Grouting anti-seepage material with high groutability and strong permeability and construction method
The highly injectable and permeable grouting material, composed of nano-silica sol and coagulant, solves the problem of water seepage in the surrounding rock of coal mine roadways, forms a dense seepage-proof structure, improves the self-bearing capacity of the surrounding rock, and achieves the long-term stability of the roadway.
Patent Information
- Application Number
- CN202411129380.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-16
- Publication Date
- 2024-11-19
AI Technical Summary
In existing technologies, conventional grouting materials cannot effectively seal micropores, and chemical grouting materials such as polyurethane have poor durability, leading to severe water seepage in the surrounding rock of coal mine roadways, anchor cable failure, and large deformation and damage to the roadways. There is a lack of grouting and seepage prevention materials with high injectability and strong permeability.
A highly injectable and permeable grouting material composed of nano-silica sol and coagulant is used to form a dense seepage-proof structure by adjusting the ratio of nano-silica sol and coagulant by different volume ratios, combined with pre-injection and delayed grouting processes, thereby blocking the seepage channels of groundwater.
It significantly improves the permeability and self-bearing capacity of the surrounding rock, reduces the amount of tunnel engineering, achieves long-term stability, and replaces highly polluting chemical materials.
Smart Images

Figure CN118978362A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a grouting anti-seepage material with high injection strength and penetration and a construction method, belonging to the field of coal mine seepage underground support engineering. Technical Background
[0002] Due to the special geological conditions, the fissure water in the surrounding rock roof is common in coal mine tunnels. The problems of anchor cable failure and large deformation damage caused by the erosion, softening and muddy surrounding rock caused by the fissure water seriously restrict the safety maintenance of the mine tunnels. Using grouting modification to effectively block the dominant seepage channel of the surrounding rock fissure water is an important technical approach to improve the physical and mechanical properties of the surrounding rock mass and exert its self-bearing capacity.
[0003] Since fractured sandstone, muddy soft rock, and loose coal bodies generally have dual porosity of fractures and matrix, the grouting modification effect is closely related to the injectability of the slurry. The minimum injectable fracture width of conventional inorganic cement slurry and ultrafine cement slurry particles is about 0.1 mm, which can only seal the macroscopic fractures of the rock mass, but has almost no effect on the sealing of fine pores (0.3-5 μm) that play a major role in groundwater seepage. Moreover, under the percolation of micro-cracks in the rock mass, the stone rate of the grouting material and the uniformity of the grouting reinforcement structure are significantly reduced. Highly injectable chemical slurries such as polyurethane and epoxy resin have poor long-term stability of the surrounding rock grouting structure due to the poor durability of the gel, and are restricted in use in some underground projects due to the toxicity, heat generation and cost of chemical slurries. Therefore, in response to the above problems, there is currently a lack of a highly injectable and highly permeable grouting anti-seepage material for underground support projects such as coal mine seepage tunnels. Summary of the invention
[0004] In view of the deficiencies of the prior art, the present invention provides a highly injectable and highly permeable grouting anti-seepage material and a construction method which are green and environmentally friendly.
[0005] To achieve the above technical objectives, the present invention discloses a grouting anti-seepage material with high injection strength and penetration, comprising nano-silica sol and a coagulant. The grouting anti-seepage material with high injection strength and penetration is obtained by adding coagulants in different volume ratios to the nano-silica sol, wherein the volume ratio of the nano-silica sol to the coagulant is (3 to 10):1; the nano-silica sol is an alkaline sodium-type industrial silica sol, and the coagulant is a strong electrolyte solution.
[0006] Furthermore, the viscosity of the alkaline sodium industrial silica sol does not exceed 5mPa·s, the alkaline sodium industrial silica sol contains nano-silicon dioxide particles, the concentration of nano-silicon dioxide is 10-30%, and the average particle size of nano-silicon dioxide does not exceed 20nm; the strong electrolyte solution is KCl solution, and the solution mass concentration is 8-10%.
[0007] A method for preparing a grouting anti-seepage material with high injection strength and penetration, wherein continuous stirring is required when adding a coagulant to the silica sol, the stirring time of the silica sol and the coagulant is not less than 1 minute, and after the coagulant is added, the mixing and stirring time is continued for 2-5 minutes, and the mixing temperature is 10-35°C; the silica sol slurry formed by sufficient mixing does not show a rapid setting phenomenon, does not have particles and snowflake-like suspended matter on a large scale, and the gel time is not less than 5 minutes.
