Method for sintering ceramic component through laser in-situ rapid reaction
Through the laser in-situ rapid reaction sintering method combined with fast microextrusion 3D printing technology, the problems of high energy consumption, long time and thermal stress in traditional ceramic sintering methods are solved, and the rapid, economical and efficient sintering of ceramic materials is achieved, which improves the The density and properties of the material reduce production costs.
Patent Information
- Application Number
- CN202410734147.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-07
- Publication Date
- 2024-11-19
AI Technical Summary
Traditional ceramic sintering methods have problems such as high energy consumption, long time, easy to generate thermal stress, uneven local sintering, difficult to control the atmosphere and high production costs, which limits the widespread application and promotion of ceramic materials.
The laser in-situ rapid reaction sintering method is adopted, combined with rapid microextrusion 3D printing technology, and ceramic dielectrics and other parts are prepared through CO2 laser scanning to achieve a fast and accurate sintering process, reducing material losses and improving material utilization.
The rapid, economical and efficient sintering of ceramic materials is achieved, the thermal stress and local uneven problems in traditional methods are avoided, the density and performance of the materials are improved, the production costs are reduced, and the versatility and flexibility are provided.
Smart Images

Figure CN118978400A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for laser sintering ceramics, in particular to a method for laser in-situ rapid reaction sintering of ceramic components. Background Art
[0002] The preparation process of ceramic materials includes steps such as raw material preparation, molding, sintering and surface treatment. First, select appropriate ceramic raw materials, finely grind and mix them to ensure uniform particles. Then, the mixed powder is molded into a green body or the desired shape by pressing, injection molding or extrusion. Next, the molded green body is placed in a high-temperature sintering furnace for sintering treatment to promote the diffusion and combination of particles to form a dense structure. Finally, the ceramic may be surface treated, such as polishing, glazing, etc., to improve appearance and performance. The entire preparation process requires strict control of process parameters at each stage to ensure that the ceramic material has the required physical, chemical and mechanical properties and is suitable for various applications.
[0003] Sintering is particularly important in the preparation process of ceramic materials. However, the traditional sintering method is a commonly used process for preparing ceramic materials, and there are some obvious disadvantages and limitations: the traditional sintering method usually requires high-temperature treatment and consumes a lot of energy. The high energy consumption during high-temperature sintering leads to an increase in preparation costs and has a certain negative impact on the environment. The sintering process requires a long time to ensure that the ceramic material is fully thermalized, diffused and combined. The long sintering cycle will increase the production cycle and reduce production efficiency. During the high-temperature sintering process, thermal stress is easily generated inside the ceramic material due to temperature gradients and changes in crystal structure, resulting in cracks and deformation, reducing the quality and reliability of the material. Due to the uneven temperature distribution of the ceramic body during the sintering process, local under-sintering or over-sintering occurs, affecting the performance and density of the material. It is difficult to effectively control the atmosphere during the sintering process with traditional sintering, which is easy to cause oxidation or reduction reactions, affecting the chemical composition and properties of the ceramic material. Due to high energy consumption, long production cycle, and expensive raw materials and equipment costs, the production cost of the traditional sintering method is relatively high, which restricts the large-scale application and promotion of ceramic materials. In summary, the traditional sintering method has the disadvantages of high energy consumption, long time, easy to produce thermal stress, local uneven sintering, difficulty in controlling the atmosphere and high production cost.
[0004] Therefore, the pursuit of a new sintering method to quickly heat and cool ceramic materials; local heating; precise control of heating temperature and heating time; better control of the sintering process and product quality; reduce material loss during the heating process, reduce costs and improve material utilization. And better applicable to various materials, including metals, ceramics, composite materials, etc., with good versatility and flexibility. This is the development direction of the new generation of ceramic sintering technology. Summary of the invention
[0005] The purpose of the present invention is to provide a method for laser in-situ rapid reaction sintering of ceramic components. The method can easily perform advanced manufacturing of embryos or sintered ceramic parts by combining 3D printing with rapid micro-extrusion. The method of the present invention can quickly, simply, and cost-effectively perform laser scanning processing of proton ceramic dielectrics, hydrogen electrodes, oxygen electrodes, oxygen / hydrogen electrode brackets, interconnects, and mixed conductive dual-phase composite materials, and can be used to realize rapid laser processing of proton ceramic energy devices in a sustainable and clean manner.
