Low-temperature fast-firing blank as well as preparation method and application thereof
By adjusting the raw material composition and sintering process of ceramic tile, the problem of poor quality of existing low-temperature fast-fired blanks is solved, and the preparation of ceramic tile with high transparency and wear resistance is achieved, meeting the demand for high-quality and high-priced products, and reducing the Cost and energy consumption.
Patent Information
- Application Number
- CN202410985473.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-22
- Publication Date
- 2024-11-19
AI Technical Summary
The existing low-temperature fast firing blanks have problems with poor quality and poor visual effects in the preparation of ceramic tiles. Especially the stick-printed edge collapse of ceramic products obtained from conventional formulas, which cannot meet customers' demand for high-quality and high-priced products.
By adjusting the composition of the raw materials of the ceramic tile, a low-temperature fast-fired blank formulation is prepared, including kaolin, bentonite, potassium-sodium feldspar, potassium feldspar, talc and bauxite. Combined with wet ball milling and sintering processes, the particle size distribution of the blank is optimized. and sintering temperature to improve the transparency and wear resistance of the glaze.
The preparation of low-temperature fast-fired blanks has been realized, the quality and visual effect of the ceramic tiles have been improved, and the high-transparency, high-temperature and wear resistance are high, and it complies with the national 3C standard, reducing costs and energy consumption.
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of ceramic tile materials, and in particular to low-temperature fast-firing blanks and preparation methods and applications thereof. Background Art
[0002] With the development of society, people have a better yearning for life, and customers have higher and higher requirements for products. Product demand has changed, and customers need higher quality and lower price products. Further innovation in technology is imperative, and the low-temperature fast-fired tile formula research and development project came into being, focusing on improving quality and quantity, while reducing costs and energy consumption, in line with the national carbon peak and carbon neutrality goals! In some formulas, the appearance, quality and taste of ceramic products obtained by using low-temperature fast-fired blanks are comprehensively improved, but ceramic products obtained by conventional formulas generally have poor visual effects of stick printing and edge collapse.
[0003] In view of the above, it is necessary to provide a new type of low-temperature fast-sintering blank and a preparation method and application to overcome the above-mentioned defects. Summary of the invention
[0004] The purpose of the present invention is to provide a low-temperature fast-firing blank and a preparation method and application thereof. By adjusting the composition of various ceramic tile raw materials, the obtained low-temperature fast-firing blank formula has the effect of low-temperature fast-firing, and improves the quality and appearance of the ceramic tile, improves the visual effect, and has a higher glaze transparency as well as corrosion resistance and wear resistance.
[0005] In order to achieve the above object, the present invention provides a low-temperature fast-sintering blank, which comprises, by weight:
[0006] Kaolin: 18-22 parts,
[0007] Bentonite: 2-4 parts,
[0008] Potassium-sodium feldspar: 12-18 parts,
[0009] Potassium feldspar: 45-55 parts,
[0010] 4-6 parts of talc,
[0011] Bauxite: 5-10 parts, liquid dissolving agent 0.5-1 part.
[0012] A method for preparing a low-temperature fast-sintering blank comprises the following steps:
[0013] S1: Mixing according to the formula amount of the blank to obtain a mixed material;
[0014] S2: dividing the mixed material obtained in step S1 into two powders, and ball-milling the two powders respectively to obtain two ball-milled materials with different average particle sizes;
[0015] S3: The two portions of ball mill materials obtained in step S2 are uniformly mixed to prepare the low-temperature fast-sintering blank.
[0016] Preferably, the mixing in step S1 is wet ball milling mixing, and the raw materials are immersed in water during the wet ball milling mixing.
[0017] Preferably, the average particle size of the mixture in step S1 is 60-180 μm.
[0018] Preferably, the mixed material obtained in step S1 is divided into a first powder and a second powder, and the mass ratio of the first powder to the second powder is 1-3:1.
[0019] Preferably, the average particle size of the first ball mill obtained by ball milling the first powder is 70-170 μm, and the average particle size of the second ball mill obtained by ball milling the second powder is 50-120 μm.
[0020] An application of the low-temperature fast-sintering blank as claimed in claim 1, comprising the following steps:
[0021] (a) preparing a low-temperature fast-firing blank formulation process slurry using a low-temperature fast-firing blank formulation process;
[0022] (b) The low-temperature fast-firing blank formulation process slurry obtained in step (a) is powder-sprayed and granulated, pressed and formed, and sintered to obtain a finished product having the low-temperature fast-firing blank formulation process.
[0023] An application of a low-temperature fast-fired blank, in which, in parts by weight, the raw materials of the low-temperature fast-fired blank formulation process slurry in step (a) include: 18-22 parts of kaolin,
[0024] Bentonite: 2-4 parts,
[0025] Potassium-sodium feldspar: 12-18 parts,
[0026] Potassium feldspar: 45-55 parts,
[0027] 4-6 parts of talc,
[0028] Bauxite: 5-10 parts, liquid dissolving agent 0.5-1 part.
[0029] An application of a low-temperature fast-sintering blank, wherein the sintering in step (b) comprises the following steps:
[0030] (i) Heating the temperature to 400-500°C at a rate of 8-10°C / min and keeping the temperature for 5-10 min;
[0031] (ii) heating to 800-900°C at a heating rate of 6-8°C / min and keeping at that temperature for 15-25 min;
[0032] (iii) heating the temperature to 1150-1250°C at a rate of 4-6°C / min and maintaining the temperature for 10-20 min;
[0033] (iv) Rapid cooling to room temperature to complete sintering.