[0008] A construction method for making a grouting anti-seepage material with high penetration strength, adjusting the proportion of the grouting anti-seepage material according to different grouting objects and grouting process requirements, and ensuring that the accelerator is added while stirring continuously until fully mixed, the specific contents are as follows:
[0009] When the grouting object is a fractured rock mass without water seepage, pre-grouting is used for pre-blocking, and grouting is performed using a grouting anti-seepage material prepared with a volume ratio of nano-silica sol and coagulant of (6-10):1;
[0010] When the grouting object is a fractured rock mass and has already seen water, delayed grouting is used for water blocking, and grouting is performed using a grouting anti-seepage material prepared with a volume ratio of nano-silica sol and coagulant of (3-7):1; to prevent the material from being washed out by running water during grouting, first prepare the grouting anti-seepage material according to a volume ratio of nano-silica sol and coagulant of 3:1 and perform grouting, and then continue to increase the proportion of nano-silica sol until the running water around the hole is blocked;
[0011] When the grouting object is mudstone and loose coal body and there is no water seepage, pre-grouting is used for pre-blocking. When grouting, a grouting anti-seepage material prepared with a volume ratio of nano-silica sol and coagulant of (8-10):1 is used for grouting. The grouting anti-seepage material with this ratio is used for long-term low-pressure slow seepage grouting;
[0012] When the grouting object is mudstone and loose coal body and has water seepage, before using delayed grouting for water blocking, first use conventional cement slurry to block larger pores and cracks. After the cement slurry solidifies, use grouting anti-seepage material prepared with nano-silica sol and coagulant in a volume ratio of (8-10):1 to perform long-term low-pressure slow seepage grouting;
[0013] The grouting construction time of the grouting anti-seepage material is controlled within 80% of the gel time of the grouting material. The gel time of the cementitious material is measured by the inverted cup method at the engineering site.
[0014] Furthermore, when conducting advance pre-grouting and delayed water-blocking grouting in fractured rock mass, the grouting pressure is 2-4 MPa; when conducting advance pre-grouting and delayed water-blocking grouting in permeable muddy rock mass and loose coal mass, the grouting pressure does not exceed 1 MPa.
[0015] Furthermore, the head distance of the delayed working face of the delayed grouting is 30 to 60 m.
[0016] Beneficial effects: The grouting anti-seepage material prepared by this method has good fluidity and strong permeability, and contains a large number of fine particles inside, with strong injectability, and can penetrate into small gaps that other materials cannot penetrate. Compared with conventional slurry materials, nano-silica sol has the remarkable characteristics of small particle size, low viscosity, strong permeability, dense gel and stable chemical properties. Compared with conventional cement slurry, the injectability is more than 300 times higher, which can effectively penetrate into the microporous cracks of the rock matrix. After solidification, it can form a dense and stable anti-seepage structure to greatly reduce the permeability coefficient of the rock mass; at the same time, according to different needs, the proportion, gel timing and grouting pressure are reasonably configured to effectively block the dominant seepage channels of groundwater under the three surrounding rocks of fractured rock mass, mudstone mass and loose coal mass, and form a surrounding rock water-stopping shielding layer. Thereby improving the bearing strength of the surrounding rock itself, reducing the amount of repair work of the tunnel surrounding rock, greatly improving the long-term stability of the seepage tunnel, and realizing the replacement of highly polluting chemical-based anti-seepage materials. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 Schematic diagram of the particle size distribution of nano-silica sol in an embodiment of the present invention;
[0018] Figure 2 This is a microstructure diagram of nano-silica sol in an embodiment of the present invention. DETAILED DESCRIPTION
[0019] An embodiment of the present invention is further described below in conjunction with the accompanying drawings:
[0020] Embodiment 1:
[0021] The surrounding rock of the roof of a certain tunnel is a fractured rock mass, and there is an aquifer above it. In order to reduce the impact of groundwater on tunnel excavation, the advanced pre-grouting process is used to carry out grouting and water blocking.
[0022] The ratio of the grouting anti-seepage material used is: the volume ratio of nano silica sol and coagulant is 8:1. The viscosity of the silica sol is 4mPa·s, the concentration of nano silicon dioxide is 30%, and the average particle size is 10nm; the strong electrolyte solution is KCl solution, and the mass concentration of the solution is 10%.
[0023] The stirring time for adding the coagulant to the silica sol is 2 minutes. After the coagulant is added, the mixing and stirring time is continued for 3 minutes, and the mixing temperature is 23°C. The silica sol slurry formed by sufficient mixing does not contain particles and snowflake-like suspended matter. The gel time of the grouting material tested on-site by the inverted cup method is 295 minutes.
[0024] The on-site grouting drilling distance is 2.4m, the grouting pressure is 3MPa, and the grouting time is set to 180min.
[0025] Embodiment 2:
[0026] The surrounding rock of the roof of a certain tunnel is a fractured rock mass with an aquifer above it. When the working face is excavated to 15-25m, water leakage occurs in the roof. The delayed grouting process is used to grout and block the water.
