Recycling method of waste lithium battery and product
By combining inorganic salt solutions with organic recycling agents, the problem of incomplete treatment of fluorine and phosphorus compounds in lithium battery recycling has been solved, achieving efficient recovery of lithium hexafluorophosphate and lithium carbonate, reducing environmental pollution and lowering costs.
Patent Information
- Application Number
- CN202411051455.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-01
- Publication Date
- 2024-11-19
AI Technical Summary
Existing lithium battery recycling methods pose environmental pollution problems, especially the incomplete treatment of fluorine and phosphorus compounds in the chemical discharge method, which leads to an increase in organic waste liquid, high costs, and difficulty in large-scale application.
By combining inorganic salt solutions with organic recovery agents, and through adjusting the pH value and repeating the process multiple times, hexafluorophosphate and lithium carbonate are precipitated, reducing environmental pollution and improving recovery efficiency.
This technology effectively recycles lithium hexafluorophosphate and lithium carbonate from lithium batteries, reducing environmental pollution and lowering process costs, thus achieving efficient recycling and reuse of waste lithium batteries.
Smart Images

Figure CN118978446A_ABST
Abstract
Description
Technical Field
[0001] The present application belongs to the technical field of lithium battery recycling, and more specifically, relates to a method and product for recycling waste lithium batteries. Background Art
[0002] With the rapid development of the new energy industry, the production of lithium-ion batteries has surged, and the amount of lithium-ion batteries scrapped has also increased significantly. The recycling of waste lithium-ion batteries has received more and more attention. Waste lithium-ion batteries generally still retain some or even most of the energy, and as the battery cycle continues, "lithium precipitation" and other behaviors may occur inside the lithium-ion battery. If the lithium-ion battery is not discharged before recycling, there will be risks of fire or even explosion during the disassembly of the battery, causing serious safety problems. Therefore, in order to ensure that there are no such problems during the crushing process of lithium-ion batteries, before the lithium battery is pre-processed for crushing, the recycled waste lithium-ion battery module needs to be disassembled into individual lithium battery cells, and each lithium battery cell needs to be discharged.
[0003] There are two main methods for discharging lithium batteries: (1) discharging by physical methods, mainly by external loads, that is, by connecting the battery to an external load, the power in the battery is consumed by heat release, but this method is difficult to apply on a large scale, and it is difficult to completely consume the energy inside the battery. At the same time, the fluorine and phosphorus compounds inside the battery will affect the performance and economic benefits of the positive electrode material recovery during subsequent high-temperature calcination and other processes; (2) by chemical discharge methods, that is, breaking the shell of the waste lithium battery and immersing it in a salt solution to accelerate the self-discharge process of the lithium-ion battery. This solution is simple and effective, but the waste lithium-ion battery with a broken shell will leach the electrolyte components into the salt solution, and the fluorine and phosphorus compounds and organic solution components therein will cause serious harm to the environment. The existing solution generally adds an oxidant to the salt solution to degrade the organic solution components, and uses chemical precipitation, flocculation sedimentation, adsorption, reverse osmosis, etc. to treat the fluorine and phosphorus compounds therein, but its pollution cannot be completely avoided and brings additional costs.
[0004] Patent document CN117567290A discloses a method for recycling waste lithium batteries, by soaking waste lithium batteries in organic solvents, obtaining crude lithium hexafluorophosphate, then dissolving it and fully mixing it with a salt composed of hydrophobic cations and hydrophilic anions, and then standing for phase separation, and obtaining a hydrophobic salt composed of hydrophobic cations and hexafluorophosphate from the organic phase. This method can recover hexafluorophosphate and lithium salt from waste lithium batteries; however, its recovery process involves multi-step phase separation, solvent evaporation, cleaning and other steps, the process is cumbersome and requires the use of complex liquid separation devices, and the recovery process will use a variety of organic solvents, which will inevitably bring more organic waste liquids while increasing the process cost, causing greater pollution and damage to the environment. Under this limitation, large-scale production and application feasibility are low. However, organic substances such as acetonitrile and diethyl carbonate are used in its recovery process, and the wastewater in the recovery process is difficult to handle, and it is easy to form organic waste, causing environmental pollution. Summary of the invention
[0005] In view of the defects of the prior art, the present application proposes a method for recycling and treating waste lithium batteries, which can recover the fluorine-phosphorus compounds dissolved in the salt solution during the self-discharge process of the chemical discharge method, thereby reducing the environmental pollution problems caused by the lithium battery recycling process.