[0034] Compared with the prior art, the beneficial effects are as follows: 1) the present invention adjusts the composition of the blank so that the low-temperature fast-firing blank formula process prepared by the present invention has the effect of low-temperature fast-firing when used for porcelain glazed tiles, and has higher transparency and high temperature resistance and wear resistance;
[0035] 2) The low-temperature fast-firing blank formulation process adjustment of the present invention is innovative, but its application method is simple. The preparation of porcelain glazed tiles can be achieved by simply adjusting the sintering rate. The prepared finished product has the effect of improving quality and quantity, and has high transparency and high temperature resistance and wear resistance.
[0036] Other features and advantages of the present invention will be set forth in the following description, and part will be apparent from the description, or can be understood by implementation of the present invention. Features and advantages of the present invention can be realized and obtained by the elements and combinations specifically pointed out in the appended application scope. These and other features of the present invention will become more clearly understood according to the following description and the appended claims, or can be understood by the implementation of the embodiments described in the present invention. DETAILED DESCRIPTION
[0037] In order to make the purpose, technical solution and beneficial technical effect of the present invention clearer, the present invention is further described in detail below in conjunction with specific implementation methods. It should be understood that the specific implementation methods described in this specification are only for explaining the present invention, not for limiting the present invention.
[0038] It should be understood that the terms "upper", "lower", "front", "back", "left", "right", "top", "bottom", "inside", "outside", etc., to indicate directions or positional relationships, are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific direction, be constructed and operated in a specific direction, and therefore should not be understood as a limitation on the present invention.
[0039] It should also be noted that, unless otherwise clearly specified and limited, the terms such as "install", "connect", "connect", "fix", "set" and the like should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral one; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements. For those of ordinary skill in the art, the specific meanings of the above terms in the present invention can be determined according to the specific circumstances.
[0040] In addition, the terms "first", "second", and "third" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, a feature defined as "first", "second", and "third" may explicitly or implicitly include one or more of the features. In addition, the meaning of "multiple" and "several" refers to two or more, unless otherwise clearly and specifically defined.
[0041] The present invention provides a low-temperature fast-firing blank, which comprises, by weight:
[0042] Kaolin: 18-22 parts,
[0043] Bentonite: 2-4 parts,
[0044] Potassium-sodium feldspar: 12-18 parts,
[0045] Potassium feldspar: 45-55 parts,
[0046] 4-6 parts of talc,
[0047] Bauxite: 5-10 parts, liquid dissolving agent 0.5-1 part.
[0048] The present invention utilizes the adjustment and optimization of different components of raw materials for ceramic tiles to achieve the following performances of low-temperature fast-fired blank formulations: whiteness after firing is greater than 18 degrees, burning loss is less than 5%, shrinkage is less than 9.5%, dry blank strength is greater than 95N, and oxidized black core is less than 2MM (70g powder 15MM thick cake kiln fired);
[0049] The present invention utilizes the adjustment and optimization innovation of different components of ceramic tile raw materials, and the blank is fired at an ambient temperature of 1135-1145 degrees Celsius.
[0050] The present invention utilizes the adjustment and optimization innovation of different components of the raw materials of the ceramic tile to determine the key chemical elements AL content of the formula to be 18-19%, Mg content to be 1.3-1.5%, K content to be 3.6-3.9%, and Na content to be 1.3-1.55%;
[0051] The sintering temperature of the low-temperature fast-firing blank formulation process of the present invention reduces the adverse effects of excessively high sintering temperature on the organic matter in the blank mud and other gas components that are easy to produce on the obtained glaze. The present invention improves the stability and controllability of the formulation by adding a specific weight portion, and can work together with the glaze to improve the appearance of the obtained high-quality tile glaze.
[0052] The components in the low-temperature fast-firing blank formulation process of the present invention cooperate with each other, so that when the low-temperature fast-firing blank formulation process is used in production, it has the effect of improving product quality and appearance. Moreover, the various raw materials of the present invention cooperate with each other, so that during the firing process, the blank and the glaze are combined more smoothly, and the glaze surface has better color and transparency.
[0053] In the low-temperature fast-firing blank provided by the present invention, kaolin: 18-22 parts, for example, it can be 18 parts, 19 parts, 20 parts, 21 parts, 22 parts, but is not limited to the listed values, other unlisted values within the numerical range are also applicable, preferably 18-20 parts.
[0054] In the low-temperature fast-firing blank provided by the present invention, bentonite: 2-4 parts, for example, it can be 2 parts, 2.5 parts, 3 parts, 3.5 parts, 4 parts, but is not limited to the listed values. Other unlisted values within the numerical range are also applicable, preferably 2-3 parts.
[0055] In the low-temperature fast-fired blank provided by the present invention, potassium-sodium feldspar: 12-18 parts, for example, it can be 12 parts, 13 parts, 14 parts, 15 parts, 16 parts, 17 parts or 18 parts, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable, preferably 14-17 parts.
[0056] In the low-temperature fast-fired blank provided by the present invention, potassium feldspar: 45-55 parts, for example, it can be 45 parts, 46 parts, 47 parts, 48 parts, 49 parts, 50 parts or 51 parts, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable, preferably 46-50 parts.
