Preparation method and application of coal gangue-phosphate tailing-based quaternary hydrotalcite

By extracting calcium, magnesium, aluminum and iron elements from coal gangue and phosphorus tailings, a high value-added quaternary hydrotalcite composite was prepared, which solved the problem of low resource utilization and achieved the reduction of coal gangue and phosphorus tailings. Chemical treatment and environmental protection.

CN118978185APending Publication Date: 2024-11-19WUHAN INST OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410908768.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-08
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

The resource utilization rate of coal gangue and phosphorus tailings is low, and the added value of products is low, resulting in land waste and environmental pollution.

Method used

The intercalation co-assembly method is used to extract calcium, magnesium, aluminum and iron elements from coal gangue and phosphorus tailings, and a high value-added gangue-phosphorus tailings-based quaternary hydrotalcite composite material is prepared through hydrothermal reaction.

Benefits of technology

The reduction and high value-added utilization of coal gangue and phosphorus tailings have been achieved, providing a resource-based treatment method for clean production, and reducing the risks of land occupation and environmental pollution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118978185A_ABST
    Figure CN118978185A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of solid waste resource utilization, and discloses a preparation method and application of coal gangue-phosphate tailing based quaternary hydrotalcite, and the preparation method comprises the following steps: step 1, calcining coal gangue and phosphate tailing samples in a muffle furnace to 300-800 DEG C for later use, extracting elements in the coal gangue and phosphate tailing acidolysis liquid through water bath stirring and heating by adopting an acid adding extraction method, centrifuging and filtering to obtain the coal gangue and phosphate tailing acidolysis liquid; and 2, mixing the two acidolysis solutions, and adding a NaOH solution to adjust the pH value of the system to 10-12. According to the invention, solid waste coal gangue and phosphate tailings are taken as main raw materials, valuable elements calcium, magnesium, aluminum and iron in the coal gangue and the phosphate tailings are fully utilized, the coal gangue-phosphate tailings based quaternary hydrotalcite with high added value is prepared, and reduction, high-added-value utilization and clean production of the solid waste coal gangue and phosphate tailings are realized; and a new thought is explored for reduction and recycling of the coal gangue and the phosphate tailings.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of solid waste resource utilization, and in particular to a preparation method and application of a gangue-phosphate tailings-based quaternary hydrotalcite. Background Art

[0002] With the rapid development of science and technology, the energy demand of various countries is rising. Coal plays an important role in global energy consumption. Coal gangue is the main solid waste generated in the process of coal mining and processing, usually accounting for 15-20% of the total raw coal output, mainly composed of carbonaceous shale, mudstone, sandstone and coal. Phosphate ore is a general term for rocks with high phosphate mineral content, while phosphate tailings are solid wastes generated after the flotation of phosphate ore to extract concentrates. Its output accounts for 20-30% of the original ore, and its main components are fluoroapatite, dolomite, aluminosilicate, etc. Due to the huge amount of coal gangue and phosphate tailings, they are usually stored in exposed piles and discarded on the surface near the mine, with extremely low utilization efficiency. In the process of large-scale accumulation, it is inevitable to occupy a large amount of land and farmland resources including cultivated land, and it also consumes huge amounts of yard construction and maintenance costs. This not only causes a serious waste of land resources, but also makes it easy for natural disasters to occur, accelerates the weathering process and dissolution of soluble components, enters the surrounding ecological environment for the migration and transformation of harmful substances, and poses a threat to human health and animal safety. Therefore, it is urgent to achieve the reduction and resource utilization of coal gangue and phosphate tailings. Exploring new ways to treat and dispose of coal gangue and phosphate tailings is of great significance to protecting the ecological environment.

