New concrete joint surface treatment method

By pretreating the concrete surface and applying a specific interface adhesive layer, the problem of reducing bonding strength of epoxy resin-based interface agents in humid environments is solved, and the high performance and safety of the bonding surfaces of new and old concrete is achieved, ensuring that Structural stability and safety of bridge reinforcement and restoration.

CN118978407APending Publication Date: 2024-11-19FOSHAN ROAD & BRIDGE MAINTENANCE CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410904625.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-08
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

The bonding strength of existing epoxy resin-based interface agents is reduced in humid environments and is very different from the linear expansion coefficient of concrete, resulting in cracks, peeling, peeling and other problems on the bonding surfaces of new and old concrete, affecting structural performance and safety. sex.

Method used

A new concrete bonding surface treatment method is adopted, including pretreatment of the concrete structure surface to be repaired, coating the interface glue to form the first interface glue layer and the second interface glue layer, and pouring new concrete on the surface of the second interface glue layer , the interface glue consists of epoxy resin, isofluorone diisocyanate, polyether glycol, fluorosilicone polymer and curing agent. The thermal deformation temperature is 60-70℃, and the water absorption rate is low, ensuring that under temperature changes and humid environments bonding strength and impact resistance.

Benefits of technology

Improve the bonding performance of the bonding surface of new and old concrete, ensure that the number of measured points with poor bonding is less than 10% of the total number of measured points. The 28d shear bonding strength and positive pull bonding strength reach 3.9MPa or above, and the interface glue is not easy to fall off due to temperature changes. , meets the reinforcement and restoration needs of water bridges, and the compressive strength and tensile strength of the new concrete reach 40.5MPa and above.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The invention discloses a new concrete joint surface treatment method which comprises the following steps: (1) pretreating the surface of a concrete structure to be repaired to enable the surface to reach a dry saturation state; (2) preparing an interface adhesive; (3) the surface of the pretreated concrete structure is evenly coated with interface glue, and the interface glue permeates into the to-be-repaired concrete structure to form a first interface glue layer; (4) after the first interface adhesive layer becomes gel, uniformly coating the interface adhesive again to form a second interface adhesive layer; (5) pouring new concrete on the surface of the second interface adhesive layer after the second interface adhesive layer is gelled; and (6) performing standard curing on the new concrete. By implementing the method, the performance of new concrete and the bonding performance of old concrete can be improved, a bonding interface does not crack or peel off, and the mechanical property and the use safety of the overall structure of the repaired concrete are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of bridge repair and reinforcement construction, and in particular to a method for processing a bonding surface of new concrete. Background Art

[0002] Concrete has good plasticity, integrity and durability, and has been widely used in the field of engineering construction. However, due to environmental effects or changes in use loads, concrete structures will deteriorate or reduce in strength during service, so it is necessary to reinforce or repair the concrete structure. The process of reinforcement and repair of concrete structures often involves the interface bonding problem between new and old concrete. The interface between new and old concrete is a transition zone where old concrete, new concrete and interface agent coexist, among which the interface agent has an important influence on the bond strength and tensile strength of the interface between new and old concrete.

[0003] Common interface agents in engineering projects mainly include cement-based, epoxy resin and polymer types, among which epoxy resin interface agents are the most widely used. The bonding strength of epoxy resin interface agents is relatively high, but the bonding strength decreases in a humid environment, which is not conducive to the reinforcement and repair of water bridges. In addition, the linear expansion coefficient of epoxy resin interface agents is quite different from that of concrete, and deformation and shedding may occur under repeated temperature changes. If the performance of the interface agent cannot meet the construction requirements, it will cause cracks, warping, peeling and other phenomena, seriously affecting the performance and safety of the overall structure of new and old concrete. Summary of the invention

[0004] The technical problem to be solved by the present invention is to provide a method for treating the bonding surface of new concrete, which can improve the performance of the bonding surface of new and old concrete and form a bonding surface of new and old concrete that is not peeled off, has no cracks and has good durability.