[0057] In the low-temperature fast-firing blank provided by the present invention, talc is 4-6 parts, for example, it can be 4 parts, 4.5 parts, 5 parts, 5.5 parts or 6 parts, but it is not limited to the listed values. Other unlisted values within the numerical range are also applicable, preferably 4-5 parts.
[0058] In the low-temperature fast-firing blank provided by the present invention, bauxite: 5-10 parts, for example, it can be 5 parts, 6 parts, 7 parts, 8 parts, 9 parts, 9.5 parts or 10 parts, but is not limited to the listed values. Other unlisted values within the numerical range are also applicable, preferably 8-10 parts.
[0059] In the low-temperature fast-firing blank provided by the present invention, the liquid disintegrator is 0.5-1 part, for example, it can be 0.5 part, 0.6 part, 0.7 part, 0.8 part, 0.9 part, 0.95 part or 1 part, but is not limited to the listed values. Other unlisted values within the numerical range are also applicable, preferably 0.5-0.7 part.
[0060] Preferably, the total weight proportion of the bentonite and talc is 7-8 parts, for example, it can be 7 parts, 7.1 parts, 7.2 parts, 7.3 parts, 7.4 parts, 7.5 parts, 7.6 parts, 7.7 parts, 7.8 parts, 7.9 parts or 8 parts, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0061] Preferably, the added fixed component of talc and bauxite is 12 parts, which can be considered to be used interchangeably, but are not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0062] Preferably, the added fixed component of kaolin and bentonite is 24 parts, which can be considered to be used interchangeably, but are not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0063] The present invention provides a method for preparing a low-temperature fast-sintering blank, the preparation method comprising the following steps:
[0064] S1: Mixing according to the formula amount of the blank to obtain a mixed material;
[0065] S2: dividing the mixed material obtained in step S1 into two powders, and ball-milling the two powders respectively to obtain two ball-milled materials with different average particle sizes;
[0066] S3: The two portions of ball mill materials obtained in step S2 are uniformly mixed to prepare the low-temperature fast-sintering blank.
[0067] Preferably, the mixing in step S1 is wet ball milling mixing, and the raw materials are immersed in water during the wet ball milling mixing.
[0068] Preferably, the average particle size of the mixture in step S1 is 60-180 μm, for example, it can be 60 μm, 70 μm, 80 μm, 90 μm, 100 μm, 110 μm, 120 μm, 130 μm, 140 μm, 150 μm, 160 μm, 170 μm or 180 μm, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0069] Preferably, the mixed material obtained in step S1 is divided into a first powder and a second powder, and the mass ratio of the first powder to the second powder is 1-3:1, for example, it can be 1:1, 1.5:1, 2:1, 2.5:1 or 3:1, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0070] Preferably, the ball milling in step S2 is wet ball milling, in which water is used to immerse the raw materials.
[0071] Preferably, the average particle size of the first ball mill obtained by ball milling the first powder is 70-170 μm, for example, it can be 70 μm, 80 μm, 90 μm, 100 μm, 110 μm, 120 μm, 130 μm, 140 μm, 150 μm, 160 μm, 170 μm, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0072] Preferably, the average particle size of the second ball mill obtained by ball milling the second powder is 50-120 μm, for example, it can be 50 μm, 60 μm, 70 μm, 80 μm, 90 μm, 100 μm, 110 μm, 120 μm, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0073] As a preferred technical solution of the preparation method of the present invention, the preparation method comprises the following steps: (1) wet ball milling the mixed raw materials according to the formula, wherein the raw materials are immersed in water during the wet ball milling to obtain a mixed material with an average particle size of 60-180 μm;
[0074] (2) dividing the mixed material obtained in step (1) into a first powder and a second powder, wherein the mass ratio of the first powder to the second powder is 1-3:1; and wet-milling the first powder and the second powder respectively, wherein the raw materials are immersed in water during the wet-milling; the average particle size of the first ball-milled material obtained by ball-milling the first powder is 70-170 μm; and the average particle size of the second ball-milled material obtained by ball-milling the second powder is 50-120 μm;
[0075] (3) The first ball mill obtained in step (2) is uniformly mixed with the second ball mill to prepare the low-temperature fast-sintering blank.
[0076] The present invention provides an application of a low-temperature fast-sintering blank, and the application comprises the following steps:
[0077] (a) preparing a low-temperature fast-firing blank formulation process slurry using a low-temperature fast-firing blank formulation process;
[0078] (b) The low-temperature fast-firing blank formulation process slurry obtained in step (a) is powder-sprayed and granulated, pressed and formed, and sintered to obtain a finished product having the low-temperature fast-firing blank formulation process.
[0079] Preferably, in parts by weight, the raw materials of the low-temperature fast-sintering blank formulation process slurry in step (a) include: 18-22 parts of kaolin,
[0080] Bentonite: 2-4 parts,
[0081] Potassium-sodium feldspar: 12-18 parts,
[0082] Potassium feldspar: 45-55 parts,
[0083] 4-6 parts of talc,
[0084] Bauxite: 5-10 parts, liquid dissolving agent 0.5-1 part.
[0085] Among the constituent raw materials of the low-temperature fast-firing blank formula process slurry described in the present invention, the weight proportion of kaolin in the low-temperature fast-firing blank formula process is, for example, 18-22 parts, for example, it can be 18 parts, 19 parts, 20 parts, 21 parts, 21.5 parts or 22 parts, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0086] In the low-temperature fast-firing blank formulation process provided by the present invention, bentonite: 2-4 parts, for example, it can be 2 parts, 2.5 parts, 3 parts, 3.5 parts, 4 parts, but is not limited to the listed values. Other unlisted values within the numerical range are also applicable, preferably 2-3 parts.
