Composite heat insulation plate for high-temperature kiln and preparation method of composite heat insulation plate

Porous foam plates are prepared by using high-purity magnesium sand, zirconium oxide, MnAl2O4 and snail shell powder to prepare columnar support and microbial foaming agent in thermal insulation materials for high-temperature kilns. The existing materials are solved by combining laser melting and chemical etching technology. The problems of low strength and poor high temperature resistance have achieved efficient compression and thermal insulation performance.

CN118978393AActive Publication Date: 2024-11-19ZIBO CITY LUZHONG REFRACTORIES CO LTD +2

Patent Information

Application Number
CN202411463867.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-21
Publication Date
2024-11-19
Estimated Expiration
2044-10-21

AI Technical Summary

Technical Problem

The existing thermal insulation materials for high-temperature kilns have low strength, are easy to compress and powder, and have poor high-temperature resistance, resulting in a decrease in thermal insulation performance and poses safety hazards.

Method used

The columnar support is prepared by high-purity magnesium sand, zirconium oxide, MnAl2O4 and snail shell powder, combined with laser melting technology and silicon boron modified polyamide epoxychlorohydrin resin as the binder, and the composite heat insulation board is prepared, and a microbial foaming agent is used. and chemical etching technology to prepare porous foam plates to increase compression resistance and thermal insulation properties.

Benefits of technology

It significantly improves the compressive and thermal insulation performance of the composite heat insulation plate, ensures that the insulation performance does not decrease under high temperature conditions, reduces thermal energy dissipation, and enhances the overall strength and stability of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118978393A_ABST
    Figure CN118978393A_ABST
Patent Text Reader

Abstract

The invention provides a composite thermal insulation board for a high-temperature kiln and a preparation method thereof, and belongs to the technical field of refractory materials, and the preparation method comprises the following steps: uniformly mixing a mixture containing zirconium oxide, MnAl2O4 and snail shell powder with sulfite waste liquid, solidifying into layers, stacking layer by layer, adding silicon-boron modified polyamide epichlorohydrin resin between layers, sintering at high temperature, and demolding to obtain the composite thermal insulation board for the high-temperature kiln. A columnar supporting body is prepared; preparing a microbial foaming agent for later use; the preparation method comprises the following steps: uniformly mixing modified aluminum silicate active powder, other auxiliaries and a microbial foaming agent, pouring into a mold, curing to obtain a modified aluminum silicate porous foam board, spraying a hydrochloric acid solution on the surface, drying, pouring a mixed solution of nano silicon dioxide and ethanol, carrying out heat treatment, spraying fluorosilicone modified polyester resin, drying and curing to obtain the composite heat insulation board. According to the invention, the heat insulation and compression resistance can be improved, and the heat-resistant thermal-insulation board of the high-temperature kiln can be integrally formed.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of refractory materials, and in particular to a composite heat-insulating board for a high-temperature kiln and a preparation method thereof. Background Art

[0002] Traditional thermal insulation materials, such as aluminum silicate fiberboard, fiber wool, lightweight castables, insulation bricks and other thermal insulation materials, have low strength, are easily compressed and crushed, and the compression ratio is generally large, which will cause the integrity of the high-temperature lining structure including the thermal insulation materials to be destroyed or deteriorated, the thermal insulation performance is reduced, and even accidents such as steel leakage from the ladle may occur. In addition, thermal insulation materials such as aluminum silicate fiber, aerogel, and nano insulation board have poor high temperature resistance and are prone to crystallization during high-temperature use; after the thermal insulation material crystallizes, if there is no large external force, the thermal insulation material can barely maintain the original porous structure, maintain the original thermal insulation performance or reduce the thermal insulation performance to a certain extent. If the thermal insulation material encounters expansion pressure such as the working lining after crystallization, the use thickness of the thermal insulation material will be sharply reduced, or even powdered, the original thermal insulation material structure will deteriorate, the overall structural property of the refractory lining structure will decrease, and the thermal insulation performance will also decrease.

[0003] Aluminum silicate refractory fiber is the fastest growing and most widely used refractory fiber in high-temperature industrial furnaces. It has the advantages of high-temperature thermal insulation, heat preservation, fire resistance, noise reduction, insulation and light weight. Its maximum operating temperature is 1260℃ and its long-term operating temperature is 950~1050℃. However, it has poor compressive and flexural strength, is prone to dust, has poor waterproof performance, has a high water absorption rate, and has the microstructure characteristics of interconnected pores, which leads to unsatisfactory thermal insulation performance under high temperature conditions.

[0004] Preparation of lightweight high-temperature thermal insulation materials of aluminum silicate for industrial furnaces [J] Metal Heat Treatment 2019 No. 04, with 200g of high-alumina refractory cement, 60g of silica powder, 100mL of water, and a water-cement ratio of 0.5, sintered at 1180℃ to prepare a bulk density of 268kg / m 3 The thermal insulation material has a thermal conductivity of 0.06W / (m·K) at 1000℃ and a compressive strength of 4.2MPa. Although this type of material has good thermal insulation, it has low strength and is prone to breakage and powdering during use, which not only greatly reduces the thermal insulation performance but also affects the structure and safety of the entire refractory lining.

[0005] Therefore, it is necessary to provide a composite heat insulation board for a high-temperature kiln and a preparation method thereof to solve the problems existing in the above-mentioned prior art. Summary of the invention

[0006] In view of this, the present invention provides a composite thermal insulation board for a high-temperature kiln and a preparation method thereof, which can improve the thermal insulation and pressure resistance performance while realizing the integrated molding of the heat-resistant thermal insulation board for the high-temperature kiln.

