Dissimilar metal binuclear catalyst based on Schiff base ligand as well as preparation method and application of dissimilar metal binuclear catalyst

Through the heterometal binuclear catalyst based on Schiff base ligand, the problems of low activity and poor stability of existing catalysts in the copolymerization of olefins and polar monomers are solved, and efficient catalytic effects and high yield polyolefin materials are achieved preparation.

CN118978553AActive Publication Date: 2024-11-19HEFEI UNIV OF TECH
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411065085.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-05
Publication Date
2024-11-19
Estimated Expiration
2044-08-05

AI Technical Summary

Technical Problem

In the copolymerization process of olefins and polar monomers, existing catalysts have problems such as low activity, poor stability and great toxicity, which makes it difficult to effectively improve the performance of polyolefin materials.

Method used

Using a heterometal binuclear catalyst based on Schiff base ligand, the metal active center is protected by introducing sterically hindered groups in the synthesis step, and the electron synergy of the bimetal center is used to improve the stability and activity of the catalyst.

Benefits of technology

The efficient stability and activity of the catalyst are improved, the occurrence of side reactions is reduced, and the copolymerization performance of olefins and polar monomers is significantly improved, with high yields and mild reaction conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118978553A_ABST
    Figure CN118978553A_ABST
Patent Text Reader

Abstract

The invention discloses a dissimilar metal binuclear catalyst based on a Schiff base ligand and a preparation method and application thereof, the structural formula of the dissimilar metal binuclear catalyst based on the Schiff base ligand is as follows: # imgabs0 #, M is Ni or Pd, and R is-H or-CH3. The dissimilar metal binuclear catalyst is used for catalyzing copolymerization of olefin and polar monomers to prepare a functionalized polyolefin material. The dissimilar metal binuclear catalyst is prepared by taking Schiff base with good coordination capability as a ligand and adopting a bimetal strategy. Different coordination environments are realized by regulating and controlling the steric hindrance of the ligand, so that the catalytic performance of the catalyst is optimized; the catalytic performance of the catalyst in the polymerization process, such as catalytic activity, relative molecular mass and distribution of a polymer, copolymerization performance and the like, is favorably regulated and controlled through the synergistic effect of double metal centers.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of catalytic olefins, and in particular to a heterometallic binuclear catalyst based on a Schiff base ligand, and a preparation method and application thereof. Background Art

[0002] Polyolefin materials are ubiquitous in daily life. They are the polymer materials with the largest annual output and the widest applications. However, one of their biggest drawbacks is their non-polar nature. By introducing polar functional groups into the non-polar skeleton of polyolefins, their compatibility with polar materials can be improved, significantly improving the various properties of the materials. Therefore, people expect to copolymerize olefins with polar monomers to obtain functionalized olefins with high performance. In the copolymerization process of olefins and polar monomers, catalysts play an extremely important role. With the development of science and technology, catalysts used to synthesize polyolefin materials are also developing.

[0003] In recent years, the research and development of catalysts has focused on the design of the ligand structure of monometallic catalysts, and the polymerization process has been regulated by strategies such as steric hindrance and electronic effects. With the further development of the research, inspired by multimetallic enzymes in biology, bimetallic catalysts have been developed and show better thermal stability and stereoregularity than mononuclear catalysts. Due to the synergistic, geometric or coupling effects, bimetallic catalysts have better catalytic activity than single metal component catalysts. Different types of active metal centers will further affect the catalytic activity of the catalyst through the interaction with ligands and polar monomers. Summary of the invention

[0004] The object of the present invention is to provide a heterometallic binuclear catalyst based on a Schiff base ligand and a preparation method and application thereof. The heterometallic binuclear catalyst is used to catalyze the copolymerization of olefins and polar monomers.

[0005] In one aspect of the present invention, the present invention provides a heterometallic binuclear catalyst based on a Schiff base ligand. According to an embodiment of the present invention, its structural formula is as follows:

[0006]

[0007] Wherein, M is Ni or Pd, and R is -H or -CH3.