[0087] In the low-temperature fast-firing billet formulation process provided by the present invention, potassium-sodium feldspar: 12-18 parts, for example, it can be 12 parts, 13 parts, 14 parts, 15 parts, 16 parts, 17 parts or 18 parts, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable, preferably 14-17 parts.
[0088] In the low-temperature fast-firing billet formulation process provided by the present invention, potassium feldspar: 45-55 parts, for example, it can be 45 parts, 46 parts, 47 parts, 48 parts, 49 parts, 50 parts or 51 parts, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable, preferably 46-50 parts.
[0089] In the low-temperature fast-firing blank formulation process provided by the present invention, talc is 4-6 parts, for example, it can be 4 parts, 4.5 parts, 5 parts, 5.5 parts or 6 parts, but is not limited to the listed values. Other unlisted values within the numerical range are also applicable, preferably 4-5 parts.
[0090] In the low-temperature fast-firing billet formulation process provided by the present invention, bauxite: 5-10 parts, for example, it can be 5 parts, 6 parts, 7 parts, 8 parts, 9 parts, 9.5 parts or 10 parts, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable, preferably 8-10 parts.
[0091] In the low-temperature fast-firing billet formulation process provided by the present invention, the liquid disintegrator is 0.5-1 part, for example, it can be 0.5 part, 0.6 part, 0.7 part, 0.8 part, 0.9 part, 0.95 part or 1 part, but is not limited to the listed values. Other values not listed within the numerical range are also applicable, preferably 0.5-0.7 part.
[0092] Preferably, the total weight proportion of the bentonite and talc is 7-8 parts, for example, it can be 7 parts, 7.1 parts, 7.2 parts, 7.3 parts, 7.4 parts, 7.5 parts, 7.6 parts, 7.7 parts, 7.8 parts, 7.9 parts or 8 parts, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0093] Preferably, the added fixed component of talc and bauxite is 12 parts, which can be considered to be used interchangeably, but are not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0094] Preferably, the added fixed component of kaolin and bentonite is 24 parts, which can be considered to be used interchangeably, but are not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0095] The sintering in step (b) comprises the following steps:
[0096] (i) Heating the temperature to 400-500°C at a rate of 8-10°C / min and keeping the temperature for 5-10 min;
[0097] (ii) heating to 800-900°C at a heating rate of 6-8°C / min and keeping at that temperature for 15-25 min;
[0098] (iii) heating the temperature to 1150-1250°C at a rate of 4-6°C / min and maintaining the temperature for 10-20 min;
[0099] (iv) Rapid cooling to room temperature to complete sintering.
[0100] During the sintering process, the holding time of step (ii) is 5-10 min, for example, 5 min, 6 min, 7 min, 8 min, 9 min or 10 min, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0101] During the sintering process, the heating rate of step (iii) is 4-6°C / min, for example, it can be 4°C / min, 4.5°C / min, 5°C / min, 5.5°C / min or 6°C / min, but is not limited to the listed values, and values not listed within the numerical range are also applicable.
[0102] During the sintering process, the heating temperature of step (iii) is 1150-1250°C, for example, it can be 1150°C, 1160°C, 1170°C, 1180°C, 1190°C, 1200°C, 1210°C, 1220°C, 1230°C, 1240°C or 1250°C, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0103] During the sintering process, the holding time of step (iii) is 20-60 min, for example, 20 min, 30 min, 40 min, 45 min, 500 min, 55 min or 60 min, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0104] The application comprises the following steps:
[0105] (a) Using volcanic rock effect glaze to prepare low-temperature fast-firing blank formula process slurry;
[0106] (b) powder spraying and granulating the low-temperature fast-firing blank formulation process slurry obtained in step (a), pressing and molding, and sintering to obtain a finished product having the low-temperature fast-firing blank formulation process;
[0107] In terms of weight, the raw materials of the low-temperature fast-sintering green body formulation process slurry in step (a) include: 18-22 parts of kaolin,
[0108] Bentonite: 2-4 parts,
[0109] Potassium-sodium feldspar: 12-18 parts,
[0110] Potassium feldspar: 45-55 parts,
[0111] 4-6 parts of talc,
[0112] Bauxite: 5-10 parts,
[0113] 0.5-1 part of liquid dissolving agent;
[0114] The sintering in step (b) comprises the following steps:
[0115] (i) heating the temperature to 400-500°C at a heating rate of 8-10°C / min and keeping the temperature for 10-40 min;
[0116] (ii) heating to 800-900°C at a heating rate of 6-8°C / min and keeping at that temperature for 10-40 min;
[0117] (iii) heating the temperature to 1150-1250°C at a heating rate of 4-6°C / min and maintaining the temperature for 20-60 min;
[0118] (iv) The temperature is naturally lowered to room temperature to complete sintering.
[0119] During the sintering process, the holding time of step (ii) is 5-10 min, for example, 5 min, 6 min, 7 min, 8 min, 9 min or 10 min, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0120] During the sintering process, the heating rate of step (iii) is 4-6°C / min, for example, it can be 4°C / min, 4.5°C / min, 5°C / min, 5.5°C / min or 6°C / min, but is not limited to the listed values, and values not listed within the numerical range are also applicable.