[0006] The objective of the present invention is achieved through the following technical solutions: A method for laser in-situ rapid reaction sintering of ceramic components comprises the following steps: (1) Prepare battery electrolyte slurry.
[0007] (2) The anode material is deposited on the carrier using digital micro-extrusion 3D printing technology.
[0008] (3) Apply CO2 laser to the sample.
[0009] (4) Characterization of samples.
[0010] Preferably, the slurry in step (1) uses isopropanol as a grinding solvent, 1.0wt% NiO as a sintering additive, and 3 mmYSZ (yttrium-doped zirconia) as a grinding medium. The stoichiometric carbonate and oxide precursor powders are ball-milled for 48 hours and dried to remove the isopropanol solvent; the ball-milled dry powder is then mixed with deionized water and a dispersant, and ball-milled with a 3 mm YSZ grinding medium for 24 hours to obtain a stable slurry; finally, HPMC (hydroxypropyl methylcellulose) binder is added to the slurry and subjected to mechanical stirring and aging to successfully prepare a BCZYYb+1wt%NiO electrolyte slurry.
[0011] Preferably, the same method is used to prepare other parts slurries with different compositions, and the amounts of slurry, water, and dispersant are adjusted to a certain extent according to different formulas. BZY20+1wt%NiO electrolyte slurry and the like are also successfully prepared.
[0012] Preferably, in step (2), the different types of part slurries prepared in step (1) are added to a prepared plastic syringe container to avoid cross contamination. Compressed air is applied to drive the paste into a micro extruder having a needle nozzle with a diameter of 0.5 mm. The distance between the nozzle and the platform substrate is generally equal to the thickness of the wet layer (printed layer before drying) of 3D printing. Typically, the paste extrusion flow rate Q is 0.3 mL / min and the stage movement speed v is 15 mm / s.
[0013] Preferably, in step (3), a CO2 laser is used to dry each wet layer immediately after printing to accelerate the 3D printing process and avoid shape deformation; the laser beam is usually defocused by 15 mm to increase its spot size to 1 mm and reduce the laser energy density. RLRS technology has the advantages of rapid in-situ reaction sintering and controllable material microstructure.
[0014] Preferably, the laser operating parameters of the CO2 laser in step (3) are: the CO2 laser power for drying and sintering BCZYYb+1wt%NiO electrolyte slurry is 2.8 W, the CO2 laser power for drying and sintering BZY20+1wt%NiO electrolyte slurry is 7 W, and the scanning speed is 1 mm / s, which can effectively dry the green layer without obvious shrinkage and reaction; in order to further reduce the time consumption of drying, the Galvano scanner is equipped with a CO2 laser, which allows the use of higher laser power and faster scanning rate for the drying process. RLRS technology shortens the processing heat treatment / sintering that previously required more than 24 hours to a few seconds or minutes, and the device has better performance than traditional sintering.
[0015] Preferably, in step (3), a CO2 laser is used to form a linear spot through a cylindrical lens for sintering and densification of the electrolyte layer; a laser beam with a defocus distance of 20 mm and a beam spot size of about 8 mm is used to achieve uniform and moderate laser energy density; and the microstructure of the sintered layer is controlled by optimizing parameters such as laser power, moving speed, defocus amount and shadow line spacing.
[0016] Preferably, the characterization of the sample in step (4) is specifically performed by grinding the prepared BCZYYb and BZY20 strips into fine powder and using X-ray diffraction (XRD) to characterize the crystal structure. The data was recorded at a rate of 1° / min in the range of 15-85 degrees using a Rigaku Ultima IV diffractometer with monochromatic CuKα radiation. The results show that the crystallinity in the RLRS sample is better after sintering. The microstructure of the proton ceramic was studied by scanning electron microscopy (SEM). The results show that after sintering, the electrolyte membrane is completely dense and a relatively large grain size is obtained, which will significantly benefit the overall proton conductivity of the film.
[0017] Beneficial effects of the present invention: The laser processing of the present invention can accelerate the drying of each layer, speed up the 3D printing process and avoid shape deformation. It also solves the problem of shape deformation caused by the gravity and fluidity of the paste.
[0018] 2. The present invention is different from the traditional sintering method. RLRS is a new and efficient method that can use cheap carbonates and oxides in a single firing step to produce proton ceramics with well-controlled microstructures. Fully dense large grains, high porosity, porous / dense / porous interlayers and dense / porous half-cell microstructures have been successfully prepared.
