Method for preparing sulphoaluminate cement from sintering process red mud and secondary aluminum ash
Through the coordinated use of red mud and secondary aluminum ash by sintering, combined with kaolin and desulfurization gypsum, the process flow is simplified, and the problems of high production cost and complex process of sulfur aluminate cement are solved, thus achieving low-cost and efficient preparation of sulfur aluminate acid Salt cement, excellent product performance and suitable for batch processing.
Patent Information
- Application Number
- CN202410916440.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-09
- Publication Date
- 2024-11-19
AI Technical Summary
In the prior art, sulfur aluminate cement has high production costs and complex processes, and it is difficult to effectively utilize sintering red mud and secondary aluminum ash, which has the problem of high-temperature pretreatment with high energy consumption and toxic substance residues.
The sintering method is used to jointly prepare sulfa aluminate cement and secondary aluminum ash. The secondary aluminum ash is treated by rapid slurry and desalting at low temperature, combined with kaolin and desulfurization gypsum, and the sulfa aluminate cement is prepared in low-cost and efficient manner, and the process flow is simplified. , improve solid waste mix and product performance.
It realizes low-cost and efficient preparation of sulfur aluminate cement, has short settling time, high compressive and flexural strength, is suitable for batch processing, and promotes industrial solid waste resource utilization.
Smart Images

Figure CN118978349A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of special cements, and in particular relates to a method for preparing sulphoaluminate cement by utilizing sintering red mud and secondary aluminium ash. Background Art
[0002] The statements in this section are merely intended to provide background information related to the technical solution of the present application to aid understanding, and they do not necessarily constitute prior art for the technical solution of the present application.
[0003] The main raw materials of sulphoaluminate cement are limestone, bauxite and gypsum. Cement products are prepared through a series of steps including raw material selection, batching, crushing, grinding, calcination and clinker grinding. Its main mineral phases are calcium sulphoaluminate, dicalcium silicate and iron phase. CaO accounts for 36-43%wt in clinker, Al 2 O 3 It accounts for 25-35%wt in clinker, and usually requires the use of large amounts of limestone and high-grade bauxite as raw materials.
[0004] With the rapid development of China's aluminum production industry, the demand for raw material bauxite is increasing, and the price of bauxite is also increasing. The high price of bauxite raw materials increases the production cost of sulphoaluminate cement, while the large-scale use of limestone not only increases the production cost, but also produces a large amount of carbon dioxide during the clinker calcination process.
[0005] Sintered red mud is the alkaline residue after the sintering process to extract alumina from bauxite. Compared with Bayer red mud, the content of CaO and SiO in sintered red mud is 2 and Al 2 O 3 The content is above 60% and the sintering red mud is calcined at high temperature, silicon, aluminum and calcium ions are easily dissolved to form CaO-Al 2 O 3 -SiO 2 The ternary system has high activity and is capable of replacing limestone and bauxite to prepare sulphoaluminate cement.
[0006] Secondary aluminum ash is the most important solid waste in the process of electrolytic aluminum and aluminum processing and smelting. The aluminum content can reach 30-55%wt. Its main components are alumina, aluminum nitride, metallic aluminum, salts and other components. After low-temperature washing, the salts can be removed to become high-aluminum material. The alumina and aluminum nitride in the high-aluminum material can be effectively utilized and converted into sulphoaluminate minerals.
[0007] Sintered red mud and secondary aluminum ash can replace limestone and bauxite in the production of sulphoaluminate cement, which can not only greatly reduce the cost of raw materials but also realize the resource utilization of industrial solid waste.
[0008] Chinese patent CN202010161255.1 discloses a method and system for preparing sulphoaluminate cement from all solid wastes pretreated with aluminum ash, wherein the aluminum ash is heated to not less than 900°C for heat treatment, the heat-treated aluminum ash is homogenized and mixed with red mud, desulfurized gypsum, and carbide slag, the mixed material is dried using hot gas generated by the heat treatment, the dried material is ground with raw powder, and the material ground with raw powder is calcined to obtain sulphoaluminate cement clinker. Although the present invention achieves the complete replacement of bauxite with aluminum ash, it requires high-temperature pretreatment of the aluminum ash, the treatment process consumes a lot of energy, and the Bayer process red mud has a high alkali content, and direct use without dealkalization will reduce the quality of sulphoaluminate cement.