[0005] In order to solve the above problems, the present invention discloses a method for treating a bonding surface of new concrete, comprising the following steps:

[0006] (1) Pre-treat the surface of the concrete structure to be repaired to make it reach a dry saturated state;

[0007] (2) Configure interface glue;

[0008] (3) uniformly coating the interface adhesive on the surface of the pretreated concrete structure, wherein the interface adhesive penetrates into the concrete structure to be repaired and forms a first interface adhesive layer;

[0009] (4) After the first interface adhesive layer becomes gelled, evenly apply the interface adhesive again to form a second interface adhesive layer;

[0010] (5) After the second interface adhesive layer becomes gelled, pouring new concrete on the surface of the second interface adhesive layer;

[0011] (6) Carry out standard curing on new concrete.

[0012] As an improvement of the above technical solution,

[0013] The interface glue comprises a matrix component and a curing component, and the mass ratio of the matrix component to the curing component is (1-5):1;

[0014] The matrix component includes the following components in parts by weight: 80-100 parts of epoxy resin, 20-45 parts of isophorone diisocyanate, 20-40 parts of polyether diol, 5-20 parts of fluorosilicone polymer, 3-6 parts of epoxy cage silsesquioxane, 80-100 parts of solvent, and 0.5-5 parts of functional additive;

[0015] The curing component comprises the following components in parts by weight: 80 to 95 parts of a curing agent and 5 to 10 parts of a solvent.

[0016] As an improvement of the above technical solution,

[0017] The fluorosilicone polymer comprises the following raw materials in weight percentage: 45-75% of 1,3,5-trimethyl-1,3,5-tris(3,3,3-trifluoropropyl)cyclotrisiloxane, 10-30% of 3-(2-aminoethyl)-aminopropyltrimethoxysilane, 0.5-1.5% of ethylenediamine, and 0.1-0.5% of water;

[0018] The epoxy cage-type silsesquioxane comprises the following raw materials in weight percentage: 35-50% phenyltriethoxysilane, 15-30% beta-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 1-10% n-octyltriethoxysilane, 20-40% solvent, 0.1-1% inorganic acid and 0.5-2% inorganic base.

[0019] As an improvement of the above technical solution, the thermal deformation temperature of the interface adhesive is 60-70° C., and the water absorption rate of the interface adhesive is 0.02-0.05%.

[0020] As an improvement of the above technical solution, the dosage of the first interface adhesive layer is 0.3-0.8 L / m 2 The amount of the interface glue of the second interface glue layer is 0.3-1.0 L / m 2 .

[0021] As an improvement of the above technical solution, in step (2) and / or step (3), the interface glue is applied by pressurized spraying, and the spraying pressure is 0.4-0.6 MPa.

[0022] As an improvement of the above technical solution, the second interface adhesive layer is also allowed to stand for 40 to 80 minutes after the second interface adhesive layer is formed.

[0023] As an improvement of the above technical solution, the new concrete includes the following components in parts by weight: 150 to 200 parts of cement, 100 to 150 parts of fly ash, 20 to 60 parts of mineral powder, 1500 to 2000 parts of aggregate, 5 to 15 parts of nano-SiO2, 15 to 30 parts of polypropylene fiber, 2 to 10 parts of surfactant, and 10 to 40 parts of admixture.

[0024] As an improvement of the above technical solution, the fiber length of the polypropylene fiber is 10 to 25 mm, and the equivalent diameter is 15 to 100 μm.

[0025] As an improvement of the above technical solution,

[0026] The aggregate is river sand and crushed stone; the fineness modulus of the river sand is 2.6-3.2; the particle size of the crushed stone is 5-20 mm, with continuous grading;

[0027] The admixture includes one or more of a water reducing agent, an air entraining agent, an early strength agent, an expansion agent, and a retarder.

[0028] The implementation of the present invention has the following beneficial effects:

[0029] 1. The present invention improves the bonding performance of the concrete structure to be repaired and the new concrete by pretreating the surface of the concrete structure to be repaired and coating the first interface adhesive layer and the second interface adhesive layer, and then pouring new concrete. After pouring the new concrete and curing, the number of measuring points with poor bonding of the overall structure is ≤10% of the total number of measuring points, the 28d shear bonding strength is ≥3.9MPa, and the 28d positive tensile bonding strength is ≥3.6MPa.

