High-strength concrete material for prefabricated duct piece of wind power mixing tower and preparation method of high-strength concrete material

By clarifying the mix ratio parameters of high-strength concrete of prefabricated pipe sheets of wind power mixed towers, the problem of insufficient mix ratio design in the existing technology is solved, efficient production and construction are achieved, and mold removal and load conditions are met. Short-cycle shipping needs improve production efficiency and durability.

CN118978364APending Publication Date: 2024-11-19GUANGDONG MINGYANG WIND POWER IND GRP CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410970070.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

The prior art cannot effectively meet the mix ratio design requirements of prefabricated high-strength concrete for wind power mixed towers, especially under the conditions of increasing the height and load of the tower, it is difficult to meet the requirements of mold removal strength, short-term shipment and appearance quality.

Method used

Provide a high-strength concrete material of prefabricated pipe sheet of wind power mixed tower and its preparation method. The mixing ratio parameters of C80~C95 high-strength concrete include key parameters such as aggregate sand ratio, water cement ratio, and slump, and reduce through adjustment The dosage of water agent and additive dosage achieves rapid calculation and styling, improving operability.

Benefits of technology

It realizes rapid calculation and finalization of high-strength concrete, meets the early compressive strength and durability requirements, shortens production and construction cycles, improves mold turnover and production efficiency, reduces production costs, and ensures the crack resistance of concrete. and appearance quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118978364A_ABST
    Figure CN118978364A_ABST
Patent Text Reader

Abstract

The invention discloses a wind power mixing tower prefabricated duct piece high-strength concrete material and a preparation method thereof.The high-strength concrete material is C80-C95 high-strength concrete and comprises the following components: 560-620 parts of a cementing material, 33-50 parts of silica fume, 80-125 parts of microbeads and 12-20 parts of a water reducing agent; wherein the aggregate sand ratio of the high-strength concrete material is 35%-39%, the real water-binder ratio is 0.20-0.23, the designed volume weight is 2450-2500 parts, and the slump is 180 + / -20 mm; the high-strength concrete material for the prefabricated duct piece of the wind power mixed tower has good durability and flowability, can meet production and construction of a horizontal mold, is easy for manual finishing and plastering, and realizes mold removal in advance while ensuring that the mechanical property and durability of the duct piece concrete meet design requirements; the turnover rate and the production efficiency of the formwork are effectively improved, short-period delivery, transportation and hoisting construction of the mixed tower duct pieces can be achieved, and the production and construction period is shortened.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of wind power high-strength concrete material manufacturing, and in particular to a wind power mixed tower prefabricated pipe segment high-strength concrete material and a preparation method thereof. Background Art

[0002] As one of the most important components in the field of new energy, wind power generation has attracted more and more attention due to its safe, clean and renewable characteristics. Due to its unique generation method, wind resources become more abundant as the height increases. With the advancement of wind power technology, in order to further improve the utilization efficiency of wind energy by wind turbines, the application of large-megawatt wind turbines has become an inevitable trend. The inevitable way to increase the capacity of a single unit is to increase the height of the tower. The tower is the main structure for supporting and obtaining the height of the wind turbine. With the increase in the capacity of the wind turbine, the height and bearing capacity of the mixed tower in the structural design are also increasing accordingly. This requires that the concrete design strength grade of the prefabricated mixed tower segments be increased accordingly. High-strength concrete of grade C80 and above is widely used in prefabricated mixed tower segments with higher heights and more complex loads. However, when using high-strength grade concrete in the production of prefabricated segments, the concrete is required to develop fast early strength to meet the needs of demolding and short-cycle delivery, and also have good crack resistance and workability to meet the requirements of durability and appearance quality after the segments are finished and plastered. Therefore, high requirements are placed on the mix ratio of high-strength concrete for wind power prefabricated mixed tower segments.