[0009] Chinese patent CN201710159979.0 discloses a system and method for preparing sulphoaluminate cement by using organic wastewater in combination with industrial solid waste. After the de-alkali red mud, carbide slag, aluminum ash, desulfurized gypsum and a portion of organic wastewater are mixed and wet-ground, the mixture is put into a rotary kiln for high-temperature calcination to obtain sulphoaluminate clinker. During the high-temperature calcination, coal powder is sprayed into the rotary kiln to burn the organic waste in the coal powder, slurry and concentrated wastewater. This technical solution requires de-alkali pretreatment of red mud, and the calcination of the organic wastewater concentrate with the raw meal will leave some toxic substances in the cement clinker, which will cause harm to the human body and the environment during the use of cement. Summary of the invention
[0010] In order to overcome the problems of high cost, complex process and low direct use dosage of the existing technology, the present invention provides a method for preparing sulphoaluminate cement by using sintered red mud and secondary aluminum ash, wherein the sintered red mud provides calcium source and silicon source, the secondary aluminum ash after low-temperature rapid slurrying and desalination provides aluminum source, and kaolin and desulfurized gypsum are used to prepare sulphoaluminate special cement. The method has not only simple process, low cost and high solid waste dosage, but also short setting time of the finished product, high compressive and flexural strength, and is suitable for batch processing.
[0011] The technical solution adopted by the present invention to solve the technical problem is: a method for preparing sulphoaluminate cement by synergistically using sintering red mud and secondary aluminum ash, comprising the following steps:
[0012] 1) Pretreatment of secondary aluminum ash slurry desalination: prepare slurry with secondary aluminum ash and water in proportion, stir and desalt under low temperature conditions, filter, and dry to obtain high-aluminum material. Specifically, the liquid-solid ratio of secondary aluminum ash to water can be selected as 1:2-1:4, and the mixed slurry is kept at a temperature less than 20°C for slurrying, the stirring speed is 100-300 rpm, the reaction time is 5-30min, and then filtered, and rinsed with cold water 1-3 times the mass of the secondary aluminum ash to obtain brine and filter residue, and then the filter residue is dried at a temperature of 100-120°C to obtain high-aluminum material. The brine after washing and filtering the secondary aluminum ash is defluorinated by lime and then filtered to obtain filtrate and filter cake. The filtrate is evaporated and crystallized to obtain a composite salt, the main components of which are sodium chloride and potassium chloride. After a brief blending, it can be used to prepare an aluminum refining agent. The main component of the filter cake is CaF 2 , used as a mineralizer in clinker sintering.
[0013] 2) Raw material pretreatment: crush and grind limestone, kaolin, sintered red mud, desulfurized gypsum and high-alumina material in a crusher and a ball mill respectively; the raw materials can be dried in a drying oven at 110-120°C for about 24 hours, and then crushed and ground to less than 0.08mm, with a sieve residue of less than 8%.
[0014] 3) Mixing and tableting: The raw materials obtained in step 2) are mixed according to the following formula: CaO accounts for 45-60%wt, Al 2 O 3 15~35%wt, SiO 2 10~25%wt, Fe 2 O 3 Accounting for 5~10%wt, SO 3 The raw materials accounting for 3-10%wt are mixed and mixed to be uniform, and dry pressed to obtain raw materials. Among them, the specific proportion of cement raw materials can be: sintered red mud accounts for 25-60%wt, high alumina accounts for 10-35%wt, limestone accounts for 10-40%wt, kaolin accounts for 15-45%wt, and desulfurized gypsum accounts for 5-15%wt.
[0015] 4) Clinker calcination: The raw material obtained in step 3) and the filter cake obtained in step 1) are calcined and quenched together to obtain sulphoaluminate cement clinker. Specifically, the raw material is calcined in a muffle furnace at 1200-1300° C. for 0.5-2 hours, then taken out and quenched to obtain sulphoaluminate cement clinker.
[0016] 5) Cement preparation: The cement clinker obtained in step 4) is crushed with a crusher, added with desulfurized gypsum, and the two are mixed and ground in a vibration mill to a specific surface area of 400±10m 2 / kg of sulphoaluminate cement. The mass of the added desulfurized gypsum is 1-15% of the mass of the cement clinker.