[0019] 3. The RLRS method of the present invention has the advantages of being instantaneous, controllable and economical, which enables it to be combined with additive manufacturing to achieve rapid processing of ceramics, opening up a new path for advanced ceramic manufacturing. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 A schematic diagram of slurry preparation for the rapid laser reaction sintering method of the present invention; Figure 2 A schematic diagram of rapid 3D printing of the rapid laser reaction sintering processing method of the present invention; Figure 3 A schematic diagram of rapid laser scanning of the rapid laser reaction sintering processing method of the present invention; Figure 4 This is the principle diagram of the CO2 laser sintering system of the present invention; Figure 5 A schematic diagram showing a comparison between the XRD spectra of the proton ceramic strips prepared by the present invention and the proton ceramic particles prepared by solid-state reaction sintering; Figure 6 The XRD spectrum of the proton ceramic element film obtained by RLRS of the present invention; Figure 7 This is a SEM image of a dense protonic ceramic element film obtained by RLRS on the surface of BCZYYb+1wt%NiO of the present invention; Figure 8 This is the cross-sectional SEM image of the BZY20+1wt%NiO electrolyte of the present invention. DETAILED DESCRIPTION
[0021] The present invention will be described in detail below with reference to the embodiments shown in the accompanying drawings. Example
[0022] (1) According to BaCe 0.7 Zr 0.1 Y 0.1 Yb 0.1 O 3-δThe composition of the precursor solids of BaCO3, CeO2, ZrO2, Y2O3 and Yb2O3 in stoichiometric amounts was mixed with 1.0wt% NiO sintering additive and ball milled for 48 hours using isopropanol solvent and 3mm YSZ grinding media. After drying and removing the isopropanol solvent, deionized water solvent and DARVAN dispersant were added to the dried precursor powders. After ball milling with 3 mm YSZ grinding media for 24 hours, a stable slurry was obtained with a solid content of about 30-50% of the total volume and a dispersant dosage of about 2-10wt% of the water weight. Then, a 1-5wt% water amount of HPMC (hydroxypropyl methylcellulose) binder was added to the slurry and mechanically stirred for 20 minutes. After aging for 24 hours, BCZYYb+1wt%NiO electrolyte slurry was successfully prepared. BZY20+1wt%NiO electrolyte slurry was also successfully prepared.
[0023] (2) The prepared paste slurry was fed into a predetermined plastic syringe reservoir to avoid cross contamination. Compressed air was applied to drive the paste onto a micro extruder with a needle nozzle of 0.5 mm in diameter to extrude the slurry layer by layer.
[0024] (3) Using a CO2 laser with a laser power of 2.8 W and a scanning speed of 1 mm / s to form a linear spot through a cylindrical lens, it is used for the sintering and densification of the electrolyte BCZYYb+1wt%NiO. Using a CO2 laser with a laser power of 7 W and a scanning speed of 1 mm / s to form a linear spot through a cylindrical lens, it is used for the sintering and densification of the electrolyte BZY20+1wt%NiO. Figure 4 Schematic diagram of CO2 laser sintering system (4) The prepared BCZYYb and BZY20 ribbons were ground into fine powders and characterized by X-ray diffraction (XRD). Data were recorded at a rate of 1° / min in the range of 15-85 degrees using a Rigaku Ultima IV diffractometer with monochromatic Cu Kα radiation. For comparison, the XRD patterns of the two corresponding BCZYYb and BZY20 particles made by SSRS are shown in Figure 2. Figure 5As shown. It can be easily seen that the BCZYYb-RLRS bars and BCZYYb-SSRS particles show exactly the same XRD pattern, which can be attributed to the pure orthorhombic perovskite structure similar to BaCeO3. Specifically, the peaks of the BCZYYb-RLRS bars are higher than those of the CZYYb-SSRS particles, which may indicate that the RLRS samples have better crystallinity. On the other hand, the BZY20-RLRS bars and Y20-SSRS particles behave similarly to the BCZYYb ceramics. Both the BZY20-RLRS bars and BZY20-SSRS particles show the same XRD pattern, which can be attributed to the cubic perovskite similar to BaZrO3. However, the difference in crystallinity of the BZY20 ceramics is not obvious. Therefore, for both BCZYYb and BZY20 ceramics, the RLRS process only takes a few seconds to achieve the same crystal structure as the state-of-the-art SSRS process at 00-1500 temperatures for at least 10 hours. XRD tests were performed on all relevant samples, and the results showed that all prepared materials were in the correct phase. Figure 6 shown.