[0003] In the existing concrete mix design method, the key mix parameters for high-strength concrete, especially prefabricated high-strength concrete used in the field of wind power towers, cannot meet the actual needs. In the actual application process, a large number of tests, verifications and adjustments are still required to obtain a mix that meets the requirements. For example, the water-binder ratio and cementitious material dosage of high-strength concrete of strength grade C80 and above in the "Technical Specification for Application of High-Strength Concrete" JGJ / T 281 are stipulated in the actual production of tower segment concrete. The water-binder ratio range is large and the cementitious material dosage is low, which makes it difficult to meet the needs of demolding strength and short-term hoisting construction in the actual application of the segment. However, there is no clear provision for the selection and calculation of mix parameters for concrete of C80 and above in the "Ordinary Concrete Mix Design Code" JGJ 55, and other provisions are not applicable to the mix design of prefabricated high-strength concrete of C80 and above. Summary of the invention

[0004] The purpose of the present invention is to overcome the shortcomings and disadvantages of the prior art, and to provide a high-strength concrete material for prefabricated segments of wind power hybrid towers and a preparation method thereof, which can meet the mix ratio of C80-C95 high-strength concrete for wind power hybrid tower segments produced by horizontal molds, realize rapid calculation and finalization of the mix ratio, and make clear provisions for key mix ratio parameters such as the amount of cementitious material, the amount of mineral admixtures, the sand ratio, the water-binder ratio, and the slump; and make provisions for the subsequent adjustment of the mix ratio obtained by the preliminary calculation, including the sand ratio, the amount of admixture and the mix ratio, which are simple to adjust, and the overall operability is strong.

[0005] To achieve the above object, the technical solution provided by the present invention is as follows: a high-strength concrete material for prefabricated pipe segments of a wind power tower, the high-strength concrete material is C80-C95 high-strength concrete, and the components include:

[0006]

[0007] The aggregate sand ratio of the high-strength concrete material is 35% to 39%, the real water-cement ratio is 0.20 to 0.23, the design bulk density is 2450 to 2500 parts, and the slump is 180±20 mm.

[0008] Furthermore, the C80-C95 high-strength concrete includes C80 high-strength concrete, C85 high-strength concrete, C90 high-strength concrete and C95 high-strength concrete.

[0009] Furthermore, the C80 high-strength concrete components include:

[0010]

[0011]

[0012] Furthermore, the C85 high-strength concrete components include:

[0013]

[0014] Furthermore, the C90 high-strength concrete components include:

[0015]

[0016] Furthermore, the C95 high-strength concrete components include:

[0017]

[0018] Furthermore, the cementitious material is one of 52.5 ordinary silicate cement and silicate cement; the water demand ratio of the silica ash is ≤120%, the activity index of the silica ash is ≥115%, and the SiO2 content of the silica ash is ≥90%; the water demand ratio of the microspheres is ≤100%, the 28d activity index of the microspheres is ≥105%, and the loss on ignition of the microspheres is ≤5%; the water reducer is a polycarboxylic acid high-performance water agent, the water reduction rate of the water reducer is ≥25%, and the solid content of the water reducer is ≥10%.

[0019] Furthermore, the grading of the aggregate is continuous grading, the fineness modulus of the river sand of the aggregate is 2.3-3.1, the mud content of the aggregate is ≤2.0%, the particle size of the crushed stone of the aggregate is 5-20 mm, and the crushing index of the crushed stone of the aggregate is ≤8%.

[0020] A method for preparing the high-strength concrete material for prefabricated segments of a wind power tower comprises the following steps:

[0021] S1. Selecting raw materials for prefabricated high-strength concrete components of wind power tower;

[0022] S2. Determine the required strength grade of concrete;

[0023] S3, preliminarily selecting the mix ratio between the component raw materials according to the strength grade determined in step S2;

[0024] S4. Determine the aggregate sand and gravel gradation and fineness modulus in concrete;

[0025] S5. Determine the concrete sand ratio;

[0026] S6. Determine the water reduction rate and solid content of the water reducer, and adjust the dosage of the water reducer according to actual needs;

[0027] S7. Determine the final raw material mix ratio, prepare high-strength concrete materials, and verify their strength.