[0017] A method for preparing sulphoaluminate cement by using sintering red mud and secondary aluminum ash. It can be seen from the ingredients that the effective raw materials of sulphoaluminate cement are calcium oxide, aluminum oxide, silicon oxide and iron oxide from most to least. The calcium oxide content of sintering red mud is greater than 30%, the aluminum oxide content is greater than 10%, and it contains 10-20% of active silicon oxide and a certain amount of active iron oxide; the secondary aluminum ash is desalted to obtain high-aluminum material, the main components of which are aluminum oxide and aluminum nitride, and then combined with limestone to supplement calcium and kaolin to supplement silicon, it can not only prepare and generate high-quality sulphoaluminate cement at a low cost, but also promote the resource utilization of industrial solid waste.
[0018] The sulphoaluminate cement clinker is composed of dicalcium silicate (2CaO·SiO 2 ), calcium sulphoaluminate (3CaO·3Al 2 O 3 ·CaSO 4 ) and aluminoferrite (4CaO·3Al 2 O 3 ·Fe 2 O 3 ) are the main mineral phases, accounting for 45-55%wt, 25-35%wt and 5-20%wt respectively.
[0019] Compared with the prior art, the beneficial technical effects of the present invention are:
[0020] (1) Sintering red mud is used as the main raw material, which not only contains a large amount of calcium oxide, aluminum oxide, silicon oxide and iron oxide, but also after high-temperature calcination, silicon, aluminum and calcium ions are easily dissolved to form CaO-Al 2 O 3 -SiO 2 The ternary system has high activity and not only provides good conditions for the formation of calcium sulfoaluminate and dicalcium silicate phases, but also fully utilizes the effective components of sintered red mud. The blending amount of red mud can reach 30-60%.
[0021] (2) Aluminum ash contains a certain amount of soluble salts such as NaCl, KCl, NaF, KF (Cl content 1-15%, Na content 2-10%, F content 3%-25%), among which Na and K are strong electropositive elements, which will reduce the liquid phase appearance temperature and increase the liquid phase viscosity during clinker sintering, which will not only affect the formation, structure and performance of clinker minerals, but also cause clinker sticking to the kiln, ringing and other phenomena, increase the difficulty of sintering, and reduce production efficiency. Free Cl and F have small ions and high activity. During the clinker sintering process, they will replace sulfur to form chloroaluminate / fluoroaluminate compounds, reduce the content of sulfoaluminate in the clinker, and affect the performance of the clinker. The secondary aluminum ash is slurried and eluted at low temperature quickly, which can not only remove the soluble salts that are unfavorable to the sintering of clinker, but also the rapid and low-temperature washing environment will not cause the hydrolysis of aluminum nitride, avoiding the large-scale production of ammonia and ensuring production safety. Finally, a high-aluminum material with an aluminum oxide and aluminum nitride content greater than 80% is obtained, which replaces bauxite to provide an aluminum source for the calcination of sulphoaluminate cement clinker.
[0022] (3) The secondary aluminum ash contains a small amount of CaF 2 The washed and filtered brine is defluorinated by lime to produce CaF 2 Its fluorine-containing insoluble matter can also react with calcium oxide to generate CaF at high temperature. 2 It can be used as a mineralizer in the calcination process to reduce the calcination temperature of clinker, assist in the formation of calcium silicate and calcium sulfoaluminate minerals, reduce the free calcium oxide content in the clinker, reduce the initial and final setting time of cement, and improve its compressive and flexural strength. The brine after washing and filtering the secondary aluminum ash is filtered after lime defluorination to obtain the filtrate, and the filtrate is evaporated and crystallized to obtain a composite salt, which is mainly composed of sodium chloride and potassium chloride. After a brief blending, it can be used to prepare aluminum refining agents, so that the secondary aluminum ash can also be fully utilized. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 Process flow chart for preparing sulphoaluminate cement from sintering red mud and secondary aluminum ash;
[0024] Figure 2 X-ray diffraction pattern of the fired cement clinker of Example 3. DETAILED DESCRIPTION
[0025] In order to make the purpose, technical scheme and advantages of the present invention more clear, the method and process for preparing sulphoaluminate cement by using sintering red mud and secondary aluminum ash of the present application are described in detail below in combination with embodiments, comparative examples and experimental data. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0026] A method for preparing sulphoaluminate cement by utilizing sintered red mud and secondary aluminum ash is a technology for complementary utilization and synergistic resource utilization of solid wastes such as sintered red mud and secondary aluminum ash. Calcium oxide, silicon oxide, aluminum oxide and iron oxide in sintered red mud and aluminum oxide and aluminum nitride in secondary aluminum ash high-aluminum material are calcined to generate sulphoaluminate main phases of dicalcium silicate, calcium sulphoaluminate and calcium aluminoferrate. Calcium fluoride in secondary aluminum ash can also play the role of mineralizer, reduce the calcination temperature of cement clinker, assist in the formation of calcium silicate and calcium sulphoaluminate minerals, reduce the free calcium oxide content in the clinker, reduce the initial and final setting time of cement, and improve its compressive and flexural strengths.