[0121] During the sintering process, the heating temperature of step (iii) is 1150-1250°C, for example, it can be 1150°C, 1160°C, 1170°C, 1180°C, 1190°C, 1200°C, 1210°C, 1220°C, 1230°C, 1240°C or 1250°C, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0122] During the sintering process, the holding time of step (iii) is 20-60 min, for example, 20 min, 30 min, 40 min, 45 min, 500 min, 55 min or 60 min, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0123] Example 1
[0124] (1) mixing by wet ball milling according to the formula, wherein the raw materials are immersed in water during the wet ball milling, and a mixed material with an average particle size of 68 μm is obtained;
[0125] (2) dividing the mixed material obtained in step (1) into a first powder and a second powder, wherein the mass ratio of the first powder to the second powder is 2:1; and wet-milling the first powder and the second powder respectively, wherein the raw materials are immersed in water during the wet-milling; the average particle size of the first ball-milled material obtained by ball-milling the first powder is 60 μm; and the average particle size of the second ball-milled material obtained by ball-milling the second powder is 80 μm;
[0126] (3) The first ball mill obtained in step (2) is uniformly mixed with the second ball mill to achieve the preparation of the low-temperature fast-sintering blank formulation process.
[0127] In terms of weight, the raw materials used in the low-temperature fast-firing blank formulation process described in this embodiment include: 18 parts of kaolin,
[0128] Bentonite: 2 parts,
[0129] Potassium-sodium feldspar: 12 parts,
[0130] Potassium feldspar: 45 parts,
[0131] 4 parts of talc,
[0132] Bauxite: 5 parts, liquid dissolving agent 0.5 parts.
[0133] Example 2
[0134] (1) wet-milling the mixed raw materials according to the formula, wherein the raw materials are submerged in water during the wet-milling process, to obtain a mixed material with an average particle size of 65 μm;
[0135] (2) dividing the mixed material obtained in step (1) into a first powder and a second powder, wherein the mass ratio of the first powder to the second powder is 3:1; and wet-milling the first powder and the second powder respectively, wherein the raw materials are immersed in water during the wet-milling; the average particle size of the first ball-milled material obtained by ball-milling the first powder is 60 μm; and the average particle size of the second ball-milled material obtained by ball-milling the second powder is 80 μm;
[0136] (3) The first ball mill obtained in step (2) is uniformly mixed with the second ball mill to prepare the low-temperature fast-sintering blank formula process slurry.
[0137] In terms of weight, the raw materials used in the low-temperature fast-firing blank formulation process described in this embodiment include: 20 parts of kaolin,
[0138] Bentonite: 3 parts,
[0139] Potassium-sodium feldspar: 14 parts,
[0140] Potassium feldspar: 50 parts,
[0141] 5 parts of talc,
[0142] Bauxite: 8 parts, liquid dissolving agent 0.8 parts.
[0143] Example 3
[0144] (1) wet-milling the mixed raw materials according to the formula, wherein the raw materials are immersed in water during the wet-milling process to obtain a mixed material with an average particle size of 100 μm;
[0145] (2) dividing the mixed material obtained in step (1) into a first powder and a second powder, wherein the mass ratio of the first powder to the second powder is 1:1; and wet-milling the first powder and the second powder respectively, wherein the raw materials are immersed in water during the wet-milling; the average particle size of the first ball-milled material obtained by ball-milling the first powder is 90 μm; and the average particle size of the second ball-milled material obtained by ball-milling the second powder is 110 μm;
[0146] (3) The first ball mill obtained in step (2) is uniformly mixed with the second ball mill to prepare the low-temperature fast-sintering blank formula process slurry.
[0147] In terms of weight, the raw materials used in the low-temperature fast-firing blank formulation process described in this embodiment include: 20 parts of kaolin,
[0148] Bentonite: 3.5 parts,
[0149] Potassium-sodium feldspar: 15 parts,
[0150] Potassium feldspar: 50 parts,
[0151] 5 parts of talc
[0152] Bauxite: 8 parts, liquid dissolving agent 0.8 parts.
[0153] Example 4
[0154] In addition to the low-temperature fast-sintering blank, the raw materials include: kaolin: 20 parts,
[0155] Bentonite: 4 parts,
[0156] Potassium-sodium feldspar: 15 parts,
[0157] Potassium feldspar: 50 parts,
[0158] 5 parts of talc,
[0159] Bauxite: 8 parts,
[0160] 1 part of liquid dissolving agent.
[0161] Example 5
[0162] In addition to the low-temperature fast-sintering blank, the raw materials include: kaolin: 18 parts,
[0163] Bentonite: 2 parts,
[0164] Potassium-sodium feldspar: 12 parts,
[0165] Potassium feldspar: 55 parts,
[0166] 6 parts of talc,
[0167] Bauxite: 10 parts,
[0168] 1 part of liquid dissolving agent.
[0169] Example 6
[0170] The raw materials of the low temperature fast burning blank include: kaolin: 19 parts, bentonite: 2 parts,
[0171] Potassium-sodium feldspar: 12 parts, potassium feldspar: 45 parts,
[0172] 4 parts of talc,
[0173] Bauxite: 5 parts,
[0174] 1 part of liquid dissolving agent.
[0175] Example 7
[0176] In addition to the raw materials of the low-temperature fast-sintering blank, which include: 20 parts of kaolin and 2 parts of bentonite,
[0177] Potassium-sodium feldspar: 12 parts, potassium feldspar: 45 parts,
[0178] 4 parts of talc,
[0179] Bauxite: 5 parts,
[0180] 1 part of liquid dissolving agent.