[0030] 2. The thermal deformation temperature of the interface adhesive of the present invention is 60°C to 70°C, and the interface adhesive will not be deformed or fall off due to changes in temperature. The water absorption rate of the interface adhesive is 0.02% to 0.05%, and the bonding strength is high in a humid environment. In addition, the interface adhesive has good bonding strength and high impact resistance, which can meet the reinforcement and repair needs of water bridges.

[0031] 3. The new concrete of the present invention is shrinkage compensating fiber concrete. The coordination of the expansion limit rate and mechanical strength of the new concrete is achieved through the component ratio design of the new concrete. The 28d compressive strength of the new concrete is ≥40.5MPa, the 28d tensile strength is ≥3.9MPa, and the expansion limit rate is 0.015% to 0.020%. DETAILED DESCRIPTION

[0032] In order to make the purpose, technical solutions and advantages of the present invention more clear, the present invention is described in further detail below.

[0033] The present invention provides a method for treating a bonding surface of new concrete, comprising the following steps:

[0034] (1) Pre-treat the surface of the concrete structure to be repaired to achieve a dry saturated state.

[0035] The surface cleanliness and roughness of the concrete structure to be repaired directly affect its bonding performance with new concrete, so the surface of the concrete structure to be repaired needs to be pretreated.

[0036] Specifically, the surface of the concrete structure to be repaired is cleaned to remove dust, loose materials, plaster, grease, corrosion deposits and algae; after cleaning, the surface is roughened by rough chiseling or sandblasting, and the loose skin is removed to expose the solid material; finally, it is rinsed with high-pressure water, and water is sprayed to keep the surface of the concrete structure to be repaired in a dry and saturated state.

[0037] (2) Configure interface glue.

[0038] Specifically, the interface glue includes a matrix component and a curing component, and the mass ratio of the matrix component to the curing component is (1-5):1. The matrix component includes the following components in parts by weight: 80-100 parts of epoxy resin, 20-45 parts of isophorone diisocyanate, 20-40 parts of polyether diol, 5-20 parts of fluorosilicone polymer, 3-6 parts of epoxy cage silsesquioxane, 80-100 parts of solvent, and 0.5-5 parts of functional additives. The curing component includes the following components in parts by weight: 80-95 parts of curing agent and 5-10 parts of solvent.

[0039] The interface adhesive of the present invention can achieve improved bonding performance. Specifically, by controlling the ratio of polyurethane and epoxy resin, it is helpful to increase the thermal deformation temperature of the interface adhesive, ensuring that it will not deform and fall off when the temperature changes; fluorosilicone polymer and epoxy cage-type silsesquioxane modification help to improve the thermal deformation temperature and toughness of the interface adhesive, so that the interface adhesive has good impact strength and shear strength, and can also improve the bonding strength in a humid environment. By limiting the mass parts of different components, while ensuring the bonding strength of the interface adhesive, the thermal deformation temperature of the interface adhesive is increased, the water absorption rate is reduced, the interface adhesive after bonding is firmly bonded to the new and old concrete, and the interface adhesive layer will not crack or peel off, thereby achieving good bonding of the new and old concrete without anchor bars in a humid environment, avoiding damage to the old concrete structure caused by buried anchor bars, and improving the safety performance of the repaired concrete structure.

[0040] The fluorosilicone polymer comprises the following raw materials in weight percentage: 45-75% of 1,3,5-trimethyl-1,3,5-tris(3,3,3-trifluoropropyl)cyclotrisiloxane, 10-30% of 3-(2-aminoethyl)-aminopropyltrimethoxysilane, 0.5-1.5% of ethylenediamine, and 0.1-0.5% of water.