[0027] The method for preparing sulphoaluminate cement by using sintering red mud and secondary aluminum ash uses sintering red mud and secondary aluminum ash as main raw materials and cooperates with solid wastes such as desulfurized gypsum to prepare sulphoaluminate cement. The whole process includes:
[0028] 1: Pretreatment of secondary aluminum ash slurry desalination: prepare slurry with secondary aluminum ash and water in proportion, stir and desalt, filter, and dry to obtain high-aluminum material. In one embodiment, secondary aluminum ash and water can be mixed at a solid-liquid ratio of 1:2-1:4, and the mixed slurry is kept at a temperature less than 20°C, with a stirring speed of 100-300r / min, and filtered after reaction for 5-30min. After rinsing with cold water 1-3 times the mass of the secondary aluminum ash, brine and filter residue are obtained. The filter residue is dried at 100-120°C to obtain high-aluminum material. The brine is defluorinated by lime and filtered to obtain filtrate and filter cake. The filtrate is evaporated and crystallized to obtain composite salt, the main components of which are sodium chloride and potassium chloride. After brief preparation, it can be used to prepare aluminum refining agent. The main component of the filter cake is CaF 2 , can be used as a mineralizer in clinker sintering;
[0029] Second: drying limestone, kaolin, sintered red mud, and desulfurized gypsum, and crushing and grinding them with high-aluminum materials to obtain raw materials. In one embodiment, the limestone, kaolin, sintered red mud, desulfurized gypsum, and high-aluminum materials can be dried, ground, sieved, crushed, and ground to 0.08 mm, with a sieve residue of less than 8%;
[0030] 3. Mixing and tableting: Mix the raw materials obtained in step 2 according to the following formula: CaO accounts for 45-60%wt, Al 2 O 3 15~35%wt, SiO 2 10~25%wt, Fe 2 O 3 Accounting for 5~10%wt, SO 3The raw materials accounting for 3-10%wt are mixed and mixed until uniform, and then dry pressed to obtain raw materials. The proportion of each raw material is calculated according to the mineral composition of cement clinker. According to the requirements of sulphoaluminate cement, the mineral composition of cement clinker is designed as follows: dicalcium silicate accounts for 40-60%wt, calcium sulphoaluminate accounts for 25-40%wt, and calcium aluminoferrite accounts for 10-30%wt; the raw material weight ratio requirements are calculated as follows: CaO accounts for 45-60%wt, Al 2 O 3 15~35%wt, SiO 2 10~25%wt, Fe 2 O 3 Accounting for 5~10%wt, SO 3 In one embodiment, the specific proportion of ingredients is: sintering red mud accounts for 25-60% wt, high aluminum material accounts for 10-35% wt, limestone accounts for 10-40% wt, kaolin accounts for 15-45% wt, and desulfurized gypsum accounts for 5-15% wt. The raw materials are mixed in proportion and then dry-pressed into a shape;
[0031] 4. Clinker calcination: calcine the raw material obtained in step 3 and the filter cake obtained in step 1 together and quench to obtain sulphoaluminate cement clinker. In one embodiment, the raw material test block is placed in a muffle furnace, calcined at 1200-1300°C for 0.5-2 hours, and then taken out and quenched to obtain sulphoaluminate cement clinker;
[0032] 5. Crush the cement clinker obtained in step 4, add desulfurized gypsum, mix the two and grind them to obtain sulphoaluminate cement. In one embodiment, after the clinker is crushed, 1-15% of the desulfurized gypsum by weight of the clinker is added in proportion, and the specific surface area of the sulphoaluminate cement product is controlled to be 400±10m 2 / kg.