[0006] To achieve the above object, the present application discloses a method for recycling waste lithium batteries, comprising the following steps:
[0007] S1. Obtaining a first salt solution; the first salt solution is an inorganic salt solution with a mass fraction of 2.5% to 15%, wherein the inorganic salt is one or more of sodium sulfate, sodium chloride, ammonium sulfate, and ammonium chloride;
[0008] S2-1. Add the waste lithium battery with the exposed battery cell to the first salt solution and soak it to fully dissolve the hexafluorophosphate and lithium ions in the waste lithium battery; filter out the waste lithium battery to obtain a first filtrate; wherein the mass ratio of the first salt solution to the waste lithium battery is (1 to 5): 1;
[0009] S2-2. Determine whether the mass fraction of hexafluorophosphate in the first filtrate obtained in the previous step is greater than or equal to a first threshold value, otherwise, let the first filtrate be the first salt solution, return to the step S2-1, and if yes, proceed to the next step; the first threshold value is 2% to 4%;
[0010] S3-1. Obtaining an organic recovery agent; the organic recovery agent is an organic salt solid or an organic salt solution having a mass fraction of 20% to 60%; the cation of the organic salt is a hydrophobic cation, and the anion of the organic salt is a hydrophilic anion;
[0011] S3-2. According to the mass ratio of 10: (1 to 3), the organic recovery agent is added to the first filtrate, so that the hexafluorophosphate in the first filtrate forms a hexafluorophosphate precipitate with the hydrophobic cation in the organic recovery agent and is filtered to obtain a second filtrate;
[0012] S3-3. Determine whether the concentration of lithium ions in the second filtrate obtained in the previous step is greater than or equal to the second threshold value, otherwise, let the second filtrate be the first salt solution, return to step S2-1, and if yes, proceed to the next step; the second threshold value is 4 to 10 g / L;
[0013] S4. Add 10% to 50% by mass of a carbonate solution to the second filtrate at a mass ratio of (4 to 11): 1, so that the carbonate ions in the carbonate solution and the lithium ions in the second filtrate form a lithium carbonate precipitate; after filtering, a third filtrate and a lithium carbonate precipitate are obtained.
[0014] Preferably, in step S2-2, the mass fraction of the hexafluorophosphate is determined by nuclear magnetic resonance spectroscopy.
[0015] Preferably, in step S3-3, the concentration of the lithium ions is determined by ICP-OES.
[0016] Preferably, before step S2-1, the method further comprises: adding an acetate buffer solution so that the pH value of the first salt solution is 7-8.
[0017] Preferably, the hydrophobic cation in step S3-1 is one or more of a quaternary ammonium cation, an imidazole cation, a pyridine cation, an oxopiperidinium cation, and a metallocene complex cation.
[0018] As further preferred, the hydrophobic cation in step S3-1 is one or more of tetra-n-butylammonium ion, 1-ethyl-3-methylimidazolium cation, N-butylpyridinium cation, 2,2,6,6-tetramethyl-1-oxopiperidinium cation or ferrocenium ion.
[0019] Preferably, the hydrophilic anion in step S3-1 is one or more of chloride ion, nitrate ion, sulfate ion, perchlorate ion, and tetrafluoroborate ion.
[0020] Preferably, the carbonate in step S4 is one or more of sodium carbonate and ammonium carbonate.
[0021] The present application also discloses hexafluorophosphate or lithium carbonate obtained by the above recovery method.