[0181] Example 8
[0182] In addition to the raw materials of the low-temperature fast-sintering blank, which include: 21 parts of kaolin and 2-4 parts of bentonite,
[0183] Potassium-sodium feldspar: 12-18 parts,
[0184] Potassium feldspar: 45-55 parts,
[0185] 4-6 parts of talc,
[0186] Except for bauxite: 5-10 parts, liquid dissolving agent: 0.5-1 parts, the rest are the same as in Example 1.
[0187] Example 9
[0188] In addition to the raw materials of the low-temperature fast-firing blank formulation process, which include: kaolin: 22 parts, bentonite: 2 parts,
[0189] Potassium-sodium feldspar: 12 parts,
[0190] Potassium feldspar: 45 parts,
[0191] 4 parts of talc
[0192] Bauxite: 5 parts
[0193] 1 part of liquid dissolving agent.
[0194] Comparative Example 1
[0195] This comparative example is the same as Example 1 except that talc is replaced with an equal amount of bauxite in Example 1.
[0196] Comparative Example 2
[0197] In this comparative example, in addition to the low-temperature fast-sintering blank formulation process, the raw materials include: 18 parts of kaolin, 2 parts of bentonite,
[0198] Potassium-sodium feldspar: 12 parts,
[0199] Potassium feldspar: 45 parts,
[0200] 4 parts of talc,
[0201] Bauxite: 8 parts, liquid dissolving agent 0.5 parts.
[0202] Comparative Example 3
[0203] In this comparative example, the glaze material includes: 20 parts of kaolin,
[0204] Bentonite: 3 parts,
[0205] Potassium-sodium feldspar: 16 parts,
[0206] Potassium feldspar: 50 parts,
[0207] 5 parts of talc,
[0208] Bauxite: 7 parts, liquid dissolving agent 0.5 parts.
[0209] Comparative Example 4
[0210] In this comparative example, in addition to the low-temperature fast-sintering green body formulation process, the raw materials include: 20 parts of kaolin, 3 parts of bentonite,
[0211] Potassium-sodium feldspar: 16 parts,
[0212] Potassium feldspar: 50 parts,
[0213] 6 parts of talc,
[0214] Bauxite: 6 parts, liquid dissolving agent 0.5 parts.
[0215] Comparative Example 5
[0216] In this comparative example, in addition to the low-temperature fast-sintering green body formulation process, the raw materials include: 20 parts of kaolin and 3 parts of bentonite.
[0217] Potassium-sodium feldspar: 16 parts,
[0218] Potassium feldspar: 50 parts,
[0219] 4.5 parts of talc, 7.5 parts of bauxite, and 0.5 parts of liquid dissolving agent.
[0220] Comparative Example 6
[0221] This comparative example provides a preparation method of a blank formulation process, and the preparation method comprises the following steps: (1) wet-milling the mixed raw materials according to the formula, wherein the raw materials are immersed in water during the wet-milling, to obtain a mixed material with an average particle size of 90 μm;
[0222] (2) The mixed material obtained in step (1) is subjected to wet ball milling, wherein the raw material is immersed in water during the wet ball milling; the average particle size of the obtained ball milled material is 90 μm, thereby realizing the preparation of the low-temperature fast-sintering blank formulation process.
[0223] In parts by weight, the raw materials of the glaze in this comparative example include 22 parts of kaolin and 4 parts of bentonite.
[0224] Potassium-sodium feldspar: 18 parts,
[0225] Potassium feldspar: 55 parts,
[0226] 5.5 parts of talc,
[0227] Bauxite: 6.5 parts, liquid dissolving agent: 1 part.
[0228] Comparative Example 7
[0229] This comparative example provides a preparation method of a low-temperature fast-sintering blank formulation process, and the preparation method comprises the following steps:
[0230] (1) wet-milling the mixed raw materials according to the formula, wherein the raw materials are immersed in water during the wet-milling, to obtain a mixed material with an average particle size of 90 μm;
[0231] (2) The mixed material obtained in step (1) is subjected to wet ball milling, wherein the raw material is immersed in water during the wet ball milling; the average particle size of the obtained ball milled material is 60 μm, thereby realizing the preparation of the process slurry of the low-temperature fast-sintering blank formula.
[0232] In parts by weight, the raw materials of the low-temperature fast-sintering blank formulation process described in this comparative example include: kaolin: 20 parts,
[0233] Bentonite: 4 parts,
[0234] Potassium-sodium feldspar: 18 parts,
[0235] Potassium feldspar: 55 parts,
[0236] 5.9 parts of talc,
[0237] Bauxite: 6.1 parts, liquid dissolving agent: 1 part.
[0238] Application Example 1
[0239] This application example provides an application of the low-temperature fast-firing blank described in Example 1, and the application example includes the following steps: (a) preparing a low-temperature fast-firing blank formulation process slurry using a low-temperature fast-firing blank formulation process;
[0240] (b) powder spraying and granulating the low-temperature fast-firing blank formulation process slurry obtained in step (a), forming, and sintering to obtain a finished product having the low-temperature fast-firing blank formulation process;
[0241] In parts by weight, the raw materials of the slurry of the formulation process in step (a) include: low-temperature fast-sintering green body formulation process; kaolin: 22 parts,
[0242] Bentonite: 4 parts,
[0243] Potassium-sodium feldspar: 18 parts,
[0244] Potassium feldspar: 54 parts
[0245] 6 parts of talc,
[0246] Bauxite: 10 parts,
[0247] 1 part of liquid dissolving agent.