[0033] Further examples of the present application are provided below.
[0034] Example 1
[0035] The secondary aluminum ash and water were mixed in a mass ratio of 1:2 to prepare a slurry, maintained at 5°C, stirred at 100r / min for 5min, filtered, rinsed with cold water 1 times the mass of the aluminum ash to obtain brine and filter residue, the brine was defluorinated and filtered to obtain a filter cake, the filter residue was dried at 100°C to obtain a high-aluminum material, and crushed and ground with dried limestone, kaolin, sintered red mud, and desulfurized gypsum respectively in a mass ratio of 10%, 25%, 15%, 45%, and 5%, respectively, and then added with the defluorinated filter cake to press into shape, calcined at 1200°C in a muffle furnace for 30min, and rapidly cooled after discharge to obtain clinker, which was mixed with 5% desulfurized gypsum by mass to obtain sulphoaluminate cement, and the specific surface area of the product was 400±10m 2 / kg. The 1d, 3d and 28d compressive strengths were measured according to GB / T 17671-1999 “Test method for strength of cement mortar”.
[0036] Example 2
[0037] The secondary aluminum ash and water were mixed in a mass ratio of 1:3 to prepare a slurry, maintained at 10°C, stirred at 200r / min for 10min, filtered, rinsed with cold water twice the mass of the aluminum ash to obtain brine and filter residue, the brine was defluorinated and filtered to obtain a filter cake, the filter residue was dried at 120°C to obtain a high-aluminum material, and crushed and ground with dried limestone, kaolin, sintered red mud, and desulfurized gypsum respectively in a mass ratio of 25%, 10%, 15%, 40%, and 10%, respectively, and then added with the defluorinated filter cake to press into shape, calcined in a muffle furnace at 1250°C for 60min, and rapidly cooled after discharge to obtain clinker, which was mixed with 8% desulfurized gypsum by mass to obtain sulphoaluminate cement. The specific surface area of the product was 400±10m 2 / kg. The 1d, 3d and 28d compressive strengths were measured according to GB / T 17671-1999 “Test method for strength of cement mortar”.
[0038] Example 3
[0039] The secondary aluminum ash and water were mixed in a mass ratio of 1:4 to prepare a slurry, maintained at 10°C, stirred at 300r / min for 15min, filtered, rinsed with cold water 3 times the mass of the aluminum ash to obtain brine and filter residue, the brine was defluorinated and filtered to obtain a filter cake, the filter residue was dried at 100°C to obtain a high-aluminum material, and crushed and ground with dried limestone, kaolin, sintered red mud, and desulfurized gypsum respectively in a mass ratio of 20%, 15%, 15%, 40%, and 10%, respectively, and then added with the defluorinated filter cake to press into shape, calcined at 1300°C in a muffle furnace for 120min, and rapidly cooled after discharge to obtain clinker, which was mixed with 10% desulfurized gypsum by mass to obtain sulphoaluminate cement. The specific surface area of the product was 400±10m 2 / kg. The 1d, 3d and 28d compressive strengths were measured according to GB / T 17671-1999 “Test method for strength of cement mortar”.
[0040] Depend on Figure 2 It can be seen that the main phase of the cement clinker fired in Example 3 is 2CaO·SiO 2 、3CaO·3Al 2 O 3 ·CaSO 4 and 4CaO·3Al 2 O 3 ·Fe 2 O 3 , which meets the composition requirements of sulphoaluminate cement and contains CaO·TiO 2(Perovskite) component can not only promote the hydration reaction of cement to form more hydration products such as calcium silicate, hydrated calcium silicate and hydrated calcium aluminate, thereby improving its compressive strength, but also form a conductive channel to improve the cement's anti-cracking performance.