[0007] To achieve the above object, the present invention provides a method for preparing a composite heat insulation board for a high temperature kiln, comprising the following steps: S1. Mix a mixture of high-purity magnesia, zirconium oxide, MnAl2O4 and snail shell powder with sulfite waste liquid; spread it evenly in a columnar mold, and solidify it into layers after laser melting; repeat the above steps, stacking layer by layer, adding silicon boron modified polyamide epichlorohydrin resin between layers, sintering at high temperature, cooling, solidifying, and demolding to obtain a columnar support body; S2, after incubating the acetic acid bacteria solution, adding sodium bicarbonate solution, stirring, and preparing a microbial foaming agent for use; S3, mixing the modified aluminum silicate active powder, other additives and microbial foaming agent evenly, pouring them into a square mold, stirring, vertically placing the prepared columnar support, sealing and wrapping, and standing to solidify to obtain a modified aluminum silicate porous foam board; S4. Spray hydrochloric acid solution on the surface of the prepared modified aluminum silicate porous foam board, dry it, pour a mixed solution of nano-silicon dioxide and ethanol, spray fluorine silicon modified polyester resin after heat treatment, dry and solidify it, and obtain a composite insulation board.

[0008] The present invention prepares a columnar support column by adding zirconium oxide, MnAl2O4 and snail shell powder to high-purity magnesia, thereby increasing the compressive strength of the columnar support body and improving the thermal insulation performance; wherein the snail shell powder is rich in calcium carbonate and has a porous structure, which can reduce the density of the material, thereby having good lightness and thermal insulation performance; at the same time, its decomposition reaction at high temperature can form gas, further increasing the porosity of the material and enhancing the thermal insulation effect; in addition, zirconium oxide and MnAl2O4 have excellent high-temperature strength and toughness, and their addition can improve the compressive strength of the support column; in addition, at high temperatures, due to the Mn 2+ and Mg 2+ The mutual diffusion of Mg-Mn-Al composite spinel is formed in the material, which promotes adhesion and increases the strength of the material, thereby improving the mechanical properties of the overall support column and further enhancing the compressive resistance.

[0009] The present invention introduces a columnar support body, which can ensure that the thermal insulation material in the composite structure is not compressed, thereby ensuring that its thermal insulation performance is not reduced or is reduced very little; by adopting laser melting technology instead of the traditional powder pressing method, a more dense high-strength columnar support body is formed; after laser melting, the composite material is made into a slurry structure and then further re-solidified into a solid, which makes the connection between the composite materials tighter and forms a dense layer. In addition, the stacking between layers creates multiple stress transfer paths, which helps to relieve local stress concentration and evenly distribute pressure, thereby improving the overall compressive resistance; and silicon boron modified polyamide epichlorohydrin resin is used as an interlayer adhesive. After silicon boron modification, the polyamide epichlorohydrin resin is endowed with high temperature resistance and high mechanical strength, and the elasticity of the adhesive provides a buffering effect, which further improves the overall compressive resistance of the columnar support body, thereby preventing the composite insulation board from being compressed.

[0010] The present invention uses a microbial foaming agent to prepare a porous foam board as a base material for a kiln heat-resistant thermal insulation board, and uses a chemical etching technology to directly perform waterproof and heat-insulating treatment on the surface to achieve the preparation of an integrally formed kiln heat-resistant thermal insulation board, thereby minimizing the heat energy dissipation of a joint; the microbial foaming is prepared by using acetobacillus as a raw material and a sodium bicarbonate solution as a foaming stabilizer; carbon dioxide is generated by the metabolism of acetobacillus and the decomposition of the sodium bicarbonate solution to form bubbles, and the carbon dioxide gas can react with water to generate carbonic acid, which is a weak acid and can reduce the surface tension of the solution. The lower surface tension is conducive to the formation and stability of bubbles, and at the same time provides a suitable fermentation environment for acetobacillus, which is more conducive to the generation of carbon dioxide; since microbial foaming is used in the preparation process, The material foaming agent is mixed with the raw materials and left to solidify statically, which makes the carbon dioxide dispersed in the unsolidified raw materials form closed pores after solidification, which reduces water absorption and heat loss. Furthermore, micro-texture is constructed on the foam surface through chemical etching technology, and nano-silicon dioxide is sprayed to form a micron-nano dual-scale rough structure, which can effectively hinder heat conduction. The reduced thermal conductivity helps to maintain the internal temperature, thereby improving the thermal insulation performance. The fluorine groups in the fluorosilicone modified polyester resin not only reduce the surface energy, but also give the material excellent high temperature resistance, and act as a binder during the high-temperature curing process to ensure that the silica particles are firmly bonded, enhance the overall strength of the material, and improve its stability and thermal insulation effect under high-temperature applications.

[0011] Optionally, in step S1, the boron-silicon modified polyamide epichlorohydrin resin is prepared by uniformly mixing organosilicon, B(OH)3 and sodium alginate in deionized water, adding calcium hydroxide solution and heating to 100-150°C, stirring for 1-2 hours, and then adding polyamide epichlorohydrin resin and ultrasonically dispersing for 10-30 minutes; wherein the mass ratio of organosilicon, B(OH)3 and sodium alginate is 2.5:1:1, the volume ratio of deionized water, calcium hydroxide solution and polyamide epichlorohydrin resin is 6:1:6, and the concentration of calcium hydroxide solution is 3%-5%.

[0012] In the process of modifying the polyamide epichlorohydrin resin, the high temperature resistance of the material is improved by introducing organic silicon. In addition, sodium alginate can form a viscous solution in water, promote the formation of a cross-linked structure, and further increase the adhesion and flexibility of the modified material. B(OH)3 provides hydroxide ions in water, and its structure can interact with other components to enhance the overall stability and mechanical strength. Organic silicon reacts with calcium hydroxide and hydroxyl groups in sodium alginate to form a three-dimensional network structure, so that the system is transformed from a liquid state to a gel state. Finally, after the polyamide epichlorohydrin resin is added to the gel, ultrasonic dispersion can be performed to effectively destroy large particles and promote their uniform distribution in the gel, which not only improves the coverage of the resin, but also enhances the mechanical properties and stability of the final material.

[0013] Optionally, the concentration of sulfite waste liquid in step S1 is 5%; the diameter of the columnar mold in step S1 is 10-30 mm; the thickness of each layer in step S1 is 1-6 mm; the mixing time in step S1 is 30-60 min; the high-temperature sintering temperature in step S1 is 1500-1600° C., and the time is 2-4 h; and the curing time in step S1 is 5-10 h.