[0003] Layered double hydroxides (LDHs), also known as hydrotalcites, are bimetallic or polymetallic clay minerals with a layered structure. Due to their special layered structure, high anion exchange capacity, large surface area and rich pore structure, they have excellent ion exchange and adsorption properties. LDHs have a unique isomorphous substitution mechanism, and their selectivity and mineralization capacity for different heavy metal ions can be adjusted through a variety of strategies. In recent years, due to the low cost, certain flame retardant function and high removal efficiency of LDHs, they have been widely used in a large number of studies. For example, Deng et al. used Mg / Al-LDH to intercalate phosphorus and nitrogen flame retardants to prepare flame-retardant plywood, and Hudcova et al. reported that MgFe-LDH and mixed oxides showed excellent adsorption efficiency for As(V), Pb(II) and Zn(II).

[0004] At present, Fu et al. prepared light glass ceramics with high added value using coal gangue and phosphate tailings as raw materials, Wang et al. prepared FeO / C / CG and Fe / C / CG composite materials as microwave absorbers using coal gangue, and Yu et al. recovered phosphorus from phosphate tailings by leaching-precipitation process, while the method of using coal gangue and phosphate tailings to prepare calcium-magnesium-aluminum-iron-based quaternary hydrotalcite composite functional materials is rare. At the same time, there is no report on the research of recovering elements such as Ca, Mg, Fe, and Al from coal gangue and phosphate tailings to prepare in-situ passivation materials. Therefore, it is of great significance to recycle Ca, Mg, Al, and Fe in coal gangue and phosphate tailings to prepare hydrotalcite-based composite materials with high added value. Summary of the invention

[0005] The present invention aims to provide a preparation method and application of a gangue-phosphate tailings-based quaternary hydrotalcite. The present invention takes gangue and phosphate tailings as raw materials, makes full use of calcium, magnesium, aluminum and iron elements in the gangue and phosphate tailings, and adopts an intercalation co-assembly method to prepare a gangue-phosphate tailings-based quaternary hydrotalcite composite material with high added value, thus opening up a new way for the comprehensive utilization of gangue and phosphate tailings, achieving the purpose of turning waste into treasure, and effectively solving the problems of low resource utilization rate of existing gangue and phosphate tailings and low product added value.

[0006] To achieve the above object, the present invention provides the following technical solution: a method for preparing a gangue-phosphate tailings-based quaternary hydrotalcite, the preparation method comprising the following steps:

[0007] Step 1: calcining the gangue and phosphate tailings samples in a muffle furnace to 300-800° C. for standby use, extracting the elements therein by stirring and heating in a water bath using an acid extraction method, and centrifuging and filtering to obtain the gangue and phosphate tailings acid hydrolyzate;

[0008] Step 2: Mix the above two acid hydrolyzates, then add NaOH solution to adjust the pH value of the system to 10-12, and then transfer to a reactor for hydrothermal reaction. After the reaction is completed, the reaction solution is cooled to room temperature and then washed and centrifuged. The product is then dried overnight and ground to obtain coal gangue-phosphate tailings-based quaternary hydrotalcite powder.

[0009] Preferably, the coal gangue and phosphate tailings samples in step 1 are placed in a muffle furnace and calcined to 300-800° C. for 2-4 hours.

[0010] Preferably, the water bath stirring in step 1 is heated at 60-80° C. for 0.5-2 h.

[0011] Preferably, the element Mg in step 1 is 2+ and Ca 2+ With Al 3+ and Fe 3+The molar ratio is 2 to 4:1.

[0012] Preferably, the concentration of the NaOH solution is 4-10 mol / L.

[0013] Preferably, the hydrothermal reaction temperature in step 2 is 100-120° C., and the hydrothermal reaction time is 24-48 h.

[0014] Compared with the prior art, the present invention has the following beneficial effects:

[0015] 1. The present invention uses solid waste coal gangue and phosphate tailings as main raw materials, makes full use of the valuable elements calcium, magnesium, aluminum and iron in the coal gangue and phosphate tailings, and adopts a hydrothermal co-precipitation method to synthesize a Ca-Mg-Al-Fe quaternary hydrotalcite with high added value, thereby achieving the reduction, high added value utilization and clean production of coal gangue and phosphate tailings solid waste, and exploring a new idea for the reduction and resource utilization of coal gangue and phosphate tailings.