[0041] Example 4
[0042] The secondary aluminum ash and water were mixed in a mass ratio of 1:4 to prepare a slurry, maintained at 20°C, stirred at 200r / min for 20min, filtered, rinsed with cold water 3 times the mass of the aluminum ash to obtain brine and filter residue, the brine was defluorinated and filtered to obtain a filter cake, the filter residue was dried at 100°C to obtain a high-aluminum material, and crushed and ground with dried limestone, kaolin, sintered red mud, and desulfurized gypsum respectively in a mass ratio of 10%, 10%, 15%, 60%, and 5%, respectively, and then added with the defluorinated filter cake to press into shape, calcined in a muffle furnace at 1250°C for 120min, and rapidly cooled after discharge to obtain clinker, which was mixed with 12% desulfurized gypsum by mass to obtain sulphoaluminate cement. The specific surface area of the product was 400±10m 2 / kg. The 1d, 3d and 28d compressive strengths were measured according to GB / T 17671-1999 “Test method for strength of cement mortar”.
[0043] Example 5
[0044] The secondary aluminum ash and water were mixed in a mass ratio of 1:4 to prepare a slurry, maintained at 20°C, stirred at 300r / min for 30min, filtered, rinsed with cold water twice the mass of the aluminum ash to obtain brine and filter residue, the brine was defluorinated and filtered to obtain a filter cake, the filter residue was dried at 100°C to obtain a high-aluminum material, and crushed and ground with dried limestone, kaolin, sintered red mud, and desulfurized gypsum respectively in a mass ratio of 35%, 20%, 15%, 25%, and 5%, respectively, and then added with the defluorinated filter cake to press into shape, calcined in a muffle furnace at 1250°C for 60min, and rapidly cooled after discharge to obtain clinker, which was mixed with 15% desulfurized gypsum by mass to obtain sulphoaluminate cement. The specific surface area of the product was 400±10m 2 / kg. The 1d, 3d and 28d compressive strengths were measured according to GB / T 17671-1999 “Test method for strength of cement mortar”.
[0045] Example 6
[0046] The secondary aluminum ash and water were mixed in a mass ratio of 1:4 to prepare a slurry, maintained at 20°C, stirred at 300r / min for 30min, filtered, rinsed with cold water twice the mass of the aluminum ash to obtain brine and filter residue, the brine was defluorinated and filtered to obtain a filter cake, the filter residue was dried at 100°C to obtain a high-aluminum material, and the dried limestone, kaolin, sintered red mud, and desulfurized gypsum were crushed and ground respectively, and mixed in a mass ratio of 35%, 10%, 15%, 25%, and 15% respectively, and then the defluorinated filter cake was added to press into shape, calcined at 1250°C in a muffle furnace for 60min, and rapidly cooled after discharge to obtain clinker, which was mixed with 15% desulfurized gypsum by mass to obtain sulphoaluminate cement. The specific surface area of the product was 400±10m 2 / kg. The 1d, 3d and 28d compressive strengths were measured according to GB / T 17671-1999 “Test method for strength of cement mortar”.
[0047] Example 7
[0048] The secondary aluminum ash and water were mixed in a mass ratio of 1:3 to prepare a slurry, maintained at 10°C, stirred at 200r / min for 10min, filtered, rinsed with cold water twice the mass of the aluminum ash to obtain brine and filter residue, the brine was defluorinated and filtered to obtain a filter cake, the filter residue was dried at 120°C to obtain a high-aluminum material, and crushed and ground with dried limestone, kaolin, sintered red mud, and desulfurized gypsum respectively in a mass ratio of 10%, 40%, 15%, 25%, and 10%, respectively, and then added with the defluorinated filter cake to press into shape, calcined in a muffle furnace at 1250°C for 60min, and rapidly cooled after discharge to obtain clinker, which was mixed with 8% desulfurized gypsum by mass to obtain sulphoaluminate cement. The specific surface area of the product was 400±10m 2 / kg. The 1d, 3d and 28d compressive strengths were measured according to GB / T 17671-1999 “Test method for strength of cement mortar”.