[0014] Optionally, in step S2, a 10% Acetobacter solution is incubated at 170 r / min in a shaker at 35° C. for 48 hours, and then a 3% sodium bicarbonate solution is added and stirred at 3000 r / min for 20 to 50 minutes to obtain a microbial foaming agent.

[0015] Optionally, the modified aluminosilicate active powder in step S3 is prepared by mixing a mixed solution of aluminosilicate active powder, copper powder, phenyltriethoxysilane and anhydrous ethanol, ultrasonically treating the mixture for 20 to 40 minutes, and then drying the mixture at 60 to 100° C. for 1 to 4 hours.

[0016] The present invention uses phenyltriethoxysilane as a coupling agent in the modification process of aluminosilicate, and combines with hydroxyl groups on the surface of aluminum silicate through silanol groups. Phenyl groups as hydrophobic groups improve its hydrophobicity and have good compatibility with organic bodies, thereby improving the bonding force between interfaces and improving the overall mechanical strength. After the hydrophobicity is enhanced, the water absorption rate of the material in a humid environment is reduced, thereby reducing the decline in mechanical properties caused by water absorption. The addition of Cu makes the average pore size smaller and denser at the same expansion rate, thereby improving the compressive strength, thereby further improving the overall hydrophobicity and compressive strength. Optionally, the ratio of the mass fraction of the aluminum silicate active powder and copper powder to the volume fraction of the mixed solution of phenyltriethoxysilane and anhydrous ethanol is 4:1:10; the ratio of the mass fraction of phenyltriethoxysilane to the volume fraction of anhydrous ethanol in the mixed solution of phenyltriethoxysilane and anhydrous ethanol is 0.1:5.

[0017] Optionally, other additives in step S3 include white cement, kaolin, and water reducing agent; the stirring time is 30 to 60 minutes; the static curing time is 22 to 26 hours; the thickness of the modified aluminum silicate porous foam board is 5 to 30 mm; the length of the square mold is 200 to 500 mm and the width is 50 to 300 mm.

[0018] Optionally, in step S4, a hydrochloric acid solution with a concentration of 5% to 10% is evenly sprayed on the surface of the prepared modified aluminum silicate porous foam board with a spray gun, and after drying at 100°C for 2 to 5 hours, a mixed solution of nano-silicon dioxide and ethanol with a concentration of 10% to 20% is poured on the surface, and after heat treatment at 200 to 400°C for 120 to 160 minutes, a fluorosilicone-modified polyester resin is sprayed with a spray gun, and then dried at 150°C and cured for 3 to 5 hours to obtain a composite insulation board.

[0019] The present invention uses hydrochloric acid solution to chemically etch the surface of the prepared modified aluminum silicate porous foam board to form a micro-scale rough structure, further uses nano-silicon dioxide to modify and improve the thermal insulation performance, and forms a micron-nano dual-scale structure, which enables water droplets to form an air cushion on the microstructure to achieve a super-hydrophobic effect, thereby reducing the water absorption rate; at the same time, fluorosilicone modified polyester resin is sprayed to enhance the heat resistance while increasing the adhesion stability of nano-silicon dioxide on the surface. In addition, the fluorosilicone modified polyester resin contains -CF2 and -CF3 groups, which have extremely low surface energy, causing surface super-hydrophobicity, and further enhancing its thermal insulation effect and thermal insulation performance.

[0020] Optionally, in step S4, the working pressure of the spray gun is 2 bar, the nozzle diameter is 0.5 mm, and the spraying distance is 400 mm.

[0021] Optionally, the composite insulation board for high-temperature kiln includes the following raw materials in parts by weight: 100-120 parts of high-purity magnesia, 2-10 parts of zirconium oxide, 10-20 parts of MnAl2O4, 10-25 parts of snail shell powder, 150-200 parts of sulfite waste liquid, 2-5 parts of silicon boron modified polyamide epichlorohydrin resin, 100-150 parts of microbial foaming agent, 200-300 parts of modified aluminum silicate active powder, and 95 parts of other additives; the raw materials of the other additives include: 50 parts of white cement, 40 parts of kaolin, and 5 parts of water reducer.

[0022] The above technical solution of the present invention includes at least the following beneficial effects: 1. The present invention relates to a method for preparing a novel columnar support column, aiming to improve its compressive strength and thermal insulation performance. The main materials are high-purity magnesia, zirconium oxide, MnAl2O4 and snail shell powder, wherein the snail shell powder is rich in calcium carbonate and has a porous structure, which helps to reduce density and enhance thermal insulation. At the same time, the addition of zirconium oxide and MnAl2O4 improves the high-temperature strength and toughness of the support column.

[0023] 2. Laser melting technology is used to replace traditional powder pressing to form a denser support body, and the slurry structure of the composite material further enhances connectivity, creates multiple stress transfer paths, and evenly distributes pressure. In addition, the use of silicon-boron modified polyamide epichlorohydrin resin as an adhesive improves high temperature resistance and mechanical strength, provides a buffering effect, and further improves the overall compressive performance.

[0024] 3. The present invention also uses microbial foaming agents to prepare porous foam boards, and combines chemical etching technology to achieve waterproof and heat-insulating treatment to minimize heat dissipation. Acetobacter reacts with sodium bicarbonate to produce carbon dioxide bubbles, forming closed pores, reducing water absorption and heat loss. The microtexture on the foam surface and nano-silicon dioxide spraying construct a dual-scale rough structure, which effectively hinders heat conduction and improves thermal insulation performance. At the same time, fluorosilicone-modified polyester resin provides excellent high temperature resistance and bonding effect, and enhances material strength and stability. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 Schematic diagram of the structure of the composite heat insulation board in an embodiment of the present invention. DETAILED DESCRIPTION

[0026] In order to make the purpose, technical solution and advantages of the embodiment of the present invention clearer, the technical solution of the embodiment of the present invention will be clearly and completely described in combination with the embodiment of the present invention. Obviously, the described embodiment is a part of the embodiment of the present invention, not all the embodiments. Based on the described embodiment of the present invention, all other embodiments obtained by ordinary technicians in this field belong to the scope of protection of the present invention.