[0008] In another aspect of the present invention, the present invention provides a method for preparing a heterometallic binuclear catalyst based on a Schiff base ligand. According to an embodiment of the present invention, the method comprises the following steps:

[0009] (1) Synthesis of the ligand: In a nitrogen atmosphere, a first reagent, glacial acetic acid, anhydrous ethanol and pyridine-2-carboxaldehyde are heated and stirred, the solvent is removed under vacuum, and then the excess raw materials are removed by vacuum filtration and washing with anhydrous ethanol, and then recrystallization is performed using methanol and petroleum ether, and the product is allowed to stand at low temperature, and the recrystallization solvent is removed under vacuum to obtain a powder product; wherein the first reagent is p-aminophenol or 3,5-dimethyl-4-aminophenol;

[0010] (2) Synthesis of metal complex: Under a nitrogen atmosphere, the powder product is mixed and dissolved with anhydrous ethanol, and then a second reagent is added and stirred at room temperature. After the reaction is completed, the reaction solution is concentrated and solids are precipitated with anhydrous ether, and the supernatant is removed, washed, and dried to obtain a metal complex; wherein the second reagent is palladium dichloride or nickel chloride hexahydrate;

[0011] (3) Synthesis of heterometallic binuclear catalyst: Under a nitrogen atmosphere, the metal complex is mixed and dissolved with dichloromethane, and then vanadium trichloride and triethylamine are added. The mixture is stirred at room temperature, and the solvent is removed in vacuo to obtain a solid powder. The solid powder is recrystallized with dichloromethane and n-hexane, and the heterometallic binuclear catalyst based on the Schiff base ligand is obtained after removing the recrystallization solvent.

[0012] In addition, the preparation method of a heterometallic binuclear catalyst based on a Schiff base ligand according to the above embodiment of the present invention may also have the following additional technical features:

[0013] In some embodiments of the present invention, in step (1), the molar ratio of the first reagent to pyridine-2-carboxaldehyde is 1-1.1:1, and the amount of glacial acetic acid used is 1-2 drops.

[0014] In some embodiments of the present invention, in step (1), the heating and stirring is reflux stirring in an oil bath for 8-12 hours, and the temperature of the oil bath is 76-80°C.

[0015] In some embodiments of the present invention, in step (2), the molar ratio of the second reagent to the powder product is 1:1-1.1.

[0016] In some embodiments of the present invention, in step (2), the stirring time at room temperature is 20-24 hours.

[0017] In some embodiments of the present invention, in step (3), the molar ratio of vanadium trichloride to the metal complex is 1-1.1:1, the amount of triethylamine used is 1-2 drops, and the stirring time at room temperature is 20-24 hours.

[0018] The general synthesis formula of the heterometallic binuclear catalyst based on Schiff base ligand is as follows:

[0019]

[0020] Wherein, M is Ni or Pd, and R is -H or -CH3.

[0021] In another aspect of the present invention, the present invention proposes an application of a heterometallic binuclear catalyst based on a Schiff base ligand. According to an embodiment of the present invention, the heterometallic binuclear catalyst is used to catalyze the copolymerization of olefins and polar monomers to prepare functionalized polyolefin materials.

[0022] In addition, the use of a heterometallic binuclear catalyst based on a Schiff base ligand according to the above embodiment of the present invention may also have the following additional technical features:

[0023] In some embodiments of the present invention, the catalytic copolymerization of olefins and polar monomers comprises the following steps: a co-catalyst, a polar monomer and a heterometallic binuclear catalyst based on a Schiff base ligand are sequentially injected into a water-free and oxygen-free high-pressure reactor while maintaining argon flow, an ethylene gas flow is introduced and stirring is started to carry out polymerization, after a certain period of time, the reaction solution is poured into an ethanol solution containing 4wt%-5wt% hydrochloric acid to precipitate a polymer, and the resulting product is washed with ethanol and then vacuum dried to constant weight to obtain a copolymer of ethylene and a polar monomer.