[0049] Example 8
[0050] The secondary aluminum ash and water were mixed in a mass ratio of 1:2 to prepare a slurry, maintained at 5°C, stirred at 100r / min for 5min, filtered, rinsed with cold water 1 times the mass of the aluminum ash to obtain brine and filter residue, the brine was defluorinated and filtered to obtain a filter cake, the filter residue was dried at 100°C to obtain a high-aluminum material, and crushed and ground with dried limestone, kaolin, sintered red mud, and desulfurized gypsum respectively in a mass ratio of 10%, 10%, 45%, 30%, and 5%, respectively, and then added with the defluorinated filter cake to press into shape, calcined at 1200°C in a muffle furnace for 30min, and rapidly cooled after discharge to obtain clinker, which was mixed with 5% desulfurized gypsum by mass to obtain sulphoaluminate cement. The specific surface area of the product was 400±10m 2 / kg. The 1d, 3d and 28d compressive strengths were measured according to GB / T 17671-1999 “Test method for strength of cement mortar”.
[0051] Comparative Example 1
[0052] The secondary aluminum ash is dried, crushed and ground with limestone, kaolin, sintered red mud and desulfurized gypsum, respectively, and then mixed with the mixture in the mass ratio of 20%, 15%, 15%, 40% and 10%, respectively, and then dry-pressed into a mold. The mixture is calcined at 1300°C for 120min in a muffle furnace, and then rapidly cooled to obtain clinker. 10% of the mass of desulfurized gypsum is added into the mixture and ground to obtain sulphoaluminate cement. The 1d, 3d and 28d compressive strengths thereof are measured according to GB / T 17671-1999 "Test method for strength of cement mortar".
[0053] Comparative Example 2
[0054] The secondary aluminum ash and water are mixed in a mass ratio of 1:4 to prepare a slurry, maintained at 10°C, stirred at 300r / min for 15min, filtered, rinsed with cold water 3 times the mass of the aluminum ash to obtain brine and filter residue, the brine is defluorinated and filtered to obtain a filter cake, the filter residue is dried at 100°C to obtain a high-aluminum material, and the material is crushed and ground with dried limestone, kaolin, Bayer red mud, and desulfurized gypsum respectively in a mass ratio of 20%, 15%, 15%, 40%, and 10%, respectively, and then the defluorinated filter cake is added to press into shape, calcined at 1300°C for 120min in a muffle furnace, and rapidly cooled after discharging to obtain clinker, which is mixed with 10% desulfurized gypsum by mass of the clinker to obtain sulphoaluminate cement, and its 1d, 3d, and 28d compressive strengths are measured according to GB / T17671-1999 "Test Method for Strength of Cement Mortar".
[0055] Comparative Example 3
[0056] The secondary aluminum ash and water are mixed in a mass ratio of 1:4 to prepare a slurry, maintained at 10°C, stirred at 300r / min for 15min, filtered, rinsed with cold water 3 times the mass of the aluminum ash to obtain brine and filter residue, the brine is defluorinated and filtered to obtain a filter cake, the filter residue is dried at 100°C to obtain a high-aluminum material, and the material is crushed and ground with dried limestone, kaolin, sintered red mud, and desulfurized gypsum respectively in a mass ratio of 5%, 40%, 20%, 20%, and 15%, respectively, and then the defluorinated filter cake is added to press into shape, calcined at 1300°C for 120min in a muffle furnace, and rapidly cooled after discharging to obtain clinker, which is mixed with 10% desulfurized gypsum by mass of the clinker to obtain sulphoaluminate cement, and its 1d, 3d, and 28d compressive strengths are measured according to GB / T17671-1999 "Test Method for Strength of Cement Mortar".
[0057] The products treated by Examples 1-8 and Comparative Examples 1-3 were tested for compressive strength and flexural strength, and the test results are shown in the following table:
[0058]
[0059] It can be seen from the above table that the sulphoaluminate cement prepared by the process provided by the present application has a 1d compressive strength greater than 40MPa and a flexural strength greater than 10MPa; a 3d compressive strength greater than 53MPa and a flexural strength greater than 12MPa; a 28d compressive strength greater than 57MPa and a flexural strength greater than 13MPa, all of which meet the strength requirements of the fast-hardening sulphoaluminate 425 grade. By comparing the comparative examples with the embodiments, it can be seen that when the raw materials lack processing steps, the parameters do not meet the requirements, or a certain parameter in the processing process is not within the scope of the present application, the quality of the cement clinker will be low, and the compressive strength and flexural strength of the prepared cement mortar test block will be low, or even not meet the standard requirements.