[0027] Example 1 Preparation of adhesive: Add 25g of silicone, 10g of B(OH)3 and 10g of sodium alginate into 300mL of deionized water, add 50mL of 3% calcium hydroxide solution and heat to 110°C. After stirring for 1h, add 300mL of polyamide epichlorohydrin resin and ultrasonically disperse for 10min to obtain silicon-boron modified polyamide epichlorohydrin resin as an interlayer adhesive.

[0028] A mixture of 100 parts of high-purity magnesia, 10 parts of zirconium oxide, 20 parts of MnAl2O4, and 20 parts of snail shell powder was mixed with 150 parts of 5% sulfite waste liquid in a mixing grinder for 30 minutes; the mixed slurry was evenly spread in a columnar mold with a diameter of 10 mm, and the slurry was locally heated by a laser beam to melt and re-solidify into a layer with a thickness of 2 mm; the above steps were repeated, layer by layer, and 5 parts of silicon-boron modified polyamide epichlorohydrin resin were added between the layers for bonding until the thickness reached 20 mm. The sample was sintered in a high-temperature gas furnace at 1600°C for 3 hours, naturally cooled to room temperature, and solidified for 7 hours before demolding to obtain a columnar support body.

[0029] After incubating 100 parts of 10% Acetobacter solution at 170 r / min in a shaker at 35°C for 48 hours, 10 parts of 3% sodium bicarbonate solution were added to the solution, and stirred at 3000 r / min for 30 minutes with a high-speed stirrer to prepare a microbial foaming agent for use.

[0030] 200 parts of aluminum silicate active powder and 50 parts of copper powder are added to a mixed solution of 500 parts of phenyltriethoxysilane and anhydrous ethanol, and the mixture is ultrasonically treated for 30 minutes. The treated powder is dried at 80°C for 2 hours to obtain modified aluminum silicate active powder; wherein the ratio of the mass portion of phenyltriethoxysilane to the volume portion of anhydrous ethanol in the mixed solution of phenyltriethoxysilane and anhydrous ethanol is 0.1:5, and the ratio unit is g / mL.

[0031] 200 parts of modified aluminum silicate active powder, 50 parts of white cement, 40 parts of kaolin, 5 parts of water reducer, and 120 parts of microbial foaming agent were mixed evenly into a slurry and poured into a square mold with a length of 200 nm and a width of 50 nm to make its thickness reach 20 mm. After stirring for 50 minutes, the prepared columnar support was evenly and vertically placed therein. After sealing and wrapping, it was left to stand and cure for 26 hours before demolding to obtain a modified aluminum silicate porous foam board.

[0032] A 7% hydrochloric acid solution is evenly sprayed on the surface of the modified aluminum silicate porous foam board using a spray gun, and after drying at 100°C for 3 hours, a mixed solution of nano-silicon dioxide and ethanol with a concentration of 12% is poured on the surface. After heat treatment at 300°C for 150 minutes, a fluorosilicone modified polyester resin is sprayed with a spray gun. After drying at 150°C and curing for 4 hours, a composite insulation board is obtained; wherein, the working pressure of the spray gun is 2 bar, the nozzle diameter is 0.5 mm, and the spraying distance is 400 mm.

[0033] Example 2 Preparation of adhesive: Add 25g of silicone, 10g of B(OH)3 and 10g of sodium alginate into 300mL of deionized water, add 50mL of 5% calcium hydroxide solution and heat to 110°C. After stirring for 2h, add 300mL of polyamide epichlorohydrin resin and ultrasonically disperse for 20min to obtain silicon-boron modified polyamide epichlorohydrin resin as an interlayer adhesive.

[0034] A mixture of 120 parts of high-purity magnesia, 5 parts of zirconium oxide, 15 parts of MnAl2O4, and 10 parts of snail shell powder was mixed with 170 parts of 5% sulfite waste liquid in a mixing grinder for 40 minutes; the mixed slurry was evenly spread in a columnar mold with a diameter of 15 mm, and the slurry was locally heated by a laser beam to melt and re-solidify into a layer with a thickness of 3 mm; the above steps were repeated, layer by layer, and 4 parts of silicon-boron modified polyamide epichlorohydrin resin were added between the layers for bonding until a thickness of 25 mm was reached. The sample was sintered in a high-temperature gas furnace at 1500°C for 4 hours, naturally cooled to room temperature, and demolded after curing for 8 hours to obtain a columnar support body.

[0035] After incubating 100 parts of 10% Acetobacter solution at 170 r / min in a shaker at 35°C for 48 hours, 15 parts of 3% sodium bicarbonate solution were added to the solution, and stirred at 3000 r / min for 40 minutes with a high-speed stirrer to prepare a microbial foaming agent for use.

[0036] 200 parts of aluminum silicate active powder and 50 parts of copper powder are added to a mixed solution of 500 parts of phenyltriethoxysilane and anhydrous ethanol, and the mixture is ultrasonically treated for 20 minutes. The treated powder is dried at 60°C for 4 hours to obtain modified aluminum silicate active powder; wherein the ratio of the mass portion of phenyltriethoxysilane to the volume portion of anhydrous ethanol in the mixed solution of phenyltriethoxysilane and anhydrous ethanol is 0.1:5, and the unit of the ratio is g / mL.

[0037] 300 parts of modified aluminum silicate active powder, 50 parts of white cement, 40 parts of kaolin, 5 parts of water reducer, and 150 parts of microbial foaming agent were mixed evenly into a slurry and poured into a square mold with a length of 500 nm and a width of 200 nm to make its thickness reach 25 mm. After stirring for 60 minutes, the prepared columnar support was evenly and vertically placed therein. After sealing and wrapping, it was left to stand and cure for 26 hours before demolding to obtain a modified aluminum silicate porous foam board.