[0022] Compared with the prior art, the waste lithium battery recycling method disclosed in the present application can recycle the fluorine-phosphorus compounds dissolved in the inorganic salt solution during the self-discharge process of the waste lithium battery by the chemical discharge method, thereby reducing the environmental pollution problem caused by the waste lithium battery recycling process;
[0023] In the recycling method of the present application, an organic salt or organic salt solution composed of hydrophobic cations and hydrophilic anions, as well as a water-soluble soluble carbonate, is introduced to recover lithium hexafluorophosphate, the most commonly used electrolyte salt in the recycling of waste lithium-ion batteries, and convert it into a salt composed of hydrophobic cations and hexafluorophosphate, and lithium carbonate; the salt composed of hydrophobic cations and hexafluorophosphate is usually used as a supporting electrolyte for organic solutions in electrochemical analysis, and lithium carbonate is an important raw material in the lithium-ion battery industry and has important value;
[0024] By repeating S2 multiple times (usually 3 to 5 times), the concentration of hexafluorophosphate in the solution is increased to ensure that a hydrophobic salt containing hexafluorophosphate can be precipitated in step S3; by adjusting the pH of the solution, the hydrolysis process of hexafluorophosphate in water is inhibited, so that step S3 can be carried out more fully and the recovery efficiency is improved;
[0025] Repeating steps S2-S3 multiple times (usually 2 to 6 times) to increase the concentration of lithium ions and ensure that lithium carbonate precipitation can be formed in step S4;
[0026] It has been verified that the third filtrate finally obtained in the recovery method of the present application can also be returned to step S2-1 for recycling, thus avoiding the generation of waste liquid. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 It is a schematic diagram of the recycling method of this application;
[0028] Figure 2 This is a schematic diagram of a drum stirring device in step S2-1 of an example of the present application;
[0029] Figure 3 is the nuclear magnetic resonance fluorine spectrum of tetra-n-butylammonium hexafluorophosphate recovered in step (3-2) of Example 1 of the present application;
[0030] Figure 4 is the nuclear magnetic resonance fluorine spectrum of the first filtrate recovered in step (2-1) of Example 1 of the present application;
[0031] Figure 5 This is the nuclear magnetic resonance fluorine spectrum of the third filtrate recovered in step (4) of Example 1 of the present application. DETAILED DESCRIPTION
[0032] In order to make the purpose, technical solution and advantages of the present application more clearly understood, the present application is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present application and are not used to limit the present application.
[0033] In the description of the present application, it should be understood that the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Thus, a feature defined as "first" or "second" may explicitly or implicitly include one or more of the feature. In the description of the present application, "plurality" means two or more, unless otherwise clearly and specifically defined.
[0034] Additionally, references throughout this specification to "one embodiment," "one embodiment," "some embodiments," "an example," or similar language indicate that a particular feature, structure, or characteristic described in connection with the embodiment is included in at least one embodiment of the present application. Thus, appearances of the phrase "in one embodiment," "in one embodiment," and similar language throughout this specification may, but do not necessarily, all refer to the same embodiment.
[0035] The present application provides a method for recycling waste lithium batteries, such as Figure 1 As shown, the following steps are included:
[0036] S1. Obtaining an inorganic salt solution having a mass fraction of 2.5% to 15%, and using the inorganic salt solution as a first salt solution; the inorganic salt is one or more of sodium sulfate, sodium chloride, ammonium sulfate, and ammonium chloride;
[0037] S2-1. Adding acetate buffer, adjusting the pH value of the first salt solution to 7-8; then adding the waste lithium battery with exposed cells to the first salt solution, Figure 2 The waste lithium battery is immersed in a similar drum stirring device for 12 to 48 hours to fully dissolve the hexafluorophosphate and lithium ions in the waste lithium battery; the waste lithium battery is filtered out to obtain a first filtrate; wherein the mass ratio of the first salt solution to the waste lithium battery is (1 to 5): 1, and the acetate buffer contains sodium acetate with a molar concentration of 0.13 mol / L to 0.34 mol / L and ammonium acetate with a molar concentration twice that of sodium acetate;