[0041] The preparation method of the fluorosilicone polymer comprises: uniformly stirring 1,3,5-trimethyl-1,3,5-tri(3,3,3-trifluoropropyl)cyclotrisiloxane, ethylenediamine and water in proportion at 50°C to 70°C, heating to 100°C for dehydration, adding 3-(2-aminoethyl)-aminopropyltrimethoxysilane to the dehydrated product at 50°C to 70°C, and reacting to obtain the fluorosilicone polymer.

[0042] The epoxy cage type silsesquioxane comprises the following raw materials in percentage by weight: 35-50% of phenyltriethoxysilane, 15-30% of beta-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 1-10% of n-octyltriethoxysilane, 20-40% of solvent, 0.1-1% of inorganic acid and 0.5-2% of inorganic base.

[0043] The preparation method of epoxy cage type silsesquioxane comprises: adding inorganic acid to a solvent in proportion, adjusting the pH to 3-4, adding phenyltriethoxysilane, β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane and n-octyltriethoxysilane in sequence, performing a hydrolysis reaction for 20h-40h to obtain a colorless transparent liquid, adjusting the pH to neutral with an inorganic base, and distilling off the solvent to obtain epoxy cage type silsesquioxane.

[0044] In the process of preparing the interface adhesive, the matrix component and the curing component can be prepared separately, and then the curing component is added to the matrix component and stirred evenly for ≥2 minutes until the color is completely uniform.

[0045] Specifically, the epoxy resin is preferably bisphenol A epoxy resin and / or bisphenol F epoxy resin.

[0046] The solvent is preferably one or more of N,N-dimethylformamide, N,N-diethylformamide, N,N-dimethylacetamide, N-methylpyrrolidone and N-ethylpyrrolidone.

[0047] Other functional additives include but are not limited to defoamers, wetting agents, film-forming aids, and thickeners. Among them, the defoamer is preferably a polyether defoamer or a modified silicone. The wetting agent is preferably a polyether-modified water-based wetting agent or a silicone-modified water-based wetting agent. The film-forming aid is preferably one or more of diethylene glycol butyl ether, dipropylene glycol methyl ether, and dipropylene glycol butyl ether. The thickener is preferably a polyurethane associative thickener.

[0048] (3) The interface adhesive is evenly coated on the surface of the pretreated concrete structure. The interface adhesive penetrates into the concrete structure to be repaired and forms a first interface adhesive layer. After coating, no defective coating film can be formed on the surface of the concrete structure.

[0049] The amount of interface glue used in the first interface glue layer is 0.3 L / m 2 ~0.8L / m2 . Preferably, the interface glue is applied by pressurized spraying, and the spraying pressure is 0.4MPa to 0.6MPa, exemplified by 0.4MPa, 0.42MPa, 0.45MPa, 0.5MPa, 0.55MPa or 0.6MPa, but not limited thereto. The spraying quality is improved by pressurized spraying. When the steel bars are dense or large-scale construction is required, an air compressor, a pressure vessel and a spray gun can be used for spraying to achieve uniform spraying of the colloid, and the colloid can be fully distributed on the spraying surface.

[0050] (3) After the first interface adhesive layer becomes gelled, the interface adhesive is evenly applied again to form a second interface adhesive layer.

[0051] The amount of interface glue used in the second interface glue layer is 0.3L / m 2 ~1.0L / m 2 After forming the first interface adhesive layer, the interface adhesive is allowed to penetrate into the concrete, and after the first interface adhesive layer becomes gelled, the second layer is applied and used as a bonding layer. Preferably, the interface adhesive is applied by pressurized spraying, and the spraying pressure is 0.4MPa to 0.6MPa.

[0052] (4) After the second interface adhesive layer becomes gelled, new concrete is poured on the surface of the second interface adhesive layer.

[0053] In one embodiment, after forming the second interface adhesive layer, the second interface adhesive layer is left to stand for 40 to 80 minutes, and new concrete is poured before the second interface adhesive layer becomes gelled and solidifies. If the second interface adhesive layer has solidified, the interface adhesive should be applied again and the above construction process should be repeated.