[0028] Furthermore, the strength grade is C80-C95.

[0029] Compared with the prior art, the present invention has the following advantages and beneficial effects:

[0030] 1. The C80-C95 high-strength concrete mix ratio of the present invention can meet the requirements that the 1d compressive strength is not less than 50% of the design strength, the 14d compressive strength is not less than 100% of the design strength, the 28d compressive strength is not less than 115% of the design strength, the 14d solid rebound strength is not less than the design strength, the 28d static elastic modulus is not less than 40GPa, and it has good durability and fluidity, can meet the horizontal mold production and construction, and is easy to manually finish and plaster. While ensuring that the mechanical properties and durability of the segment concrete meet the design requirements, it can realize early demolding, effectively improve the turnover rate and production efficiency of the template, and can realize the short-cycle delivery, transportation and hoisting construction of the tower segment, shortening the production and construction cycle.

[0031] 2. The C80-C95 mix ratio specified in the present invention can be used to quickly calculate and finalize the mix ratio of concrete of the corresponding strength grade, and can achieve early demolding when horizontal molds are used in prefabrication plants. The turnover rate of the mold is accelerated, and production efficiency is improved. At the same time, the early age compressive strength of the concrete develops at a faster rate. The 14d-old test block and entity strength can reach 100% of the design strength, which means that transportation and hoisting construction can be carried out 14d after production, shortening the stacking cycle of the pipe segments and reducing production costs. At the same time, when using horizontal molds for production, the concrete under the mix ratio has good working performance and crack resistance, and the surface quality is good after demolding and after artificial finishing and plastering. The production and pouring construction are smooth, and it has good practicality.

[0032] In summary, the mix ratio specified in the present invention can effectively improve production efficiency, shorten production and construction period, and effectively reduce production costs under the premise of meeting the basic requirements of mechanical properties, durability and working performance. It has good technical stability and reliability, and the design process is simple and fast in application, with strong operability, and has good practical and popularization and application value. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 The present invention is a flow chart of a method for preparing high-strength concrete materials for prefabricated segments of wind turbine hybrid towers. DETAILED DESCRIPTION

[0034] The present invention is further described below in conjunction with a number of specific embodiments.

[0035] Example 1

[0036] See also Figure 1 As shown, this embodiment provides a method for preparing a high-strength concrete material for a prefabricated pipe segment of a wind power tower, comprising the following steps:

[0037] S1. Selecting raw materials for prefabricated high-strength concrete components of wind power tower;

[0038] S2. Determine the required strength grade of C80 to C95 for concrete;

[0039] S3, preliminarily selecting the mix ratio between the component raw materials according to the strength grade determined in step S2;

[0040] S4. Determine the aggregate sand and gravel gradation and fineness modulus in concrete;

[0041] S5. Determine the concrete sand ratio;

[0042] S6. Determine the water reduction rate and solid content of the water reducer, and adjust the dosage of the water reducer according to actual needs;

[0043] S7. Determine the final raw material mix ratio, prepare high-strength concrete materials, and verify their strength.

[0044] Example 2

[0045] This embodiment provides a process for determining the mix ratio of the C80 high-strength concrete material for the wind power prefabricated mixed tower segment prepared according to Example 1 as follows:

[0046] A. Select cementitious materials, silica fume and microspheres. The cementitious material is P·O52·5 cement. The water demand ratio of silica fume is 113%, the activity index measured by the 7d rapid method is 121%, the SiO2 content is 92%, the water demand ratio of microspheres is 95%, the 28d activity index is 110%, the ignition loss is 3.4%, the gradation of aggregates is continuous gradation, the fineness modulus of river sand is 2.6, the mud content is 1.7%, the particle size of crushed stone is 5-20mm, the crushing index is 6%, the water reduction rate of water reducer is 28%, and the solid content is 20%;

[0047] B. The mix parameters are selected according to the design strength grade C80, including the following parameters: 560 parts of cementitious materials, 447 parts of P·O52·5 cement, 33 parts of silica fume, 80 parts of microspheres, true water-binder ratio of 0.23, and design bulk density of 2450 parts;

[0048] C. Adjust the sand ratio according to the sand and gravel grading and the fineness modulus of sand. The optimal sand ratio is 36%. The water reducing agent is adjusted to 12 parts when the slump reaches 180±20mm. The measured slump is 160mm and the actual water consumption is 119 parts.