[0038] S2-2. Determine whether the mass fraction of hexafluorophosphate in the first filtrate obtained in the previous step is greater than or equal to the first threshold value, otherwise, let the first filtrate be the first salt solution and return to the step S2-1; if yes, proceed to the next step; the first threshold value is 2% to 4%; the first threshold value is 2% to 4%; when a waste lithium battery is treated for the first time, the mass fraction of hexafluorophosphate in the first filtrate can be determined by nuclear magnetic resonance spectroscopy, but when the same waste lithium battery is treated repeatedly, empirical parameters can be used; usually after the step S2-1 is performed 3-5 times, the mass fraction of hexafluorophosphate in the first filtrate can reach the recovery standard;
[0039] S3-1. Obtain an organic recovery agent; the organic recovery agent is an organic salt solid or an organic salt solution with a mass fraction of 20% to 60%; the cation of the organic salt is a hydrophobic cation, such as one or more of a quaternary ammonium cation, an imidazole cation, a pyridinium cation, an oxopiperidinium cation, and a metallocene complex cation. In some embodiments, the hydrophobic cation is a tetra-n-butylammonium ion, a 1-ethyl-3-methylimidazolium cation, an N-butylpyridinium cation, a 2,2,6,6-tetramethyl-1-oxopiperidinium cation, or a ferrocenium ion; the anion of the organic salt is a hydrophilic anion, such as one or more of a chloride ion, a nitrate ion, a sulfate ion, a perchlorate ion, and a tetrafluoroborate ion;
[0040] When an organic salt is used as an organic recovery agent, the hydrophobic cation in step S3-1 is one or more of 1-ethyl-3-methylimidazolium cation, N-butylpyridinium cation, 2,2,6,6-tetramethyl-1-oxopiperidinium cation or ferrocenium ion, and the hydrophilic anion is chloride ion, nitrate ion, sulfate ion, perchlorate ion, tetrafluoroborate ion;
[0041] When an organic salt solution is used as an organic recovery agent, the hydrophobic cation is a tetra-n-butylammonium ion, and the hydrophilic anion is a sulfate ion; when the organic salt solution is used as an organic recovery agent, the mass fraction of the organic salt solution is 20% to 60%;
[0042] S3-2. According to the mass ratio of 10: (1 to 3), the organic recovery agent is added to the first filtrate, so that the hexafluorophosphate in the first filtrate forms a hexafluorophosphate precipitate with the hydrophobic cation in the organic recovery agent and is filtered to obtain a second filtrate;
[0043] S3-3. Determine whether the concentration of lithium ions in the second filtrate obtained in the previous step is greater than or equal to the second threshold value, otherwise, let the second filtrate be the first salt solution, and return to step S2-1; if yes, proceed to the next step; the second threshold value is 4 to 10 g / L; when a waste lithium battery is treated for the first time, the concentration of lithium ions in the second filtrate can be determined by ICP-OES, but when the same waste lithium battery is treated repeatedly, empirical parameters can be used; usually after the steps S2-1 to S3-2 are performed 2 to 6 times, the concentration of lithium ions in the second filtrate can reach the recovery standard;
[0044] S4. According to the mass ratio of (4 to 11): 1, a carbonate solution (such as sodium carbonate or ammonium carbonate) having a mass fraction of 10% to 50% is added to the second filtrate, so that the carbonate ions in the carbonate solution and the lithium ions in the second filtrate form a lithium carbonate precipitate, wherein the carbonate is one or more of sodium carbonate and ammonium carbonate; after filtering, a third filtrate and a lithium carbonate precipitate are obtained;
[0045] Similarly, parameters such as the ratio of the organic recovery agent to the first filtrate, the concentration of the inorganic salt solution, the selection of the organic recovery agent, the mass ratio of the first salt solution to the waste lithium battery, the concentration of the carbonate solution, the mass ratio of the second filtrate to the carbonate solution, etc. are within the scope of protection required by the present application and can be set or adjusted according to the test results of the nuclear magnetic resonance spectrum and ICP-OES to ensure that the hexafluorophosphate and lithium carbonate can be completely precipitated; when repeatedly treating the same type of waste lithium batteries, empirical parameters can be used.
[0046] The third filtrate recovered by the method of the present application can be returned to step S2-1 and recycled as the first salt solution; and the hexafluorophosphate and lithium carbonate precipitates can be used for the reproduction of lithium batteries.