[0054] Specifically, the new concrete includes the following components in parts by weight: 150-200 parts of cement, 100-150 parts of fly ash, 20-60 parts of mineral powder, 1500-2000 parts of aggregate, 5-15 parts of nano-SiO2, 15-30 parts of polypropylene fiber, 2-10 parts of surfactant, and 10-40 parts of admixture.

[0055] Surfactants can adhere nano-SiO2 to polypropylene fibers. Nano-SiO2 and polypropylene fibers are evenly distributed in the concrete without agglomeration, ensuring the tensile strength and shrinkage compensation performance of the concrete. They can improve the performance of the bonding surface between new and old concrete, forming a bonding surface between new and old concrete that is non-peeling, crack-free, and has good durability.

[0056] The fiber length of the polypropylene fiber is preferably 10 mm to 25 mm, and is exemplarily 10 mm, 12 mm, 15 mm, 18 mm, 20 mm or 25 mm, but not limited thereto. The equivalent diameter of the polypropylene fiber is 15 μm to 100 μm, and is exemplarily 15 μm, 30 μm, 40 μm, 50 μm, 80 μm or 100 μm, but not limited thereto. By optimizing the length, diameter and doping amount of the polypropylene fiber, the mechanical properties of the new concrete are improved.

[0057] The selection of other components is as follows: the alkali content of silicate cement is ≤0.60%, the C3A content in clinker is ≤8.0%; the chloride ion content in fly ash is ≤0.02%.

[0058] The aggregate is preferably non-active, specifically river sand and crushed stone. The aggregate is tested for alkali activity before construction, and the alkali-carbonate reaction expansion rate of the aggregate is ≤0.20%. When the alkali-silica reaction expansion rate of the aggregate is between 0.10% and 0.20%, the total alkali content in the concrete should not be greater than 1.8kg / m 3 , and should be verified by the effectiveness test of alkali-aggregate reaction inhibition measures. The fineness modulus of river sand is 2.6-3.2; the particle size of crushed stone is 5mm-20mm, with continuous grading; the maximum particle size of crushed stone is ≤25mm, and the maximum particle size of crushed stone is ≤3 / 4 of the minimum clear distance of steel bars.

[0059] The surfactant can be polyvinyl alcohol-4000.

[0060] The admixture includes one or more of a water reducer, an air entraining agent, a retarder, and an expansion agent. Preferably, the water reducer adopts a high-efficiency polycarboxylic acid high-performance water reducer, and the performance indicators of the other admixtures shall comply with the provisions of GB 8076-2008 "Concrete Admixtures". The expansion agent adopts UEA expansion agent, and the performance indicators shall comply with the provisions of GB / T 23439-2017 "Concrete Expansion Agents".

[0061] The new concrete mix design of the present invention can achieve coordination between concrete strength and expansion rate, with the new concrete having a 28d compressive strength of ≥40.5MPa, a 28d tensile strength of ≥3.9MPa, and a limited expansion rate of 0.015% to 0.020%. The combination of the new concrete and the interface adhesive has a high bonding strength, and will not peel off or fall off after being subjected to stress for a long time.

[0062] The present invention will be further described below with specific embodiments:

[0063] Example 1

[0064] This embodiment provides a method for treating a bonding surface of new concrete, comprising the following steps:

[0065] (1) Pre-treat the surface of the concrete structure to be repaired to achieve a dry saturated state.

[0066] Clean the surface of the concrete structure to be repaired to remove dust, loose materials, plaster, grease, corrosion deposits and algae; after cleaning, roughen the surface by rough chiseling or sandblasting, and remove the loose skin to expose the solid material; finally, rinse it with high-pressure water and spray water to keep the surface of the concrete structure to be repaired in a dry and saturated state.

[0067] (2) The interface adhesive is applied to the pre-treated surface of the concrete structure and completely covers it. The interface adhesive penetrates into the concrete structure to be repaired and forms a first interface adhesive layer. After the application, no defective coating film can be formed on the surface of the concrete structure.