[0027] Grouting of anti-seepage material prepared by nano-silica sol and coagulant in a volume ratio of (3-7): 1 is used. The viscosity of silica sol is 3mPa·s, the concentration of nano-silica is 10%, and the average particle size is 10nm; the strong electrolyte solution is KCl solution, and the mass concentration of the solution is 10%.
[0028] First, the grouting anti-seepage material was prepared according to the volume ratio of nano-silica sol and coagulant 3:1. The coagulant was added to the silica sol and stirred for 1 minute. After the coagulant was added, the mixing time was continued for 2 minutes, and the mixing temperature was 28°C. The silica sol slurry formed by the mixture did not have particles and snowflake-like suspended matter. The gel time of the grouting material tested on site by the inverted cup method was 11 minutes. The on-site grouting position was 55 meters away from the front of the working face, the grouting drilling distance was 1 meter, the grouting pressure was 4MPa, and the grouting time was set to 8 minutes.
[0029] After the above slurry solidifies, the grouting anti-seepage material is prepared according to the volume ratio of nano silica sol and coagulant 5:1. The coagulant is added to the silica sol and stirred for 1 minute. After the coagulant is added, the mixing time is continued for 3 minutes, and the mixing temperature is 28°C; the silica sol slurry formed by the mixture does not have particles and snowflake-like suspended matter. The gel time of the grouting material tested on site by the inverted cup method is 52 minutes. The on-site grouting position is 55m away from the front of the working face, the grouting drilling distance is 1.5m, the grouting pressure is 3MPa, and the grouting time is set to 39 minutes.
[0030] After the above slurry solidifies, the grouting anti-seepage material is prepared according to the volume ratio of nano silica sol and coagulant 7:1. The coagulant is added to the silica sol and stirred for 1 minute. After the coagulant is added, the mixing time is continued for 4 minutes, and the mixing temperature is 28°C; the silica sol slurry formed by the mixture does not have particles and snowflake-like suspended matter. The gel time of the grouting material tested on site by the inverted cup method is 167 minutes. The on-site grouting position is 55m away from the front of the working face, the grouting drilling distance is 2m, the grouting pressure is 2MPa, and the grouting time is set to 120min.
[0031] Embodiment 3:
[0032] The surrounding rock of the roof of a certain tunnel is mudstone, and there is an aquifer above it. In order to reduce the impact of groundwater on tunnel excavation, the advanced pre-grouting technology is used to carry out grouting and water blocking.
[0033] The ratio of the grouting anti-seepage material used is: the volume ratio of nano silica sol and coagulant is 10:1. The viscosity of the silica sol is 3mPa·s, the concentration of nano silicon dioxide is 30%, and the average particle size is 10nm; the strong electrolyte solution is KCl solution, and the mass concentration of the solution is 10%.
[0034] The stirring time for adding the coagulant to the silica sol is 2 minutes. After the coagulant is added, the mixing and stirring time is continued for 5 minutes, and the mixing temperature is 26°C. The silica sol slurry formed by sufficient mixing does not contain particles and snowflake-like suspended matter. The gel time of the grouting material tested on-site by the inverted cup method is 645 minutes.
[0035] The on-site grouting drilling distance is 3.5m, the grouting pressure is 0.5MPa, and the grouting time is set to 416min.
[0036] Embodiment 4:
[0037] The surrounding rock of the roof of a certain tunnel is loose coal body, with an aquifer above it. When the working face is excavated to 15-25m, water leakage occurs in the roof. In order to reduce the impact of groundwater on tunnel excavation, cement slurry is first used for grouting, and the grouting anti-seepage material is used for grouting and water blocking.
[0038] When using cement grouting, the water-cement ratio is 0.8, the grouting drilling distance is 0.8m, the grouting pressure is 3MPa, and the grouting time is 34min.
[0039] After the cement slurry solidifies, grouting is performed using a grouting anti-seepage material with a volume ratio of nano-silica sol and coagulant of 9:1. The viscosity of the silica sol is 3mPa·s, the concentration of nano-silica is 20%, and the average particle size is 10nm; the strong electrolyte solution is a KCl solution with a mass concentration of 8%.
[0040] The stirring time for adding the coagulant to the silica sol is 2 minutes. After the coagulant is added, the mixing and stirring time is continued for 4 minutes, and the mixing temperature is 24°C. The silica sol slurry formed by sufficient mixing does not contain particles and snowflake-like suspended matter. The gel time of the grouting material tested on-site by the inverted cup method is 452 minutes.
[0041] The on-site grouting drilling distance is 2.5m, the grouting pressure is 0.8MPa, and the grouting time is set to 320min.