[0047] The following contents are examples
[0048] Example 1
[0049] This embodiment takes 450kg of discarded 100Ah lithium iron phosphate||graphite square shell batteries as an example to recover valuable components therein. The specific steps are as follows:
[0050] (1) breaking the battery shell of the waste lithium iron phosphate battery to expose the internal battery core of the lithium battery, and evenly dividing it into 9 portions, each weighing 50 kg; and simultaneously preparing 75 kg of ammonium sulfate solution with a mass fraction of 3.5% as the first salt solution;
[0051] (2-1) adding a mixed solution of ammonium acetate and sodium acetate with a mass fraction of 3% (the molar ratio of the two is 1:2) to a first salt solution, and adjusting the pH value of the first salt solution to 7.5; soaking a portion of the broken waste lithium iron phosphate battery obtained in step (1) in the first salt solution for 24 hours, and mixing them thoroughly by rolling stirring, and finally dissolving the fluorine and phosphorus components in the waste lithium battery in the first salt solution, filtering, and obtaining a first filtrate and the discharged waste lithium iron phosphate battery;
[0052] (2-2) Through nuclear magnetic resonance spectroscopy detection, the mass fraction of hexafluorophosphate in the first filtrate obtained for the first time is detected to be about 0.8%, which is insufficient to form enough precipitation in the subsequent steps; the first filtrate is used as the first salt solution and returned to step (2-1) for recycling the broken waste lithium iron phosphate batteries; after three times of treatment to recover the broken waste lithium iron phosphate batteries, the concentration of hexafluorophosphate in the first filtrate is increased to three times that after the first immersion, the mass fraction accounts for 2.2%, and the mass is about 70kg;
[0053] (3-1) 20.5 kg of 50% tetra-n-butylammonium sulfate aqueous solution was used as an organic recovery agent;
[0054] (3-2) adding an organic recovery agent to the first filtrate, so that the hexafluorophosphate in the first filtrate and the hydrophobic cation (i.e., tetra-n-butylammonium ion) in the organic recovery agent form a precipitate, and filtering to obtain 4.5 kg of tetra-n-butylammonium hexafluorophosphate and 76 kg of the second filtrate;
[0055] (3-3) The concentration of lithium ions in the second filtrate was determined by ICP-OES detection; the concentration of lithium ions in the second filtrate obtained for the first time was about 1.3 g / L, which was not enough to form precipitation in the subsequent steps; therefore, the second filtrate was used as the first salt solution and returned to step (2-1) for recovery; after repeating the steps between step (2-1) and step (3-3) three times, all 9 waste lithium iron phosphate batteries were recovered; at this time, the total mass of tetra-n-butylammonium hexafluorophosphate recovered was 13.8 kg, and the mass of the second filtrate was 76.7 kg;
[0056] (4) The second filtrate obtained in step (3) is added to 9 kg of 50% by mass sodium carbonate solution to precipitate lithium carbonate with the lithium ions therein, and filtered to obtain 3.0 kg of lithium carbonate solid and 82.7 kg of the third filtrate. The third filtrate can be returned to step (2-1) as the first salt solution for use.