[0038] A 10% hydrochloric acid solution is evenly sprayed on the surface of the modified aluminum silicate porous foam board using a spray gun, and after drying at 100°C for 5 hours, a mixed solution of 15% nano-silicon dioxide and ethanol is poured on the surface, and after heat treatment at 200°C for 160 minutes, a fluorosilicone-modified polyester resin is sprayed with a spray gun, dried at 150°C, and cured for 5 hours to obtain a composite insulation board; wherein, the working pressure of the spray gun is 2 bar, the nozzle diameter is 0.5 mm, and the spraying distance is 400 mm.

[0039] Example 3 Preparation of adhesive: Add 25g of silicone, 10g of B(OH)3 and 10g of sodium alginate into 300mL of deionized water, add 50mL of 4% calcium hydroxide solution and heat to 110°C. After stirring for 2h, add 300mL of polyamide epichlorohydrin resin and ultrasonically disperse for 20min to obtain silicon-boron modified polyamide epichlorohydrin resin as an interlayer adhesive.

[0040] A mixture of 110 parts of high-purity magnesia, 2 parts of zirconium oxide, 20 parts of MnAl2O4, and 13 parts of snail shell powder was mixed with 150 parts of 5% sulfite waste liquid in a mixing grinder for 60 minutes; the mixed slurry was evenly spread in a columnar mold with a diameter of 30 mm, and the slurry was locally heated by a laser beam to melt and re-solidify into a layer with a thickness of 1 mm; the above steps were repeated, layer by layer, and 4 parts of silicon-boron modified polyamide epichlorohydrin resin were added between the layers for bonding until a thickness of 5 mm was reached. The sample was sintered in a high-temperature gas furnace at 1500°C for 2 hours, naturally cooled to room temperature, and demolded after curing for 5 hours to obtain a columnar support body.

[0041] After incubating 100 parts of 10% Acetobacter solution at 170 r / min in a shaker at 35°C for 48 hours, 10 parts of 3% sodium bicarbonate solution were added to the solution, and stirred at 3000 r / min for 20 minutes with a high-speed stirrer to prepare a microbial foaming agent for use.

[0042] 200 parts of aluminum silicate active powder and 50 parts of copper powder are added to a mixed solution of 500 parts of phenyltriethoxysilane and anhydrous ethanol, and the mixture is ultrasonically treated for 40 minutes. The treated powder is dried at 100°C for 1 hour to obtain modified aluminum silicate active powder; wherein the ratio of the mass portion of phenyltriethoxysilane to the volume portion of anhydrous ethanol in the mixed solution of phenyltriethoxysilane and anhydrous ethanol is 0.1:5, and the ratio unit is g / mL.

[0043] 200 parts of modified aluminum silicate active powder, 50 parts of white cement, 40 parts of kaolin, 5 parts of water reducer, and 100 parts of microbial foaming agent were mixed evenly into a slurry and poured into a square mold with a length of 400 nm and a width of 300 nm to make its thickness reach 5 mm. After stirring for 30 minutes, the prepared columnar support was evenly and vertically placed therein. After sealing and wrapping, it was left to stand and cure for 22 hours before demolding to obtain a modified aluminum silicate porous foam board.

[0044] A 5% hydrochloric acid solution is evenly sprayed on the surface of the modified aluminum silicate porous foam board using a spray gun, and after drying at 100°C for 2 hours, a mixed solution of 10% nano-silicon dioxide and ethanol is poured on the surface. After heat treatment at 200°C for 120 minutes, a fluorosilicone modified polyester resin is sprayed with a spray gun. After drying at 150°C and curing for 2 hours, a composite insulation board is obtained; wherein, the working pressure of the spray gun is 2 bar, the nozzle diameter is 0.5 mm, and the spraying distance is 400 mm.

[0045] Example 4 Preparation of adhesive: Add 25g of silicone, 10g of B(OH)3 and 10g of sodium alginate into 300mL of deionized water, add 50mL of 5% calcium hydroxide solution and heat to 110°C. After stirring for 1.5h, add 300mL of polyamide epichlorohydrin resin and ultrasonically disperse for 30min to obtain silicon-boron modified polyamide epichlorohydrin resin as an interlayer adhesive.

[0046] A mixture of 100 parts of high-purity magnesia, 10 parts of zirconium oxide, 15 parts of MnAl2O4, and 25 parts of snail shell powder was mixed with 200 parts of 5% sulfite waste liquid in a mixing grinder for 30 minutes; the mixed slurry was evenly spread in a columnar mold with a diameter of 10 mm, and the slurry was locally heated by a laser beam to melt and re-solidify into a layer with a thickness of 6 mm; the above steps were repeated, stacked layer by layer, and 2 parts of silicon boron modified polyamide epichlorohydrin resin were added between the layers for bonding until the thickness reached 30 mm. The sample was sintered in a high-temperature gas furnace at 1600°C for 4 hours, naturally cooled to room temperature, and demolded after curing for 10 hours to obtain a columnar support body.

[0047] After incubating 100 parts of 10% Acetobacter solution at 170 r / min in a shaker at 35°C for 48 hours, 10 parts of 3% sodium bicarbonate solution were added to the solution, and stirred at 3000 r / min for 20 minutes with a high-speed stirrer to prepare a microbial foaming agent for use.

[0048] 200 parts of aluminum silicate active powder and 50 parts of copper powder are added to a mixed solution of 500 parts of phenyltriethoxysilane and anhydrous ethanol, and the mixture is ultrasonically treated for 40 minutes. The treated powder is dried at 100°C for 1 hour to obtain modified aluminum silicate active powder; wherein the ratio of the mass portion of phenyltriethoxysilane to the volume portion of anhydrous ethanol in the mixed solution of phenyltriethoxysilane and anhydrous ethanol is 0.1:5, and the ratio unit is g / mL.