[0049] Example 3

[0050] This embodiment provides a process for determining the concrete mix ratio of the C85 high-strength concrete material for the wind power prefabricated mixed tower segment prepared according to Embodiment 1 as follows:

[0051] A. According to the provisions of the present invention, cement, silica fume and microspheres are selected. P·O52·5 cement is selected as cement, the water demand ratio of silica fume is 108%, the activity index measured by the 7d rapid method is 125%, the SiO2 content is 91%, the water demand ratio of microspheres is 96%, the 28d activity index is 115%, the loss on ignition is 2.7%, the gradation of aggregates is continuous gradation, the fineness modulus of river sand is 2.8, the mud content is 1.4%, the particle size of crushed stone is 5-20mm, the crushing index is 6%, the water reduction rate of water reducer is 28%, and the solid content is 20%;

[0052] B. The mix parameters are selected according to the design strength grade C85, including the following parameters: the amount of cementitious materials is 580 parts, P·O52·5 cement is 450 parts, silica fume is 35 parts, micro beads are 95 parts, the real water-binder ratio is 0.22, and the design bulk density is 2460 parts;

[0053] C. Adjust the sand ratio according to the sand and gravel grading and the fineness modulus of sand. The optimal sand ratio is 37%. The water reducing agent is adjusted to 14 parts when the slump reaches 180±20mm. The actual slump is 170mm and the actual water consumption is 116 parts.

[0054] Example 4

[0055] This embodiment provides a process for determining the concrete mix ratio of the C90 high-strength concrete material for the prefabricated mixed tower segment of a wind power plant prepared according to Embodiment 1 as follows:

[0056] A. According to the provisions of the present invention, cement, silica fume and microspheres are selected. P·O52·5 cement is selected as cement, the water requirement ratio of silica fume is 108%, the activity index measured by the 7d rapid method is 125%, the SiO2 content is 92%, the water requirement ratio of microspheres is 98%, the 28d activity index is 113%, the loss on ignition is 3.1%, the gradation of aggregates is continuous gradation, the fineness modulus of river sand is 2.9, the mud content is 1.6%, the particle size of crushed stone is 5-20mm, the crushing index is 5%, the water reduction rate of water reducer is 30%, and the solid content is 21%;

[0057] B. The mix parameters are selected according to the design strength grade C90, including the following parameters: 600 parts of cementitious materials, 442 parts of P·O52·5 cement, 48 parts of silica fume, 110 parts of microspheres, true water-binder ratio of 0.21, and design bulk density of 2480 parts;

[0058] C. Adjust the sand ratio according to the sand and gravel grading and the fineness modulus of sand. The optimal sand ratio is 38%. The water reducing agent is adjusted to 17 parts when the slump reaches 180±20mm. The measured slump is 190mm and the actual water consumption is 113 parts.

[0059] Example 5

[0060] This embodiment provides a process for determining the concrete mix ratio of the C95 high-strength concrete material for the wind power prefabricated mixed tower segment prepared according to Embodiment 1 as follows:

[0061] A. According to the provisions of the present invention, cement, silica fume and microspheres are selected. P·O52·5 cement is selected as cement, the water requirement ratio of silica fume is 110%, the activity index measured by the 7d rapid method is 124%, the SiO2 content is 95%, the water requirement ratio of microspheres is 93%, the 28d activity index is 111%, the ignition loss is 3.2%, the gradation of aggregates is continuous gradation, the fineness modulus of river sand is 3.0, the mud content is 1.2%, the particle size of crushed stone is 5-20mm, the crushing index is 5%, the water reduction rate of water reducer is 30%, and the solid content is 21%;