[0024] In some embodiments of the present invention, the polar monomer is one of 6-chloro-1-hexene, 10-undecene-1-ol, and 10-undecenoic acid methyl ester, the co-catalyst is diethylaluminum chloride, the polymerization is carried out in a toluene solution, the molar ratio of the heterometallic binuclear catalyst based on the Schiff base ligand to the polar monomer is 1:500-1500, the reaction temperature is 25-60°C, and the stirring reaction time is 5-10 min.

[0025] The general formula of the above olefin coordination polymerization is as follows:

[0026]

[0027]

[0028] Wherein, M is Ni or Pd, and R is -H or -CH3.

[0029] Compared with the prior art, the present invention has the following beneficial effects:

[0030] (1) The catalyst synthesis steps in the present invention are relatively simple, the raw materials used are low-priced and easy to obtain, the reaction conditions are relatively mild, the reaction has no by-products and the yield of the product is relatively high.

[0031] (2) In the present invention, the spatial structure of the Schiff base ligand is regulated and the metal active center is protected by introducing a steric group, thereby effectively reducing the occurrence of side reactions and further improving the stability and catalytic activity of the catalyst.

[0032] (3) The present invention adopts a dual metal center strategy, and the two metal centers enhance the catalytic activity of the catalyst through the electronic synergy between the ligands. Compared with single metal catalysts, the poisoning effect of the catalyst is greatly reduced and the catalytic activity is significantly improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 is the H NMR spectrum of the Schiff base ligand 1 of pyridine-2-carboxaldehyde condensed with p-aminophenol in Example 1 of the present invention;

[0034] Figure 2 is the H NMR spectrum of the metal complex 1 in Example 1 of the present invention;

[0035] Figure 3 is an infrared image of the heterometallic binuclear catalyst based on Schiff base ligand in Example 1 of the present invention;

[0036] Figure 4 This is the H NMR spectrum of the Schiff base ligand 2 of pyridine-2-carboxaldehyde condensed with 3,5-dimethyl-4-aminophenol in Example 2 of the present invention;

[0037] Figure 5 is the H NMR spectrum of the metal complex 2 in Example 2 of the present invention;

[0038] Figure 6 is an infrared image of a heterometallic binuclear catalyst based on a Schiff base ligand in Example 2 of the present invention;

[0039] Figure 7 is an infrared image of the ethylene homopolymer in Example 4 of the present invention;

[0040] Figure 8 is an infrared image of the copolymer of ethylene and 6-chloro-1-hexene in Example 5 of the present invention;

[0041] Fig. 9 This is the infrared image of the copolymer of ethylene and 10-undecene-1-ol in Example 6 of the present invention. DETAILED DESCRIPTION

[0042] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0043] Example 1

[0044] A method for preparing a heterometallic binuclear catalyst based on a Schiff base ligand comprises the following steps:

[0045] (1) p-Aminophenol (1.09 g, 10 mmol) was weighed into a 250 mL round-bottom flask. Under nitrogen protection, anhydrous ethanol (20 mL), glacial acetic acid (0.1 mL) and pyridine-2-carboxaldehyde (1.07 g, 10 mmol) were added in sequence. The double-necked flask was placed in an oil bath and refluxed with stirring for 12 h. After the solvent was removed under vacuum, it was filtered under reduced pressure and washed with anhydrous ethanol. The filter cake was dissolved in a small amount of slightly hot methanol, and petroleum ether was added to precipitate a yellow powder. The mixture was placed in a refrigerator at 0°C and allowed to stand for 4 h. The solvent was removed under vacuum to obtain 1.39 g of a yellow powder of pyridine-2-carboxaldehyde condensed p-aminophenol Schiff base ligand, with a yield of 70.2%.