[0049] 300 parts of modified aluminum silicate active powder, 50 parts of white cement, 40 parts of kaolin, 5 parts of water reducer, and 130 parts of microbial foaming agent were mixed evenly into a slurry and poured into a square mold with a length of 300 nm and a width of 100 nm to make its thickness reach 30 mm. After stirring for 50 minutes, the prepared columnar support was evenly and vertically placed therein. After sealing and wrapping, it was left to stand and cure for 26 hours before demolding to obtain a modified aluminum silicate porous foam board.

[0050] A 10% hydrochloric acid solution is evenly sprayed on the surface of the modified aluminum silicate porous foam board using a spray gun, and after drying at 100°C for 5 hours, a mixed solution of 20% nano-silicon dioxide and ethanol is poured on the surface, and after heat treatment at 400°C for 160 minutes, a fluorosilicone modified polyester resin is sprayed with a spray gun, dried at 150°C, and cured for 5 hours to obtain a composite insulation board; wherein, the working pressure of the spray gun is 2 bar, the nozzle diameter is 0.5 mm, and the spraying distance is 400 mm.

[0051] Example 5 Preparation of adhesive: Add 25g of silicone, 10g of B(OH)3 and 10g of sodium alginate into 300mL of deionized water, add 50mL of 5% calcium hydroxide solution and heat to 110°C. After stirring for 1.5h, add 300mL of polyamide epichlorohydrin resin and ultrasonically disperse for 35min to obtain silicon-boron modified polyamide epichlorohydrin resin as an interlayer adhesive.

[0052] A mixture of 120 parts of high-purity magnesia, 5 parts of zirconium oxide, 10 parts of MnAl2O4, and 15 parts of snail shell powder was mixed with 150 parts of 5% sulfite waste liquid in a mixing grinder for 40 minutes; the mixed slurry was evenly spread in a columnar mold with a diameter of 20 mm, and the slurry was locally heated by a laser beam to melt and re-solidify into a layer with a thickness of 5 mm; the above steps were repeated, layer by layer, and the layers were bonded with 2 parts of silicon boron modified polyamide epichlorohydrin resin until the thickness reached 20 mm. The sample was sintered in a high-temperature gas furnace at 1600°C for 3.5 hours, naturally cooled to room temperature, and demolded after curing for 6 hours to obtain a columnar support body.

[0053] After incubating 100 parts of 10% Acetobacter solution at 170 r / min in a shaker at 35°C for 48 hours, 10 parts of 3% sodium bicarbonate solution were added to the solution, and stirred at 3000 r / min for 30 minutes with a high-speed stirrer to prepare a microbial foaming agent for use.

[0054] 200 parts of aluminum silicate active powder and 50 parts of copper powder are added to a mixed solution of 500 parts of phenyltriethoxysilane and anhydrous ethanol, and the mixture is ultrasonically treated for 45 minutes. The treated powder is dried at 100°C for 1.5 hours to obtain modified aluminum silicate active powder; wherein the ratio of the mass portion of phenyltriethoxysilane to the volume portion of anhydrous ethanol in the mixed solution of phenyltriethoxysilane and anhydrous ethanol is 0.1:5, and the unit of the ratio is g / mL.

[0055] 260 parts of modified aluminum silicate active powder, 50 parts of white cement, 40 parts of kaolin, 5 parts of water reducer, and 140 parts of microbial foaming agent were mixed evenly into a slurry and poured into a square mold with a length of 300 nm and a width of 150 nm to make its thickness reach 20 mm. After stirring for 40 minutes, the prepared columnar support was evenly and vertically placed therein. After sealing and wrapping, it was left to stand and cure for 25 hours before demolding to obtain a modified aluminum silicate porous foam board.

[0056] A hydrochloric acid solution with a concentration of 7% is evenly sprayed on the surface of the modified aluminum silicate porous foam board with a spray gun, and after drying at 100°C for 4 hours, a mixed solution of nano-silicon dioxide and ethanol with a concentration of 16% is poured on the surface. After heat treatment at 400°C for 160 minutes, a fluorosilicone-modified polyester resin is sprayed with a spray gun, dried at 150°C, and cured for 4 hours to obtain a composite insulation board; wherein, the working pressure of the spray gun is 2 bar, the nozzle diameter is 0.5 mm, and the spraying distance is 400 mm.

[0057] Example 6 Preparation of adhesive: Add 25g of silicone, 10g of B(OH)3 and 10g of sodium alginate into 300mL of deionized water, add 50mL of 5% calcium hydroxide solution and heat to 110°C. After stirring for 1.5h, add 300mL of polyamide epichlorohydrin resin and ultrasonically disperse for 35min to obtain silicon-boron modified polyamide epichlorohydrin resin as an interlayer adhesive.

[0058] A mixture of 110 parts of high-purity magnesia, 3 parts of zirconium oxide, 20 parts of MnAl2O4, and 12 parts of snail shell powder was mixed with 180 parts of 5% sulfite waste liquid in a mixing grinder for 40 minutes; the mixed slurry was evenly spread in a columnar mold with a diameter of 20 mm, and the slurry was locally heated by a laser beam to melt and re-solidify into a layer with a thickness of 4 mm; the above steps were repeated, layer by layer, and 3 parts of silicon-boron modified polyamide epichlorohydrin resin were added between the layers for bonding until the thickness reached 22 mm. The sample was sintered in a high-temperature gas furnace at 1600°C for 3 hours, naturally cooled to room temperature, and demolded after curing for 5 hours to obtain a columnar support body.

[0059] After incubating 100 parts of 10% Acetobacter solution at 170 r / min in a shaker at 35°C for 48 hours, 10 parts of 3% sodium bicarbonate solution were added to the solution, and stirred at 3000 r / min for 50 minutes with a high-speed stirrer to prepare a microbial foaming agent for use.

[0060] 200 parts of aluminum silicate active powder and 50 parts of copper powder are added to a mixed solution of 500 parts of phenyltriethoxysilane and anhydrous ethanol, and the mixture is ultrasonically treated for 40 minutes. The treated powder is dried at 100°C for 2 hours to obtain modified aluminum silicate active powder; wherein the ratio of the mass portion of phenyltriethoxysilane to the volume portion of anhydrous ethanol in the mixed solution of phenyltriethoxysilane and anhydrous ethanol is 0.1:5, and the unit of the ratio is g / mL.