[0060] The aluminum ash in Comparative Example 1 has not been desalted, and the sodium, potassium and chloride ions contained therein will affect the production of sulfoaluminate compounds during the clinker sintering process, resulting in insufficient compressive and flexural strength of the cement product; Comparative Example 2 uses Bayer process red mud instead of sintering process red mud. Since the alkali content in the Bayer process red mud is too high, the calcium oxide content is low, and the silicon and aluminum activity therein are insufficient, the sintered product cannot meet the requirements of sulfoaluminate cement; the proportion of limestone in Comparative Example 3 is not within the scope of the patent, resulting in insufficient calcium content in the product, resulting in insufficient content of calcium sulfoaluminate and dicalcium silicate in the clinker, thereby affecting the product properties.
[0061] Having thus described several aspects of at least one embodiment of the present invention, it will be appreciated that various changes, modifications and improvements will readily occur to those skilled in the art. Such changes, modifications and improvements are intended to be within the spirit and scope of the present invention. Although the present invention has been described by way of some embodiments, the present invention is not limited to the embodiments described herein, and also includes various changes and variations made without departing from the scope of the present invention.
Claims
1. A method for preparing sulphoaluminate cement using sintering red mud and secondary aluminum ash, characterized in that The following steps are involved: 1) Pretreatment of secondary aluminum ash slurry desalination: secondary aluminum ash and water are mixed in a solid-liquid ratio of 1:2-1:4 to prepare slurry, the slurry temperature is less than or equal to 20°C, the stirring speed is 100-300 rpm, and the mixture is stirred for 5-30 minutes before filtering and rinsed with cold water to obtain brine and filter residue, and the filter residue is dried at a temperature of 100-120°C to obtain high-aluminum material; the brine is defluorinated by lime and then filtered to obtain a filtrate and a filter cake, and the filtrate is evaporated and crystallized to obtain a composite salt; 2) Raw material pretreatment: limestone, kaolin, sintered red mud, and desulfurized gypsum are dried and crushed and ground with high-aluminum materials to obtain raw materials; 3) Mixing and tableting: the raw materials obtained in step 2) are mixed according to the raw material proportion of 45-60%wt of CaO, 15-35%wt of Al2O3, 10-25%wt of SiO2, 5-10%wt of Fe2O3, and 3-10%wt of SO3, mixed until uniform, and dry pressed to obtain raw material; 4) Clinker calcination: calcining the raw material obtained in step 3) and the filter cake obtained in step 1) together and then rapidly cooling to obtain sulphoaluminate cement clinker; 5) Cement preparation: The cement clinker obtained in step 4) is crushed, added with desulfurized gypsum, and the two are mixed and ground to obtain sulphoaluminate cement.
2. The method for preparing sulphoaluminate cement according to claim 1, wherein: In step 2), the raw materials are dried, crushed and ground to less than 0.08 mm, and the residue on sieve is less than 8%.
3. The method for preparing sulphoaluminate cement according to claim 1, wherein: The specific proportions of raw materials in step 3) are: sintered red mud accounts for 25-60% wt, high alumina accounts for 10-35% wt, limestone accounts for 10-40% wt, kaolin accounts for 15-45% wt, and desulfurized gypsum accounts for 5-15% wt.
4. The method for preparing sulphoaluminate cement according to claim 1, wherein: In step 4), the raw material is calcined in a muffle furnace at 1200-1300° C. for 0.5-2 hours, taken out and rapidly cooled to obtain sulphoaluminate cement clinker.
5. The method for preparing sulphoaluminate cement according to claim 1, wherein: In step 5), the mass of the added desulfurized gypsum is 1-15% of the mass of the cement clinker.
6. The method for preparing sulphoaluminate cement according to any one of claims 1 to 5, wherein: In step 5), the specific surface area of the sulphoaluminate cement obtained is 400±10m 2 / ㎏.
Citation Information
Patent Citations
Overall treatment and utilization method for aluminum ash
CN106399693A
Method for preparing sulphate aluminium cement by red mud
CN1837121A
Method and system for producing low-alkalinity sulphoaluminate cement with new mineral system using steel slag
US20210130234A1