[0016] 2. The present invention uses solid waste coal gangue and phosphate tailings as raw materials, which are easy to obtain, have simple preparation steps, are low in cost, and have broad application prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 is the XRD pattern of coal gangue-phosphate tailings based quaternary hydrotalcite;

[0018] Figure 2 This is the SEM image of coal gangue-phosphate tailings based quaternary hydrotalcite. DETAILED DESCRIPTION

[0019] The technical scheme in the embodiment of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiment of the present invention. Obviously, the described embodiment is only a part of the embodiment of the present invention, not all of the embodiments. Based on the embodiment of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0020] Example 1

[0021] The preparation method of coal gangue-phosphate tailings-based quaternary hydrotalcite comprises the following steps:

[0022] 1) The gangue and phosphate tailings samples were placed in a muffle furnace and calcined at 300°C for 2h, and the elements therein were extracted by acid extraction method by stirring in a water bath at 60°C for 0.5h, and the acid hydrolyzed solution of the gangue and phosphate tailings was obtained by centrifugation and filtration;

[0023] 2) Pipette a certain amount of coal gangue and phosphate tailings acid solution into a beaker so that the Mg content of the mixed solution is 2+ and Ca 2+ With Al3+ and Fe 3+ The molar ratio of 2:1 was 2:1. Under continuous magnetic stirring, 4 mol / L NaOH solution was slowly added dropwise to adjust the pH value of the system and stabilize it at 10±0.02. The obtained mixed solution was transferred to a polytetrafluoroethylene reactor liner, sealed with a metal shell and placed in a 100°C oven for hydrothermal reaction for 24 hours.

[0024] 3) After the reaction is completed, the reactor is taken out and opened after cooling to room temperature. The slurry therein is centrifuged at 5000 rpm for 3 min using a high-speed centrifuge to remove the supernatant to obtain the precipitate therein;

[0025] 4) Repeatedly washing with ultrapure water and centrifuging for 3 times, then washing with ethanol and centrifuging once, to wash away the free cations attached to the surface of the precipitate in the solution after the reaction, reduce the interference of impurity cations on the reaction and prevent the introduction of other ions into the environment during the reaction, and then dry the product in an oven at 50° C. overnight, take it out and grind it to obtain hydrotalcite powder.

[0026] Example 2

[0027] The preparation method of coal gangue-phosphate tailings-based quaternary hydrotalcite comprises the following steps:

[0028] 1) The gangue and phosphate tailings samples were placed in a muffle furnace and calcined at 500°C for 3 h, and the elements therein were extracted by acid extraction method by stirring in a water bath at 70°C for 1 h, and the acid hydrolyzed solution of the gangue and phosphate tailings was obtained by centrifugation and filtration;

[0029] 2) Pipette a certain amount of coal gangue and phosphate tailings acid solution into a beaker so that the Mg content of the mixed solution is 2+ and Ca 2+ With Al 3+ and Fe 3+ The molar ratio of 3:1 was 3:1. Under continuous magnetic stirring, 8 mol / L NaOH solution was slowly added dropwise to adjust the pH value of the system and stabilize it at 11±0.02. The obtained mixed solution was transferred to a polytetrafluoroethylene reactor liner, sealed with a metal shell and placed in a 110°C oven for hydrothermal reaction for 36 hours.

[0030] 3) After the reaction is completed, the reactor is taken out and opened after cooling to room temperature. The slurry therein is centrifuged at 5000 rpm for 3 min using a high-speed centrifuge to remove the supernatant to obtain the precipitate therein;

[0031] 4) Repeatedly washing with ultrapure water and centrifuging for 3 times, then washing with ethanol and centrifuging once, to wash away the free cations attached to the surface of the precipitate in the solution after the reaction, reduce the interference of impurity cations on the reaction and prevent the introduction of other ions into the environment during the reaction, and then dry the product in an oven at 50° C. overnight, take it out and grind it to obtain hydrotalcite powder.