[0057] Example 2
[0058] This example takes 420kg of discarded 100Ah nickel-cobalt-manganese ternary||graphite square shell batteries as an example to recover valuable components therein. The specific steps are as follows:
[0059] (1) breaking the battery shell of the waste graphite square shell battery to expose the internal battery core of the lithium battery, and evenly dividing it into 6 portions, each weighing 70 kg; directly using 82.7 kg of the third filtrate obtained in Example 1 as the first salt solution;
[0060] (2-1) adding a mixed solution of ammonium acetate and sodium acetate with a mass fraction of 8% (the molar ratio of the two is 1:2) to a first salt solution, and adjusting the pH value of the first salt solution to 7.5; soaking a portion of the broken waste graphite square shell battery obtained in step (1) in the first salt solution for 30 hours, and mixing them thoroughly by rolling stirring, and finally dissolving the fluorine and phosphorus components in the waste graphite square shell battery in the first salt solution, filtering, and obtaining a first filtrate and the discharged waste graphite square shell battery;
[0061] (2-2) Through nuclear magnetic resonance spectroscopy detection, the mass fraction of hexafluorophosphate in the first filtrate obtained for the first time is detected to be about 0.8%, which is insufficient to form enough precipitation in the subsequent steps; the first filtrate is used as the first salt solution and returned to step (2-1) for recycling the broken waste graphite square shell batteries; after three times of treatment to recover the broken waste lithium iron phosphate batteries, the concentration of hexafluorophosphate in the first filtrate is increased to three times that after the first immersion, the mass fraction accounts for 2.1%, and the mass is about 70kg;
[0062] (3-1) 19.6 kg of a 50% by mass aqueous solution of tetra-n-butylammonium sulfate is used as an organic recovery agent;
[0063] (3-2) adding an organic recovery agent to the first filtrate, so that the hexafluorophosphate in the first filtrate and the hydrophobic cation (i.e., tetra-n-butylammonium ion) in the organic recovery agent form a precipitate, and filtering to obtain 6.4 kg of tetra-n-butylammonium hexafluorophosphate and 89.5 kg of the second filtrate;
[0064] (3-3) The concentration of lithium ions in the second filtrate is determined by ICP-OES detection; the concentration of lithium ions in the second filtrate obtained for the first time is about 1.4 g / L, which is not enough to form precipitation in the subsequent steps; therefore, the second filtrate is used as the first salt solution and returned to step (2-1) for recovery; after repeating the steps between step (2-1) and step (3-3) twice, all 6 waste lithium iron phosphate batteries are recovered; at this time, the total mass of tetra-n-butylammonium hexafluorophosphate recovered is 12.7 kg, and the mass of the second filtrate is 89.8 kg;
[0065] (4) The second filtrate obtained in step (3) is added to 8 kg of 50% by mass sodium carbonate solution to precipitate lithium carbonate with the lithium ions therein, and filtered to obtain 3.0 kg of lithium carbonate solid and 94.5 kg of the third filtrate. The third filtrate can be returned to step (2-1) as the first salt solution for use.
[0066] Example 3
[0067] Example 1 was repeated with the same steps as described, except that, in step (3-1), 7 kg of 1-ethyl-3-methylimidazolium chloride was used as an organic recovery agent; similarly, after repeatedly returning to step (2-1) to soak the waste lithium iron phosphate batteries, the hexafluorophosphate content of the first filtrate reached the standard; after repeating the steps between step (2-1) and step (3-3), the lithium ion content of the second filtrate reached the standard.
[0068] Example 4
[0069] Example 1 was repeated with the same steps, except that in step (1), the first salt solution was 250 kg of a sodium chloride solution with a mass fraction of 15%.
[0070] Comparative Example 1
[0071] Example 1 was repeated with the same steps, except that in step (2-1), a mixed solution of ammonium acetate and sodium acetate with a mass fraction of 3% (the molar ratio of the two was 1:2) was not added to adjust the pH value. As a result, the mass fraction of fluorophosphate in the first filtrate obtained for the first time was only 0.2%. After ten times of processing and recycling of broken waste lithium iron phosphate batteries, the mass fraction of hexafluorophosphate in the first filtrate reached more than 2%.
[0072] Comparative Example 2
[0073] Example 1 was repeated with the same steps, except that in step (3-1), the mass fraction of the tetra-n-butylammonium sulfate aqueous solution was 15%. As a result, the total mass of the recovered tetra-n-butylammonium hexafluorophosphate was 3.9 kg.
[0074] Experimental results verification
[0075] Figure 3 This is the NMR fluorine spectrum of the recovered tetra-n-butylammonium hexafluorophosphate of Example 1. Figure 3 It can be seen that no other fluorine-containing impurities appear and the product purity can reach 95%.
[0076] Figure 4 This is the hydrogen nuclear magnetic resonance spectrum of the first filtrate recovered for the first time in step (2-1) of Example 1, Figure 5The H NMR spectrum of the third filtrate recovered in step (4) of Example 1 shows that, except for the excess tetra-n-butylammonium sulfate added, no other impurities containing hydrogen atoms appear, which is no different from the first salt solution; it is confirmed that it can be repeatedly used as the first salt solution. The detection of Examples 2-4 also shows similar results to Example 1.