[0068] The interface adhesive includes a matrix component and a curing component, and the mass ratio of the matrix component to the curing component is 3:1. The matrix component includes the following components in parts by weight: 90 parts of epoxy resin, 30 parts of isophorone diisocyanate, 25 parts of polyether diol, 5 parts of fluorosilicone polymer, 4 parts of epoxy cage silsesquioxane, 85 parts of solvent, and 2 parts of functional additives. The curing component includes the following components in parts by weight: 85 parts of curing agent and 5 parts of solvent. Prepare the curing component and the matrix component separately, add the curing component to the matrix component and stir evenly, and stir for 5 minutes until the color is completely uniform.

[0069] The epoxy cage-type silsesquioxane comprises the following raw materials in percentage by weight: 74% vinyltrimethoxysilane, 24.6% solvent, 0.4% hydrochloric acid and 1% sodium hydroxide.

[0070] The fluorosilicone polymer comprises the following raw materials in weight percentage: 95% of 1,3,5-trimethyl-1,3,5-tris(3,3,3-trifluoropropyl)cyclotrisiloxane, 3.7% of ethylenediamine, and 1.3% of water.

[0071] The amount of interface glue used in the first interface glue layer is 0.3L / m 2 , the spraying pressure is 0.5MPa.

[0072] (3) After the first interface adhesive layer is formed, the interface adhesive is allowed to penetrate into the concrete. After the first interface adhesive layer becomes gelled, the interface adhesive is applied again to form the second interface adhesive layer.

[0073] The amount of interface glue used in the second interface glue layer is 0.3L / m 2 , the spraying pressure is 0.5MPa.

[0074] (4) The second interface adhesive layer is allowed to stand for 60 minutes. After the second interface adhesive layer becomes gelled, new concrete is poured on the surface of the second interface adhesive layer.

[0075] Specifically, the new concrete includes the following components in parts by weight: 180 parts of cement, 120 parts of fly ash, 40 parts of mineral powder, 1670 parts of aggregate, 20 parts of polypropylene fiber, 2 parts of water reducing agent, 1 part of air entraining agent, 1 part of retarder, and 20 parts of expansion agent.

[0076] Example 2

[0077] This embodiment provides a method for treating the bonding surface of new concrete, which differs from Embodiment 1 in that the interface adhesive includes a matrix component and a curing component, and the mass ratio of the matrix component to the curing component is 3:1. The matrix component includes the following components in parts by weight: 90 parts of epoxy resin, 30 parts of isophorone diisocyanate, 25 parts of polyether diol, 4 parts of epoxy cage-type silsesquioxane, 85 parts of solvent, and 2 parts of functional additives. The curing component includes the following components in parts by weight: 85 parts of curing agent and 5 parts of solvent. Prepare the curing component and the matrix component separately, add the curing component to the matrix component and stir evenly, and stir for 5 minutes until the color is completely uniform.

[0078] The epoxy cage-type silsesquioxane comprises the following raw materials in percentage by weight: 43% phenyltriethoxysilane, 25% β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 6% n-octyltriethoxysilane, 24.6% solvent, 0.4% hydrochloric acid and 1% sodium hydroxide.

[0079] The rest are the same as in Example 1.

[0080] Example 3

[0081] This embodiment provides a method for treating the bonding surface of new concrete, which differs from Embodiment 1 in that the interface adhesive includes a matrix component and a curing component, and the mass ratio of the matrix component to the curing component is 3:1. The matrix component includes the following components in parts by weight: 90 parts of epoxy resin, 30 parts of isophorone diisocyanate, 25 parts of polyether diol, 5 parts of fluorosilicone polymer, 85 parts of solvent, and 2 parts of functional additives. The curing component includes the following components in parts by weight: 85 parts of curing agent and 5 parts of solvent. Separately configure the curing component and the matrix component, add the curing component to the matrix component and stir evenly, and stir for 5 minutes until the color is completely uniform.