[0248] The sintering in step (b) comprises the following steps:
[0249] (i) Heating the temperature to 450°C at a rate of 9°C / min and keeping the temperature for 10 min;
[0250] (ii) heating to 850 °C at a rate of 7 °C / min and holding for 10 min; (iii) heating at a rate of 5°C / min to 1200°C and maintaining for 20 min;
[0251] (iv) The temperature is naturally lowered to room temperature to complete sintering.
[0252] Application Example 2
[0253] This application example provides an application of the low-temperature fast-sintering blank described in Example 1, and the application includes the following steps:
[0254] (a) preparing a low-temperature fast-firing blank formulation process slurry using a low-temperature fast-firing blank formulation process;
[0255] (b) powder spraying and granulating the low-temperature fast-firing blank formulation process slurry obtained in step (a), forming, and sintering to obtain a finished product having the low-temperature fast-firing blank formulation process;
[0256] In parts by weight, the raw materials of the low-temperature fast-sintering blank formulation process slurry in step (a) include: 22 parts of kaolin,
[0257] Bentonite: 3 parts,
[0258] Potassium-sodium feldspar: 18 parts,
[0259] Potassium feldspar: 55 parts,
[0260] 6 parts of talc,
[0261] Bauxite: 10 parts,
[0262] 1 part of liquid dissolving agent;
[0263] The sintering in step (b) comprises the following steps:
[0264] (i) Heating the temperature to 400 °C at a rate of 8 °C / min and keeping the temperature for 10 min;
[0265] (ii) heating to 800 °C at a rate of 6 °C / min and holding for 10 min;
[0266] (iii) heating the temperature to 1150°C at a rate of 4°C / min and maintaining the temperature for 20 min;
[0267] (iv) The temperature is naturally lowered to room temperature to complete sintering.
[0268] Application Example 3
[0269] This application example provides an application of the low-temperature fast-sintering blank described in Example 1, and the application includes the following steps:
[0270] (a) preparing a low-temperature fast-firing blank formulation process slurry using a low-temperature fast-firing blank formulation process;
[0271] (b) powder spraying and granulating the low-temperature fast-firing blank formulation process slurry obtained in step (a), and forming and sintering to obtain a finished product having the low-temperature fast-firing blank formulation process;
[0272] In parts by weight, the raw materials of the low-temperature fast-sintering blank formulation process slurry in step (a) include: 22 parts of kaolin,
[0273] Bentonite: 4 parts,
[0274] Potassium-sodium feldspar: 18 parts,
[0275] Potassium feldspar: 55 parts,
[0276] 6 parts of talc,
[0277] Bauxite: 9 parts,
[0278] 1 part of liquid dissolving agent;
[0279] The sintering in step (b) comprises the following steps:
[0280] (i) Heating the temperature to 500°C at a rate of 10°C / min and keeping the temperature for 10 min;
[0281] (ii) heating to 900 °C at a rate of 8 °C / min and holding for 10 min;
[0282] (iii) heating the temperature to 1250°C at a rate of 6°C / min and maintaining the temperature for 20 min;
[0283] (iv) The temperature is naturally lowered to room temperature to complete sintering.
[0284] Application Example 4
[0285] This application example provides an application of the low-temperature fast-sintering blank described in Example 1, and the application includes the following steps:
[0286] (a) preparing a low-temperature fast-firing blank formulation process slurry using a low-temperature fast-firing blank formulation process;
[0287] (b) powder spraying and granulating the low-temperature fast-firing blank formulation process slurry obtained in step (a), and forming and sintering to obtain a finished product having the low-temperature fast-firing blank formulation process;
[0288] In parts by weight, the raw materials of the low-temperature fast-sintering blank formulation process slurry in step (a) include:
[0289] Kaolin: 22 parts,
[0290] Bentonite: 4 parts,
[0291] Potassium-sodium feldspar: 18 parts,
[0292] Potassium feldspar: 55 parts,
[0293] 6 parts of talc,
[0294] Bauxite: 10 parts,
[0295] 0.5 parts of liquid dissolving agent;
[0296] The sintering in step (b) comprises the following steps:
[0297] (i) Heating the temperature to 450°C at a rate of 9°C / min and keeping the temperature for 10 min;
[0298] (ii) heating the sample to 850 °C at a rate of 7 °C / min and maintaining the temperature for 15 min;
[0299] (iii) heating to 1200°C at a rate of 5°C / min and holding for 20 min;
[0300] (iv) The temperature is naturally lowered to room temperature to complete sintering.
[0301] Application Example 5
[0302] This application example provides an application of the low-temperature fast-sintering blank described in Example 1, and the application includes the following steps:
[0303] (a) preparing a low-temperature fast-firing blank formulation process slurry using a low-temperature fast-firing blank formulation process;
[0304] (b) The low-temperature fast-firing blank formulation process slurry obtained in step (a) is powder-sprayed and granulated, and after forming and sintering, a finished product having the low-temperature fast-firing blank formulation process is obtained.