[0046] (2) Pyridine-2-carboxaldehyde condensed p-aminophenol Schiff base ligand 1 (198 mg, 1 mmol) was weighed into a 100 mL round-bottom flask, 10 mL of methanol was added thereto to dissolve, and then palladium dichloride (177 mg, 1 mmol, dissolved in 10 mL of methanol) was added thereto, the system was replaced with a nitrogen atmosphere, stirred at room temperature for 24 h to ensure that the reaction was complete, and then transferred to a single-necked bottle, the reaction solution was concentrated to 3 mL, anhydrous ether was added to precipitate the product and washed 3 times, and the solvent was removed in vacuo to obtain a metal complex 1 (yellow-brown powder 315 mg, yield 84%);

[0047] (3) In a glove box, weigh the metal complex 1 (37.5 mg, 0.1 mmol) and place it in a 20 mL screw-capped bottle. Add dichloromethane (10 mL), VCl3 (15.7 mg, 0.1 mmol), and triethylamine (10 mg). Stir at room temperature for 24 h and stop the reaction. The color of the solution changes from yellow to yellow-brown. After the reaction is completed, transfer the product to a single-mouth bottle and remove the solvent under reduced pressure to obtain a yellow-brown solid. Add a small amount of DCM until the product is completely dissolved, then add 15 mL of n-hexane to precipitate the product, remove the supernatant, and remove the solvent under reduced pressure to obtain a heterometallic binuclear catalyst cat.1 based on a Schiff base ligand (23 mg of yellow-brown powder, yield 46.3%). Its structural formula is shown below:

[0048]

[0049] Example 2

[0050] A method for preparing a heterometallic binuclear catalyst based on a Schiff base ligand comprises the following steps:

[0051] (1) Weigh 3,5-dimethyl-4-aminophenol (1.37 g, 10 mmol) into a 250 mL round-bottom flask. Under nitrogen protection, add anhydrous ethanol (20 mL), glacial acetic acid (0.1 mL) and pyridine-2-carboxaldehyde (1.07 g, 10 mmol) in sequence. Place the double-necked flask in an oil bath and reflux with stirring for 12 h. Remove the solvent in vacuo and then filter under reduced pressure and wash with anhydrous ethanol. Dissolve the filter cake in a small amount of slightly hot methanol. Add petroleum ether to precipitate a dark green powder. Place the mixture in a refrigerator at 0°C and let stand for 4 h. Remove the solvent in vacuo to obtain 2.06 g of dark green powder pyridine-2-carboxaldehyde condensate 3,5-dimethyl-4-aminophenol Schiff base ligand II. The yield is 91.2%.

[0052] (2) Pyridine-2-carboxaldehyde 3,5-dimethyl-4-aminophenol Schiff base ligand (226 mg, 1 mmol) was weighed into a 100 mL round-bottom flask, 10 mL of methanol was added to dissolve, and then palladium dichloride (177 mg, 1 mmol, dissolved in 10 mL of methanol) was added to replace the system with nitrogen atmosphere, stirred at room temperature for 24 h to ensure the reaction was complete, and then transferred to a single-mouth bottle, the reaction solution was concentrated to 3 mL, anhydrous ether was added to precipitate the product and washed 3 times, and the solvent was removed in vacuo to obtain metal complex II (green powder 317 mg, yield 78.7%);

[0053] (3) In a glove box, weigh the metal complex II (80.6 mg, 0.2 mmol) and place it in a 20 mL screw-capped bottle. Add dichloromethane (10 mL), VCl3 (31.4 mg, 0.2 mmol), and triethylamine (10 mg). Stir at room temperature for 24 h and stop the reaction. The color of the solution changes from purple to coffee brown. After the reaction is completed, transfer the product to a single-mouth bottle and remove the solvent under reduced pressure to obtain a dark brown solid. Add a small amount of DCM until the product is completely dissolved, then add 15 mL of n-hexane to precipitate the product, remove the supernatant, and remove the solvent under reduced pressure to obtain a heterometallic binuclear catalyst cat.2 based on a Schiff base ligand (96 mg of dark brown powder, yield 91.4%). Its structural formula is shown below:

