nitrogen, argon and helium, and the flow rate is 4-400 mL / min.

7. The method for preparing a melamine-modified acrylic resin hard carbon material according to claim 1, characterized in that: The nitrogen ventilation flow rate during the high temperature carbonization is 6-350 mL / min.

8. The method for preparing a melamine-modified acrylic resin hard carbon material according to claim 7, characterized in that: The heating rate during the two-stage heat treatment process can be 0.5-10°C / min.

Citation Information

Patent Citations

  • Hard carbon cathode material for lithium ion power and energy storage battery and preparation method of hard carbon cathode material

    CN103094528A

  • Defect-rich sodium ion battery negative electrode material and preparation method and application thereof

    CN110809558A

  • Pre-sodium hard carbon negative electrode material and preparation method and application thereof

    CN116598488A

  • Composite negative electrode material, negative electrode plate and sodium ion battery

    CN117691074A

  • Biomass derived porous carbon materials, composites and methods of production

    US20220352501A1

Cited By

  • Preparation method of hard carbon doped with pre-oxidized heavy organic matter in situ

    CN119430148A