[0082] The fluorosilicone polymer includes the following raw materials in percentage by weight: 72.3% of 1,3,5-trimethyl-1,3,5-tris(3,3,3-trifluoropropyl)cyclotrisiloxane, 26.8% of 3-(2-aminoethyl)-aminopropyltrimethoxysilane, 0.9% of ethylenediamine, and 0.3% of water.

[0083] The rest are the same as in Example 1.

[0084] Example 4

[0085] This embodiment provides a method for treating the bonding surface of new concrete, which differs from Embodiment 1 in that the interface adhesive includes a matrix component and a curing component, and the mass ratio of the matrix component to the curing component is 3:1. The matrix component includes the following components in parts by weight: 90 parts of epoxy resin, 30 parts of isophorone diisocyanate, 25 parts of polyether diol, 5 parts of fluorosilicone polymer, 4 parts of epoxy cage-type silsesquioxane, 85 parts of solvent, and 2 parts of functional additives. The curing component includes the following components in parts by weight: 85 parts of curing agent and 5 parts of solvent. Separately configure the curing component and the matrix component, add the curing component to the matrix component and stir evenly, and stir for 5 minutes until the color is completely uniform.

[0086] The fluorosilicone polymer comprises the following raw materials in weight percentage: 72.3% of 1,3,5-trimethyl-1,3,5-tris(3,3,3-trifluoropropyl)cyclotrisiloxane, 26.8% of 3-(2-aminoethyl)-aminopropyltrimethoxysilane, 0.9% of ethylenediamine, and 0.3% of water;

[0087] The epoxy cage type silsesquioxane comprises the following raw materials in percentage by weight: 43% of phenyltriethoxysilane, 25% of beta-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 6% of n-octyltriethoxysilane, 24.6% of solvent, 0.4% of hydrochloric acid and 1% of sodium hydroxide.

[0088] The rest are the same as in Example 1.

[0089] Example 5

[0090] This embodiment provides a method for treating the bonding surface of new concrete, which differs from Embodiment 4 in that the new concrete includes the following components in parts by weight: 180 parts of cement, 120 parts of fly ash, 40 parts of mineral powder, 1670 parts of aggregate, 8 parts of nano-SiO2, 20 parts of polypropylene fiber, 6 parts of surfactant, 2 parts of water reducer, 1 part of air entraining agent, 1 part of retarder, and 20 parts of expansion agent.

[0091] The rest are the same as in Example 4.

[0092] Comparative Example 1

[0093] This embodiment provides a method for treating the bonding surface of new concrete, which differs from Embodiment 1 in that the interface adhesive includes a matrix component and a curing component, and the mass ratio of the matrix component to the curing component is 3:1. The matrix component includes the following components in parts by weight: 90 parts of epoxy resin, 80 parts of solvent, and 3 parts of functional additives. The curing component includes the following components in parts by weight: 85 parts of curing agent and 5 parts of solvent. The curing component and the matrix component are separately prepared, and the curing component is added to the matrix component and stirred evenly for 5 minutes until the color is completely uniform.

[0094] The rest are the same as in Example 1.

[0095] The old concrete structure was treated by the bonding surface treatment methods of Examples 1 to 5 and Comparative Example 1, and performance tests were performed according to GB 50367-2013 "Concrete Structure Reinforcement Design Code" and GB 50550-2010 "Concrete Structure Reinforcement Engineering Construction Quality Acceptance Code". The specific results are as follows:

[0096]

[0097]

[0098] It can be seen from Examples 1 to 5 that by optimizing the interface adhesive component and the new concrete component, the shear bonding strength and positive tensile bonding strength of the concrete can be improved. The interface adhesive of the embodiment of the present invention has good bonding performance and is not prone to peeling and cracking. The new concrete formula of the embodiment of the present invention can be well matched with the interface adhesive and is not prone to falling off. Comparative Example 1 uses conventional epoxy resin as the interface adhesive, the adhesive layer has a low thermal deformation temperature, and the bonding strength is low in a humid environment, resulting in poor mechanical properties of the repaired concrete, affecting the safety of the repaired concrete.