[0061] 270 parts of modified aluminum silicate active powder, 50 parts of white cement, 40 parts of kaolin, 5 parts of water reducer, and 100 parts of microbial foaming agent were mixed evenly into a slurry and poured into a square mold with a length of 400 nm and a width of 230 nm to make its thickness reach 22 mm. After stirring for 40 minutes, the prepared columnar support was evenly and vertically placed therein. After sealing and wrapping, it was left to stand and cure for 23 hours before demolding to obtain a modified aluminum silicate porous foam board.

[0062] A 7% hydrochloric acid solution was evenly sprayed on the surface of the modified aluminum silicate porous foam board using a spray gun, and after drying at 100°C for 4 hours, a mixed solution of nano-silicon dioxide and ethanol with a concentration of 13% was poured on the surface. After heat treatment at 400°C for 160 minutes, a fluorosilicone-modified polyester resin was sprayed with a spray gun. After drying at 150°C and curing for 3.5 hours, a composite insulation board was obtained. The working pressure of the spray gun was 2 bar, the nozzle diameter was 0.5 mm, and the spraying distance was 400 mm.

[0063] Comparative Example 1 Compared with Example 1, the only difference is that the preparation of the columnar support body does not use laser melting technology and silicon boron modified polyamide epichlorohydrin resin as an interlayer adhesive, that is: a mixture of 100 parts of high-purity magnesia, 10 parts of zirconium oxide, 20 parts of MnAl2O4, and 20 parts of snail shell powder is mixed with 150 parts of 5% sulfite waste liquid in a mixing grinder for 30 minutes; the mixed slurry is evenly spread in a columnar mold with a diameter of 10 mm, pressed into a 20 mm column, and the sample is sintered in a high-temperature gas furnace at 1600°C for 3 hours, naturally cooled to room temperature, and demolded after curing for 7 hours to obtain a columnar support body; the remaining raw materials and steps are consistent with Example 1, and finally a composite insulation board is obtained.

[0064] Comparative Example 2 Compared with Example 1, the only difference is that copper powder and phenyltriethoxysilane are no longer added to the aluminum silicate active powder for modification treatment, and the remaining raw materials and steps are consistent with Example 1, and finally a composite thermal insulation board is prepared.

[0065] Comparative Example 3 Compared with Example 1, the only difference is that the modified aluminum silicate porous foam board is no longer prepared using a microbial foaming agent, and the aluminum silicate fiberboard is directly prepared, that is: 200 parts of aluminum silicate refractory fiber, 50 parts of white cement, 40 parts of kaolin, and 5 parts of water reducer are fully stirred and slurried, and then poured into a square mold with a length of 200 nm and a width of 50 nm, so that its thickness reaches 20 mm, and the prepared columnar support is evenly and vertically placed therein, and the mold is demolded after being allowed to stand and solidify for 26 hours to obtain an aluminum silicate fiberboard; the remaining raw materials and steps are consistent with Example 1, and a composite insulation board is finally obtained.

[0066] Comparative Example 4 Compared with Example 1, the only difference is that the modified aluminum silicate porous foam board is no longer subjected to chemical etching and surface modification, and the remaining raw materials and steps are consistent with Example 1, and finally a composite thermal insulation board is prepared.

[0067] Comparative Example 5 Compared with Example 1, the only difference is that no columnar support body is prepared, and the remaining raw materials and steps are consistent with Example 1, and finally a composite thermal insulation board is prepared.

[0068] The composite insulation boards prepared in Examples 1 to 6 and Comparative Examples 1 to 5 were subjected to relevant performance tests. The dry density, water absorption, compressive strength, flexural strength and static compressive elastic modulus test methods are derived from GB / T11969-2020 Autoclaved aerated concrete performance test method, and the thermal conductivity test method is derived from GB / T10294-2008 Insulation material steady-state thermal resistance and related properties determination guarded hot plate method. The relevant performance test results are shown in Table 1.

[0069] Table 1: Composite insulation board related performance test table

[0070] As shown in Table 1, the thermal insulation performance, relevant compressive strength, flexural strength and static compressive elastic modulus of the composite thermal insulation boards prepared in Examples 1 to 6 are significantly higher than those of the composite thermal insulation boards prepared in Comparative Examples 1 to 5; Combined with the data in Table 1, it can be seen from Example 1 compared with Comparative Example 3 that the dry density of the overall composite insulation board finally obtained is significantly higher due to the lack of microbial foaming agent in preparing the porous foam board, which in turn affects the thermal conductivity and makes the insulation effect poor; it can be seen from Example 1 compared with Comparative Example 4 that the surface of the aluminum silicate porous foam board in Example 1 is modified with nano-silicon dioxide and fluorine-silicon modified polyester resin, so that the water absorption rate and thermal conductivity are significantly reduced; it can be seen from Example 1 compared with Comparative Example 1 that the laser melting technology is combined with the preparation layer in the embodiment. The columnar support body is prepared by using an intermediate adhesive instead of the traditional direct pressing, so that the compressive strength and static compressive elastic modulus of the composite insulation board are significantly improved; it can be seen from the comparison between Example 1 and Comparative Example 5 that the addition of the columnar support body in Example 1 significantly improves the mechanical properties of the composite insulation board; it can be seen from the comparison between Example 1 and Comparative Example 2 that the water absorption rate and thermal conductivity coefficient are significantly reduced due to the modification of the aluminum silicate active powder and the addition of phenyltriethoxysilane and Cu; experiments have shown that the relevant performances of Examples 1~6 are significantly better than those of Comparative Examples 1~5.

[0071] The above are preferred embodiments of the present invention. It should be pointed out that, for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present invention. These improvements and modifications should also be regarded as within the scope of protection of the present invention.