[0054]

[0055] Example 3

[0056] A method for preparing a heterometallic binuclear catalyst based on a Schiff base ligand comprises the following steps:

[0057] (1) Weigh 3,5-dimethyl-4-aminophenol (1.37 g, 10 mmol) into a 250 mL round-bottom flask. Under nitrogen protection, add anhydrous ethanol (20 mL), glacial acetic acid (0.1 mL) and pyridine-2-carboxaldehyde (1.07 g, 10 mmol) in sequence. Place the double-necked flask in an oil bath and reflux with stirring for 12 h. Remove the solvent in vacuo and then filter under reduced pressure and wash with anhydrous ethanol. Dissolve the filter cake in a small amount of slightly hot methanol. Add petroleum ether to precipitate a dark green powder. Place the mixture in a refrigerator at 0°C and let stand for 4 h. Remove the solvent in vacuo to obtain 2.06 g of dark green powder pyridine-2-carboxaldehyde condensate 3,5-dimethyl-4-aminophenol Schiff base ligand II. The yield is 91.2%.

[0058] (2) Pyridine-2-carboxaldehyde 3,5-dimethyl-4-aminophenol Schiff base ligand II (226 mg, 1 mmol) was weighed into a 100 mL round-bottom flask, 10 mL of methanol was added thereto to dissolve, and then nickel chloride hexahydrate (237 mg, 1 mmol, dissolved in 10 mL of methanol) was added thereto, the system was replaced with a nitrogen atmosphere, stirred at room temperature for 24 h to ensure that the reaction was complete, and then transferred to a single-mouth bottle, the reaction solution was concentrated to 3 mL, anhydrous ether was added to precipitate the product and washed 3 times, and the solvent was removed in vacuo to obtain metal complex III (orange-yellow powder 293 mg, yield 82.4%);

[0059] (3) In a glove box, weigh the metal complex three (106.7 mg, 0.3 mmol) and place it in a 20 mL screw-capped bottle. Add dichloromethane (10 mL), VCl3 (47.1 mg, 0.3 mmol), and triethylamine (10 mg). Stir at room temperature for 24 h and stop the reaction. The color of the solution changes from purple to brown-yellow. After the reaction is completed, transfer the product to a single-mouth bottle and remove the solvent under reduced pressure to obtain a brown-yellow solid. Add a small amount of DCM until the product is completely dissolved, then add 15 mL of n-hexane to precipitate the product, remove the supernatant, and remove the solvent under reduced pressure to obtain a heterometallic binuclear catalyst cat.3 based on a Schiff base ligand (brown-yellow powder 140 mg, yield 98.02%). Its structural formula is shown below:

[0060]

[0061] Example 4

[0062] The ethylene homopolymerization method comprises the following steps:

[0063] In the glove box, weigh 2 μmol of the heterometallic binuclear catalyst cat.1 (main catalyst) based on Schiff base ligand prepared in Example 1 into a 10 mL schlenk bottle, add 2 mL of dichloromethane to dissolve, and add 3 mL of toluene; weigh 1 mmol of the co-catalyst diethylaluminum chloride into a 25 mL schlenk bottle, add 5 mL of toluene; ensure that the total volume of toluene is 10 mL. Seal the two schlenk bottles with sealing film and take them out of the glove box, connect the double-row pipes, replace the gas in the pipeline, and after three replacements, use a syringe to inject the co-catalyst diethylaluminum chloride and the catalyst cat.1 into the reactor in sequence while ensuring the flow of argon. Dry the reactor in an oven for 12 hours before use and evacuate.