[0032] Example 3

[0033] The preparation method of coal gangue-phosphate tailings-based quaternary hydrotalcite comprises the following steps:

[0034] 1) The gangue and phosphate tailings samples were placed in a muffle furnace and calcined at 700°C for 4 hours, and the elements therein were extracted by acid extraction method by stirring in a water bath at 80°C for 2 hours, and the coal gangue and phosphate tailings acid solution was obtained by centrifugation and filtration;

[0035] 2) Pipette a certain amount of coal gangue and phosphate tailings acid solution into a beaker so that the Mg content of the mixed solution is 2+ and Ca 2+ With Al 3+ and Fe 3+ The molar ratio of 4:1 was 4:1. Under continuous magnetic stirring, 10 mol / L NaOH solution was slowly added dropwise to adjust the pH value of the system and stabilize it at 12±0.02. The obtained mixed solution was transferred to a polytetrafluoroethylene reactor liner, sealed with a metal shell and placed in a 120°C oven for hydrothermal reaction for 48 hours.

[0036] 3) After the reaction is completed, the reactor is taken out and opened after cooling to room temperature. The slurry therein is centrifuged at 5000 rpm for 3 min using a high-speed centrifuge to remove the supernatant to obtain the precipitate therein;

[0037] 4) Repeatedly washing with ultrapure water and centrifuging for 3 times, then washing with ethanol and centrifuging once, to wash away the free cations attached to the surface of the precipitate in the solution after the reaction, reduce the interference of impurity cations on the reaction and prevent the introduction of other ions into the environment during the reaction, and then dry the product in an oven at 50° C. overnight, take it out and grind it to obtain hydrotalcite powder.

[0038] For matters not mentioned above, the prior art applies.

[0039] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.

[0040] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A method for preparing a gangue-phosphate tailings-based quaternary hydrotalcite, characterized in that: The preparation method comprises the following steps: Step 1: calcining the gangue and phosphate tailings samples in a muffle furnace to 300-800° C. for standby use, extracting the elements therein by stirring and heating in a water bath using an acid extraction method, and centrifuging and filtering to obtain the gangue and phosphate tailings acid hydrolyzate; Step 2: Mix the above two acid hydrolyzates, add NaOH solution to adjust the pH value of the system to 10-12, and then transfer to a reactor for hydrothermal reaction. After the reaction is completed, the reaction solution is cooled to room temperature, washed and centrifuged, and the product is dried overnight and ground to obtain coal gangue-phosphate tailings-based quaternary hydrotalcite powder.

2. The method for preparing the gangue-phosphate tailings-based quaternary hydrotalcite according to claim 1, characterized in that: The coal gangue and phosphate tailings samples in step 1 are placed in a muffle furnace and calcined to 300-800° C. for 2-4 hours.

3. The method for preparing the gangue-phosphate tailings-based quaternary hydrotalcite according to claim 1, characterized in that: The water bath stirring in step 1 is heated at 60-80° C. for 0.5-2 h.

4. The method for preparing the gangue-phosphate tailings-based quaternary hydrotalcite according to claim 1, characterized in that: The element Mg in step 1 2+ and Ca 2+ With Al 3+ and Fe 3+ The molar ratio is 2 to 4:

1.

5. The method for preparing the gangue-phosphate tailings-based quaternary hydrotalcite according to claim 1, characterized in that: The concentration of the NaOH solution is 4-10 mol / L.

6. The method for preparing the gangue-phosphate tailings-based quaternary hydrotalcite according to claim 1, characterized in that: The hydrothermal reaction temperature in step 2 is 100-120° C., and the hydrothermal reaction time is 24-48 hours.