[0305] In parts by weight, the raw materials of the low-temperature fast-sintering blank formulation process slurry in step (a) include: 18 parts of kaolin,
[0306] Bentonite: 2 parts,
[0307] Potassium-sodium feldspar: 12 parts,
[0308] Potassium feldspar: 45 parts,
[0309] 4 parts of talc,
[0310] Bauxite: 5 parts,
[0311] 0.7 parts of liquid dissolving agent;
[0312] The sintering in step (b) comprises the following steps:
[0313] (i) Heating the temperature to 450°C at a rate of 9°C / min and keeping the temperature for 10 min;
[0314] (ii) heating the sample to 850 °C at a rate of 7 °C / min and maintaining the temperature for 15 min;
[0315] (iii) heating to 1200°C at a rate of 5°C / min and holding for 20 min;
[0316] (iv) The temperature is naturally lowered to room temperature to complete sintering.
[0317] The flatness, light transmittance and wear resistance of the low-temperature fast-firing blank formulation process obtained in Examples 1-8 and Comparative Application Examples 1-5 were tested, wherein the flatness was tested using a gloss meter, and the light transmittance was tested using a transmittance meter; the wear resistance was measured in accordance with the method specified in GB 11950-89. In summary, the present invention adjusts the components of the low-temperature fast-firing blank formulation process so that the low-temperature fast-firing blank formulation process prepared when used for porcelain glazed tiles has porcelain glazed tiles that meet the national 3C performance, and has higher transparency, high temperature resistance and wear resistance;
[0318] The application method of the low-temperature fast-firing blank formulation process of the present invention is simple, and the preparation of porcelain glazed tiles can be achieved by only adjusting the sintering rate. The prepared porcelain glazed tiles meet the national 3C standards and have the effects of increasing production, improving quality, improving efficiency and reducing costs.
[0319] The present invention is not limited to what is described in the specification and implementation modes, and therefore additional advantages and modifications can be easily realized by those skilled in the art. Therefore, without departing from the spirit and scope of the general concept defined by the claims and the equivalent scope, the present invention is not limited to the specific details, representative devices, and examples shown and described herein.
Claims
1. A low-temperature fast-sintering blank, which comprises, by weight: Kaolin: 18-22 parts, Bentonite: 2-4 parts, Potassium-sodium feldspar: 12-18 parts, Potassium feldspar: 45-55 parts, 4-6 parts of talc, Bauxite: 5-10 parts, Liquid dissolving agent 0.5-1 part.
2. A method for preparing a low-temperature fast-sintering blank as claimed in claim 1, characterized in that: The steps include: S1: Mixing according to the formula amount of the blank to obtain a mixed material; S2: dividing the mixed material obtained in step S1 into two powders, and ball-milling the two powders respectively to obtain two ball-milled materials with different average particle sizes; S3: The two portions of ball mill materials obtained in step S2 are uniformly mixed to prepare the low-temperature fast-sintering blank.
3. The method for preparing a low-temperature fast-sintering blank according to claim 2, characterized in that: The mixing in step S1 is wet ball milling mixing, and water is used to immerse the raw materials during wet ball milling mixing.
4. The method for preparing a low-temperature fast-sintering blank according to claim 2, characterized in that: The average particle size of the mixture in step S1 is 60-180 μm.
5. The method for preparing a low-temperature fast-sintering blank according to claim 2, characterized in that: The mixed material obtained in step S1 is divided into a first powder material and a second powder material, and the mass ratio of the first powder material to the second powder material is 1-3:
1.
6. The method for preparing a low-temperature fast-sintering blank according to claim 2, characterized in that: The average particle size of the first ball mill obtained by ball milling the first powder is 70-170 μm, and the average particle size of the second ball mill obtained by ball milling the second powder is 50-120 μm.
7. An application of the low temperature fast sintering blank as claimed in claim 1, characterized in that: The application comprises the following steps: (a) preparing a low-temperature fast-firing blank formulation process slurry using a low-temperature fast-firing blank formulation process; (b) The low-temperature fast-firing blank formulation process slurry obtained in step (a) is powder-sprayed and granulated, pressed and formed, and sintered to obtain a finished product having the low-temperature fast-firing blank formulation process.
8. An application of the low temperature fast sintering blank as claimed in claim 7, characterized in that: In parts by weight, the raw materials of the low-temperature fast-sintering blank formulation process slurry in step (a) include: 18-22 parts of kaolin, Bentonite: 2-4 parts, Potassium-sodium feldspar: 12-18 parts, Potassium feldspar: 45-55 parts, 4-6 parts of talc, Bauxite: 5-10 parts, 0.5-1 part of liquid dissolving agent.
9. An application of the low temperature fast sintering blank as claimed in claim 7, characterized in that: The sintering in step (b) comprises the following steps: (i) Heating the temperature to 400-500°C at a rate of 8-10°C / min and keeping the temperature for 5-10 min; (ii) heating to 800-900°C at a heating rate of 6-8°C / min and keeping at that temperature for 15-25 min; (iii) heating the temperature to 1150-1250°C at a rate of 4-6°C / min and maintaining the temperature for 10-20 min; (iv) Rapid cooling to room temperature to complete sintering.
Citation Information
Patent Citations
High-whiteness glazed tile and preparation method thereof
CN111439988A
Volcanic drift rock glaze as well as preparation method and application thereof
CN112939460A
Low-energy-consumption fast-firing green body, ceramic tile and preparation method of low-energy-consumption fast-firing green body
CN115745586A
Lightweight ceramics
EP4361118A1
Composition for low-temperature firing porcelain and method for manufacturing low-temperature firing porcelain
JP2011184245A