[0025] Surface image of BCZYYb+1wt%NiO Figure 7 It is clearly shown that the electrolyte membrane is fully dense. The relative density based on ImageJ analysis of multiple SEM images is above 95%. A relatively large grain size is obtained, which will significantly benefit the overall proton conductivity of this film. Figure 8 It shows that the most refractory protonic ceramic electrolyte BZY20 is fully densified with the help of 1wt% NiO sintering aid.
Claims
1. A method for laser in-situ rapid reaction sintering of ceramic components, characterized in that: The method comprises the following steps: (1) preparing battery electrolyte slurry; (2) Depositing the anode material on the support using digital micro-extrusion 3D printing technology; (3) Applying CO2 laser to the sample; (4) Sample characterization; The slurry in the above step (1) uses isopropanol as a grinding solvent, 1.0wt% NiO as a sintering additive, and 3 mm YSZ (yttrium-doped zirconium oxide) as a grinding medium. The stoichiometric carbonate and oxide precursor powders are ball-milled for 48 hours and dried to remove the isopropanol solvent; then the ball-milled dry powder is mixed with deionized water and a dispersant, and ball-milled with a 3 mm YSZ grinding medium for 24 hours to obtain a stable slurry; finally, HPMC (hydroxypropyl methylcellulose) binder is added to the slurry and mechanically stirred and aged to prepare BCZYYb+1wt%NiO (BaCe 0.7 Zr 0.1 Y 0.1 Yb 0.1 O 3-δ +1wt%NiO) electrolyte slurry; In the above step (2), the component slurry prepared in step (1) is added to a prepared plastic syringe container to avoid cross contamination; compressed air is applied to drive the paste into a micro extruder with a needle nozzle with a diameter of 0.5 mm; the distance between the nozzle and the platform substrate is equal to the thickness of the wet layer (printed layer before drying) of the 3D printing; In the above step (3), the CO2 laser dries each wet layer immediately after printing to accelerate the 3D printing process and avoid shape deformation; the laser beam is defocused by 15 mm to increase its spot size to 1 mm and reduce the laser energy density; In step (4), the sample is subjected to X-ray diffraction (XRD) to analyze its diffraction pattern to obtain the composition of the material, the structure or morphology of the atoms or molecules inside the material; and the sample is subjected to scanning electron microscopy (SEM) analysis to characterize the microscopic morphology of the sample.
2. The method for laser in-situ rapid reaction sintering of ceramic components according to claim 1, characterized in that: The method is used to prepare component slurries of different components, and the amounts of slurry, water and dispersant are adjusted according to different formulas; for example, BZY20+1wt%NiO(BaZr 0.8 Y 0.2 O 3−δ +1wt%NiO) electrolyte slurry.
3. The method for laser in-situ rapid reaction sintering of ceramic components according to claim 1, characterized in that: The paste extrusion flow rate Q of the extruder is 0.3 mL / min, and the stage moving speed v is 15 mm / s.
4. The method for laser in-situ rapid reaction sintering of ceramic components according to claim 1, characterized in that: The laser operating parameters of the CO2 laser in step (3) are: the CO2 laser power for drying and sintering BCZYYb+1wt%NiO electrolyte slurry is 2.8 W, and the CO2 laser power for drying and sintering BZY20+1wt%NiO(BaZr 0.8 Y 0.2 O 3−δ The CO2 laser power for the electrolyte slurry (+1wt%NiO) was 7 W and the scanning speed was 1 mm / s.
5. The method for laser in-situ rapid reaction sintering of ceramic components according to claim 1, characterized in that: In the step (3), a CO2 laser is used to form a linear spot through a cylindrical lens for sintering and densification of the electrolyte layer; a laser beam with a defocus distance of 20 mm and a beam spot size of about 8 mm is used to achieve uniform laser energy density; and the microstructure of the sintered layer is controlled by optimizing the laser power, moving speed, defocus amount and shadow line spacing parameters.
Citation Information
Patent Citations
Method for preparing piezoelectric ceramics based on femtosecond lasers and 3D printing
CN105058549A
Integrated additive manufacturing and laser processing systems and methods for ceramic, glass, and silicon carbide applications
US20220009124A1
Cited By
METHOD FOR PRODUCING THIN-FILM ELECTROLYTE BASED ON Ce1-XGdXO2 ON SURFACE OF NiO / GDC ANODE BLANK