[0042] Table 1 shows the material properties and grouting effects of the four embodiments. It can be seen that in the case of no water seepage, the pre-grouting of the grouting anti-seepage material can achieve no water seepage on the roof, and in the case of water seepage, the delayed grouting of the grouting anti-seepage material can achieve no water dripping on the roof. Figure 1 and Figure 2 Figure 2 is the particle size distribution curve and microstructure diagram of nano-silica sol.
[0043] Table 1 Material properties and grouting effects
[0044]
Claims
1. A grouting anti-seepage material with high injection strength and penetration, characterized in that: The invention comprises nano silica sol and a coagulant. By adding the coagulant in different volume ratios to the nano silica sol, a grouting anti-seepage material with high injection strength and penetration is obtained, wherein the volume ratio of the nano silica sol to the coagulant is (3-10):1; the nano silica sol is an alkaline sodium type industrial silica sol, and the coagulant is a strong electrolyte solution.
2. A grouting anti-seepage material with high injection strength and penetration according to claim 1, characterized in that: The viscosity of the alkaline sodium type industrial silica sol does not exceed 5mPa·s. The alkaline sodium type industrial silica sol contains nano silicon dioxide particles with a concentration of 10-30% and an average particle size of no more than 20nm. The strong electrolyte solution is KCl solution with a mass concentration of 8-10%.
3. A method for configuring the highly injectable and highly permeable grouting anti-seepage material according to claim 1, characterized in that: When adding the coagulant to the silica sol, continuous stirring is required. The stirring time for adding the silica sol and the coagulant should not be less than 1 minute. After the coagulant is added, the mixing and stirring time should continue for 2-5 minutes, and the mixing temperature should be 10-35°C. The silica sol slurry formed by sufficient mixing does not show rapid setting phenomenon, and particles and snowflake-like suspended matter do not appear on a large scale, and the gel time is not less than 5 minutes.
4. A construction method using the high-injection-strength-permeable grouting anti-seepage material according to claim 1, characterized in that: According to different grouting objects and grouting process requirements, adjust the ratio of grouting anti-seepage materials, and ensure that the accelerator is added while stirring until fully mixed. The specific contents are as follows: When the grouting object is a fractured rock mass without water seepage, pre-grouting is used for pre-blocking, and grouting is performed using a grouting anti-seepage material prepared with a volume ratio of nano-silica sol and coagulant of (6-10):1; When the grouting object is a fractured rock mass and has already seen water, delayed grouting is used for water blocking, and grouting is performed using a grouting anti-seepage material prepared with a volume ratio of nano-silica sol and coagulant of (3-7):1; to prevent the material from being washed out by running water during grouting, first prepare the grouting anti-seepage material according to a volume ratio of nano-silica sol and coagulant of 3:1 and perform grouting, and then continue to increase the proportion of nano-silica sol until the running water around the hole is blocked; When the grouting object is mudstone and loose coal body and there is no water seepage, pre-grouting is used for pre-blocking. When grouting, a grouting anti-seepage material prepared with a volume ratio of nano-silica sol and coagulant of (8-10):1 is used for grouting. The grouting anti-seepage material with this ratio is used for long-term low-pressure slow seepage grouting; When the grouting object is mudstone and loose coal body and has water seepage, before using delayed grouting for water blocking, first use conventional cement slurry to block larger pores and cracks. After the cement slurry solidifies, use grouting anti-seepage material prepared with nano-silica sol and coagulant in a volume ratio of (8-10):1 to perform long-term low-pressure slow seepage grouting; The grouting construction time of the grouting anti-seepage material is controlled within 80% of the gel time of the grouting material. The gel time of the cementitious material is measured by the inverted cup method at the engineering site.
5. The construction method according to claim 4, characterized in that: When conducting advance pre-grouting and delayed water plugging grouting in fractured rock mass, the grouting pressure is 2-4 MPa; When conducting advance pre-grouting and delayed water-blocking grouting in permeable muddy rock and loose coal, the grouting pressure shall not exceed 1MPa.
6. The construction method according to claim 4, characterized in that: The head distance of the delayed working face of the delayed grouting is 30 to 60m.
Citation Information
Patent Citations
Silica sol slow infiltration reinforcing method of argillaceous soft rock
CN105201528A
Penetration curing construction method for weak-permeability stratum and silica sol nano slurry
CN111472345A
Silicon-based grouting material suitable for reinforcement and anti-permeability treatment of compact and soft stratum and preparation method of silicon-based grouting material
CN116199490A
High-performance cement-silica sol grouting material and preparation method thereof
CN118084447A
Manufacturing method of cement-free water blocking grout forming silica-sol phase and grouting method using the same
KR102435539B1
Cited By
Low-temperature inorganic grouting reinforcement material as well as production equipment and processing method thereof
CN120622903A