[0099] The above is a preferred embodiment of the invention. It should be pointed out that a person skilled in the art can make several improvements and modifications without departing from the principle of the invention. These improvements and modifications are also considered to be within the scope of protection of the invention.

Claims

1. A method for treating the bonding surface of new concrete, characterized in that: The following steps are involved: (1) Pre-treat the surface of the concrete structure to be repaired to make it reach a dry saturated state; (2) Configure interface glue; (3) uniformly coating the interface adhesive on the surface of the pretreated concrete structure, wherein the interface adhesive penetrates into the concrete structure to be repaired and forms a first interface adhesive layer; (4) After the first interface adhesive layer becomes gelled, evenly apply the interface adhesive again to form a second interface adhesive layer; (5) After the second interface adhesive layer becomes gelled, pouring new concrete on the surface of the second interface adhesive layer; (6) Carry out standard curing on new concrete.

2. The method for treating the bonding surface of new concrete according to claim 1, characterized in that: The interface glue comprises a matrix component and a curing component, and the mass ratio of the matrix component to the curing component is (1-5):1; The matrix component includes the following components in parts by weight: 80-100 parts of epoxy resin, 20-45 parts of isophorone diisocyanate, 20-40 parts of polyether diol, 5-20 parts of fluorosilicone polymer, 3-6 parts of epoxy cage silsesquioxane, 80-100 parts of solvent, and 0.5-5 parts of functional additive; The curing component comprises the following components in parts by weight: 80 to 95 parts of a curing agent and 5 to 10 parts of a solvent.

3. The method for treating the bonding surface of new concrete according to claim 2, characterized in that: The fluorosilicone polymer comprises the following raw materials in weight percentage: 45-75% of 1,3,5-trimethyl-1,3,5-tris(3,3,3-trifluoropropyl)cyclotrisiloxane, 10-30% of 3-(2-aminoethyl)-aminopropyltrimethoxysilane, 0.5-1.5% of ethylenediamine, and 0.1-0.5% of water; The epoxy cage-type silsesquioxane comprises the following raw materials in weight percentage: 35-50% phenyltriethoxysilane, 15-30% beta-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 1-10% n-octyltriethoxysilane, 20-40% solvent, 0.1-1% inorganic acid and 0.5-2% inorganic base.

4. The method for treating the bonding surface of new concrete according to claim 3, characterized in that: The thermal deformation temperature of the interface glue is 60-70° C., and the water absorption rate of the interface glue is 0.02-0.05%.

5. The method for treating the bonding surface of new concrete according to claim 1, characterized in that: The dosage of the first interface adhesive layer is 0.3-0.8 L / m 2 The amount of the interface glue of the second interface glue layer is 0.3-1.0 L / m 2 .

6. The method for treating the bonding surface of new concrete according to claim 1, characterized in that: In step (2) and / or step (3), the interface glue is applied by pressurized spraying, and the spraying pressure is 0.4-0.6 MPa.

7. The method for treating the bonding surface of new concrete according to claim 1, characterized in that: The method also includes allowing the second interface adhesive layer to stand for 40 to 80 minutes after the second interface adhesive layer is formed.

8. The method for treating the bonding surface of new concrete according to claim 1, characterized in that: The new concrete comprises the following components in parts by weight: 150-200 parts of cement, 100-150 parts of fly ash, 20-60 parts of mineral powder, 1500-2000 parts of aggregate, 5-15 parts of nano-SiO2, 15-30 parts of polypropylene fiber, 2-10 parts of surfactant and 10-40 parts of admixture.

9. The method for treating the bonding surface of new concrete according to claim 8, characterized in that: The fiber length of the polypropylene fiber is 10 to 25 mm, and the equivalent diameter is 15 to 100 μm.

10. The method for treating the bonding surface of new concrete according to claim 8, characterized in that: The aggregate is river sand and crushed stone; the fineness modulus of the river sand is 2.6-3.2; the particle size of the crushed stone is 5-20 mm, with continuous grading; The admixture includes one or more of a water reducing agent, an air entraining agent, an early strength agent, an expansion agent, and a retarder.