Claims

1. A method for preparing a composite heat insulation board for a high temperature kiln, characterized in that: The following steps are involved: S1. Mix a mixture of high-purity magnesia, zirconium oxide, MnAl2O4 and snail shell powder with sulfite waste liquid; spread it evenly in a columnar mold, and solidify it into layers after laser melting; repeat the above steps, stacking layer by layer, adding silicon boron modified polyamide epichlorohydrin resin between layers, sintering at high temperature, cooling, solidifying, and demolding to obtain a columnar support body; S2, after incubating the acetic acid bacteria solution, adding sodium bicarbonate solution, stirring, and preparing a microbial foaming agent for use; S3, mixing the modified aluminum silicate active powder, other additives and microbial foaming agent evenly, pouring them into a square mold, stirring, vertically placing the prepared columnar support, sealing and wrapping, and standing to solidify to obtain a modified aluminum silicate porous foam board; S4. Spray hydrochloric acid solution on the surface of the prepared modified aluminum silicate porous foam board, dry it, pour a mixed solution of nano-silicon dioxide and ethanol, spray fluorine silicon modified polyester resin after heat treatment, dry and solidify it, and obtain a composite insulation board.

2. The method for preparing a composite heat insulation board for a high temperature kiln according to claim 1, characterized in that: In step S1, the boron-silicon modified polyamide epichlorohydrin resin is prepared by uniformly mixing organosilicon, B(OH)3 and sodium alginate in deionized water, adding calcium hydroxide solution and heating to 100-150°C, stirring for 1-2 hours, and then adding polyamide epichlorohydrin resin and ultrasonically dispersing for 10-30 minutes; wherein the mass ratio of organosilicon, B(OH)3 and sodium alginate is 2.5:1:1, the volume ratio of deionized water, calcium hydroxide solution and polyamide epichlorohydrin resin is 6:1:6, and the concentration of calcium hydroxide solution is 3%-5%.

3. The method for preparing a composite heat insulation board for a high temperature kiln according to claim 1, characterized in that: The concentration of the sulfite waste liquid in step S1 is 5%; the diameter of the columnar mold in step S1 is 10-30 mm; the thickness of each layer in step S1 is 1-6 mm; the mixing time in step S1 is 30-60 min; the high-temperature sintering temperature in step S1 is 1500-1600° C., and the time is 2-4 h; and the curing time in step S1 is 5-10 h.

4. The method for preparing a composite heat insulation board for a high temperature kiln according to claim 1, characterized in that: In the step S2, a 10% acetic acid bacteria solution is incubated at 170 r / min in a shaker at 35° C. for 48 hours, and then a 3% sodium bicarbonate solution is added and stirred at 3000 r / min for 20 to 50 minutes to prepare a microbial foaming agent.

5. The method for preparing a composite heat insulation board for a high temperature kiln according to claim 1, characterized in that: The modified aluminosilicate active powder in step S3 is prepared by mixing a mixed solution of aluminosilicate active powder, copper powder, phenyltriethoxysilane and anhydrous ethanol, ultrasonically treating for 20 to 40 minutes, and then drying at 60 to 100° C. for 1 to 4 hours.

6. The method for preparing a composite heat insulation board for a high temperature kiln according to claim 5, characterized in that: The mass ratio of aluminum silicate active powder and copper powder to the volume ratio of a mixed solution of phenyltriethoxysilane and anhydrous ethanol is 4:1:10; the mass ratio of phenyltriethoxysilane to the volume ratio of anhydrous ethanol in the mixed solution of phenyltriethoxysilane and anhydrous ethanol is 0.1:

5.

7. The method for preparing a composite heat insulation board for a high temperature kiln according to claim 1, characterized in that: The other additives in step S3 include white cement, kaolin, and water reducing agent; the stirring time is 30 to 60 minutes; the static curing time is 22 to 26 hours; the thickness of the modified aluminum silicate porous foam board is 5 to 30 mm; the length of the square mold is 200 to 500 mm and the width is 50 to 300 mm.

8. The method for preparing a composite heat insulation board for a high temperature kiln according to claim 1, characterized in that: In the step S4, a hydrochloric acid solution with a concentration of 5% to 10% is evenly sprayed on the surface of the prepared modified aluminum silicate porous foam board with a spray gun, and after drying at 100° C. for 2 to 5 hours, a mixed solution of nano-silicon dioxide and ethanol with a concentration of 10% to 20% is poured on the surface, and after heat treatment at 200 to 400° C. for 120 to 160 minutes, a fluorosilicone-modified polyester resin is sprayed with a spray gun, and then dried at 150° C. and cured for 3 to 5 hours to obtain a composite insulation board.

9. The method for preparing a composite heat insulation board for a high temperature kiln according to claim 1, characterized in that: In step S4, the working pressure of the spray gun is 2 bar, the nozzle diameter is 0.5 mm, and the spraying distance is 400 mm.

10. A composite heat insulation board, characterized in that: The composite heat insulation board for a high-temperature kiln is prepared by the preparation method of any one of claims 1 to 9, comprising the following raw materials in parts by weight: 100 to 120 parts of high-purity magnesia, 2 to 10 parts of zirconium oxide, 10 to 20 parts of MnAl2O4, 10 to 25 parts of snail shell powder, 150 to 200 parts of sulfite waste liquid, 2 to 5 parts of silicon boron modified polyamide epichlorohydrin resin, 100 to 150 parts of microbial foaming agent, 200 to 300 parts of modified aluminum silicate active powder, and 95 parts of other additives; The raw materials of the other additives include: 50 parts of white cement, 40 parts of kaolin, and 5 parts of water reducing agent.

Citation Information

Patent Citations

  • High-density production method for bacteriocin reuteri by using co-fermentation of lactobacillus reuteri and acetic acid bacteria

    CN107739747A

  • Environment-friendly waterproof adhesive and preparation method thereof

    CN111849415A

  • Magnesium-manganese spinel refractory material as well as preparation method and application thereof

    CN113024228A

  • Protective structure of zirconia-carbon based refractory

    JP2020083689A

  • Refractories and use thereof

    US20170341984A1

Cited By

  • Sintering method for porous carriers

    TWI929993B