[0064] Ethylene gas at a pressure of 4 atm was introduced into the kettle, the valve on the top of the kettle was opened, the nitrogen in the kettle was removed, and the magnetic stirring was turned on to start the reaction. The reaction time was 10 minutes. After the reaction was completed, the main valve of the ethylene cylinder was closed, and the pressure was released and the kettle was disassembled. The reaction liquid in the kettle was poured into 50 mL of ethanol solution containing 5% hydrochloric acid, stirred for 12 hours, and the white solid was collected and vacuum dried at 50°C to constant weight to obtain ethylene homopolymer.

[0065] Example 5

[0066] The copolymerization method of ethylene and 6-chloro-1-hexene comprises the following steps:

[0067] In the glove box, weigh 2 μmol of the heterometallic binuclear catalyst cat.2 (main catalyst) based on Schiff base ligand prepared in Example 2 in a 10 mL schlenk bottle, add 2 mL of dichloromethane to dissolve; weigh 1 mmol of the co-catalyst diethylaluminum chloride in a 25 mL schlenk bottle, add 5 mL of toluene; weigh 6-chloro-1-hexene (236 mg, 2.0 mmol) in a 25 mL schlenk bottle, add 5 mL of toluene, and ensure that the total volume of toluene is 10 mL. Seal the three schlenk bottles with sealing film and take them out of the glove box, connect the double-row pipe, replace the gas in the pipeline, and replace it three times. In the case of ensuring argon gas, use a syringe to inject the co-catalyst diethylaluminum chloride, polar monomer 6-chloro-1-hexene, and main catalyst cat.2 into the reactor in sequence. The reactor was dried in an oven for 12 hours before use and evacuated.

[0068] Ethylene gas at a pressure of 4 atm was introduced into the kettle, the valve above the kettle was opened, the nitrogen in the kettle was removed, and the magnetic stirring was turned on to start the reaction. The reaction time was 10 minutes. After the reaction was completed, the main valve of the ethylene cylinder was closed, and the pressure was released and the kettle was disassembled. The reaction liquid in the kettle was poured into 50 mL of ethanol solution containing 5% hydrochloric acid, stirred for 12 hours, and the white solid was collected and vacuum dried at 50°C to constant weight to obtain a copolymer of ethylene and 6-chloro-1-hexene.

[0069] Example 6

[0070] The copolymerization method of ethylene and 10-undecene-1-ol comprises the following steps:

[0071] In the glove box, weigh 2 μmol of the heterometallic binuclear catalytic cat.2 (main catalyst) based on Schiff base ligand prepared in Example 2 in a 10mL schlenk bottle, add 2mL of dichloromethane to dissolve; weigh 1mmol of the cocatalyst diethylaluminum chloride in a 25mL schlenk bottle, add 5mL of toluene; weigh 10-undecene-1-ol (340mg, 2.0mmol) in a 25mL schlenk bottle, add 5mL of toluene, and ensure that the total volume of toluene is 10mL. Seal the three schlenk bottles with sealing film and take them out of the glove box, connect the double-row pipe, replace the gas in the pipeline, and replace it three times. In the case of ensuring argon gas, use a syringe to inject the cocatalyst diethylaluminum chloride, polar monomer 10-undecene-1 alcohol, and main catalyst cat.2 into the reactor in sequence. The reactor was dried in an oven for 12h before use and evacuated.

[0072] Ethylene gas at a pressure of 4 atm was introduced into the kettle, the valve above the kettle was opened, the nitrogen in the kettle was removed, and the magnetic stirring was turned on to start the reaction. The reaction time was 10 minutes. After the reaction was completed, the main valve of the ethylene cylinder was closed, and the pressure was released and the kettle was disassembled. The reaction liquid in the kettle was poured into 50 mL of ethanol solution containing 5% hydrochloric acid, stirred for 12 hours, and the white solid was collected and vacuum dried at 50°C to constant weight to obtain a copolymer of ethylene and 10-undecene-1-ol.