[0062] B. The mix parameters are selected according to the design strength grade C95, including the following parameters: 620 parts of cementitious materials, 445 parts of P·O52·5 cement, 50 parts of silica fume, 125 parts of microspheres, true water-binder ratio of 0.20, and design bulk density of 2500 parts;

[0063] C. Adjust the sand ratio according to the sand and gravel grading and the fineness modulus of sand. The optimal sand ratio is 39%. The water reducing agent is adjusted to 20 parts when the slump reaches 180±20mm. The actual slump is 200mm and the actual water consumption is 108 parts.

[0064] The embodiments described above are only preferred embodiments of the present invention and are not intended to limit the scope of implementation of the present invention. Therefore, all changes made according to the shape and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A high-strength concrete material for prefabricated segments of wind power towers, characterized in that: The high-strength concrete material is C80-C95 high-strength concrete, and the components include: The aggregate sand ratio of the high-strength concrete material is 35% to 39%, the real water-cement ratio is 0.20 to 0.23, the design bulk density is 2450 to 2500 parts, and the slump is 180±20 mm.

2. The high-strength concrete material for prefabricated segments of wind turbine towers according to claim 1 is characterized in that: The C80-C95 high-strength concrete includes C80 high-strength concrete, C85 high-strength concrete, C90 high-strength concrete and C95 high-strength concrete.

3. The high-strength concrete material for prefabricated segments of wind turbine towers according to claim 2 is characterized in that: The C80 high-strength concrete components include:

4. The high-strength concrete material for prefabricated segments of wind turbine towers according to claim 2, characterized in that: The C85 high-strength concrete components include:

5. The high-strength concrete material for prefabricated segments of wind power tower according to claim 2, characterized in that: The C90 high-strength concrete components include:

6. The high-strength concrete material for prefabricated segments of wind power tower according to claim 2, characterized in that: The C95 high-strength concrete components include:

7. The high-strength concrete material for prefabricated segments of wind turbine towers according to claim 1, characterized in that: The cementitious material is one of 52.5 ordinary silicate cement and silicate cement; the water demand ratio of the silica ash is ≤120%, the activity index of the silica ash is ≥115%, and the SiO2 content of the silica ash is ≥90%; the water demand ratio of the microspheres is ≤100%, the 28d activity index of the microspheres is ≥105%, and the ignition loss of the microspheres is ≤5%; the water reducer is a polycarboxylic acid high-performance water agent, the water reduction rate of the water reducer is ≥25%, and the solid content of the water reducer is ≥10%.

8. The high-strength concrete material for prefabricated segments of wind turbine towers according to claim 1, characterized in that: The grading of the aggregate is continuous grading, the fineness modulus of the river sand of the aggregate is 2.3-3.1, the mud content of the aggregate is ≤2.0%, the particle size of the crushed stone of the aggregate is 5-20mm, and the crushing index of the crushed stone of the aggregate is ≤8%.

9. A method for preparing the high-strength concrete material for prefabricated segments of a wind power tower according to any one of claims 1 to 8, characterized in that: The following steps are involved: S1. Selecting raw materials for prefabricated high-strength concrete components of wind power tower; S2. Determine the required strength grade of concrete; S3, preliminarily selecting the mix ratio between the component raw materials according to the strength grade determined in step S2; S4. Determine the aggregate sand and gravel gradation and fineness modulus in concrete; S5. Determine the concrete sand ratio; S6. Determine the water reduction rate and solid content of the water reducer, and adjust the dosage of the water reducer according to actual needs; S7. Determine the final raw material mix ratio, prepare high-strength concrete materials, and verify their strength.

10. The method for preparing high-strength concrete material for prefabricated segments of wind power tower according to claim 9, characterized in that: The strength grade is C80-C95.