[0077] It will be easily understood by those skilled in the art that the above description is only a preferred embodiment of the present application and is not intended to limit the present application. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present application shall be included in the protection scope of the present application.
Claims
1. A method for recycling waste lithium batteries, characterized in that: The following steps are involved: S1. Obtaining a first salt solution; the first salt solution is an inorganic salt solution with a mass fraction of 2.5% to 15%, wherein the inorganic salt is one or more of sodium sulfate, sodium chloride, ammonium sulfate, and ammonium chloride; S2-1. Add the waste lithium battery with the exposed battery cell to the first salt solution and soak it to fully dissolve the hexafluorophosphate and lithium ions in the waste lithium battery; filter out the waste lithium battery to obtain a first filtrate; wherein the mass ratio of the first salt solution to the waste lithium battery is (1 to 5): 1; S2-2. Determine whether the mass fraction of hexafluorophosphate in the first filtrate obtained in the previous step is greater than or equal to a first threshold value, otherwise, let the first filtrate be the first salt solution, return to the step S2-1, and if yes, proceed to the next step; the first threshold value is 2% to 4%; S3-1. Obtaining an organic recovery agent; the organic recovery agent is an organic salt solid or an organic salt solution having a mass fraction of 20% to 60%; the cation of the organic salt is a hydrophobic cation, and the anion of the organic salt is a hydrophilic anion; S3-2. According to the mass ratio of 10: (1 to 3), the organic recovery agent is added to the first filtrate, so that the hexafluorophosphate in the first filtrate forms a hexafluorophosphate precipitate with the hydrophobic cation in the organic recovery agent and is filtered to obtain a second filtrate; S3-3. Determine whether the concentration of lithium ions in the second filtrate obtained in the previous step is greater than or equal to the second threshold value, otherwise, let the second filtrate be the first salt solution, return to step S2-1, and if yes, proceed to the next step; the second threshold value is 4 to 10 g / L; S4. Add 10% to 50% by mass of a carbonate solution to the second filtrate at a mass ratio of (4 to 11): 1, so that the carbonate ions in the carbonate solution and the lithium ions in the second filtrate form a lithium carbonate precipitate; after filtering, a third filtrate and a lithium carbonate precipitate are obtained.
2. The method for recycling waste lithium batteries according to claim 1, characterized in that: In the step S2-2, the mass fraction of the hexafluorophosphate is determined by nuclear magnetic resonance spectroscopy.
3. The method for recycling waste lithium batteries according to claim 1, characterized in that: In the step S3-3, the concentration of the lithium ions is determined by ICP-OES.
4. The method for recycling waste lithium batteries according to claim 1, characterized in that: Before step S2-1, the method further includes: adding an acetate buffer solution so that the pH value of the first salt solution is 7-8.
5. The method for recycling waste lithium batteries according to claim 1, characterized in that: The hydrophobic cation in step S3-1 is one or more of a quaternary ammonium cation, an imidazole cation, a pyridine cation, an oxopiperidinium cation, and a metallocene complex cation.
6. The method for recycling waste lithium batteries according to claim 5, characterized in that: The hydrophobic cation is one or more of a tetra-n-butylammonium ion, a 1-ethyl-3-methylimidazolium cation, an N-butylpyridinium cation, a 2,2,6,6-tetramethyl-1-oxopiperidinium cation or a ferrocenium ion.
7. The method for recycling waste lithium batteries according to claim 1, characterized in that: The hydrophilic anion in step S3-1 is one or more of chloride ion, nitrate ion, sulfate ion, perchlorate ion, and tetrafluoroborate ion.
8. The method for recycling waste lithium batteries according to claim 1, characterized in that: The carbonate in step S4 is one or more of sodium carbonate and ammonium carbonate.
9. Hexafluorophosphate or lithium carbonate obtained by the recovery method according to any one of claims 1 to 8.