[0073] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the structure of the present invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.

Claims

1. A heterometallic binuclear catalyst based on a Schiff base ligand, characterized in that: The structural formula is as follows: Wherein, M is Ni or Pd, and R is -H or -CH3.

2. A method for preparing a heterometallic binuclear catalyst based on a Schiff base ligand according to claim 1, characterized in that: The following steps are involved: (1) Synthesis of the ligand: In a nitrogen atmosphere, a first reagent, glacial acetic acid, anhydrous ethanol and pyridine-2-carboxaldehyde are heated and stirred, the solvent is removed under vacuum, and then the excess raw materials are removed by vacuum filtration and washing with anhydrous ethanol, and then recrystallization is performed using methanol and petroleum ether, and the product is allowed to stand at low temperature, and the recrystallization solvent is removed under vacuum to obtain a powder product; wherein the first reagent is p-aminophenol or 3,5-dimethyl-4-aminophenol; (2) Synthesis of metal complex: Under a nitrogen atmosphere, the powder product is mixed and dissolved with anhydrous ethanol, and then a second reagent is added and stirred at room temperature. After the reaction is completed, the reaction solution is concentrated and solids are precipitated with anhydrous ether, and the supernatant is removed, washed, and dried to obtain a metal complex; wherein the second reagent is palladium dichloride or nickel chloride hexahydrate; (3) Synthesis of heterometallic binuclear catalyst: Under a nitrogen atmosphere, the metal complex is mixed and dissolved with dichloromethane, and then vanadium trichloride and triethylamine are added. The mixture is stirred at room temperature, and the solvent is removed in vacuo to obtain a solid powder. The solid powder is recrystallized with dichloromethane and n-hexane, and the heterometallic binuclear catalyst based on the Schiff base ligand is obtained after removing the recrystallization solvent.

3. The method for preparing a heterometallic binuclear catalyst based on a Schiff base ligand according to claim 2, characterized in that: In the step (1), the molar ratio of the first reagent to pyridine-2-carboxaldehyde is 1-1.1:

1.

4. The method for preparing a heterometallic binuclear catalyst based on a Schiff base ligand according to claim 2, characterized in that: In the step (1), the heating and stirring is performed by reflux stirring in an oil bath for 8-12 hours, and the temperature of the oil bath is 76-80°C.

5. The method for preparing a heterometallic binuclear catalyst based on a Schiff base ligand according to claim 2, characterized in that: In the step (2), the molar ratio of the second reagent to the powder product is 1:1-1.

1.

6. The method for preparing a heterometallic binuclear catalyst based on a Schiff base ligand according to claim 2, characterized in that: In the step (2), the stirring time at room temperature is 20-24 hours.

7. The method for preparing a heterometallic binuclear catalyst based on a Schiff base ligand according to claim 2, characterized in that: In the step (3), the molar ratio of vanadium trichloride to the metal complex is 1-1.1:1, and the stirring time at room temperature is 20-24 hours.

8. An application of the heterometallic binuclear catalyst based on Schiff base ligand according to claim 1, characterized in that: The heterometallic binuclear catalyst is used to catalyze the copolymerization of olefins and polar monomers to prepare functionalized polyolefin materials.

9. The use of a heterometallic binuclear catalyst based on a Schiff base ligand according to claim 8, characterized in that: The catalytic copolymerization of olefins and polar monomers comprises the following steps: a co-catalyst, a polar monomer and a heterometallic binuclear catalyst based on a Schiff base ligand are sequentially injected into a water-free and oxygen-free high-pressure reactor while maintaining argon flow, an ethylene gas flow is introduced and stirring is started to carry out polymerization, after a certain period of time, the reaction liquid is poured into an ethanol solution containing 4wt%-5wt% hydrochloric acid to precipitate a polymer, and the obtained product is washed with ethanol and then vacuum dried to constant weight to obtain a copolymer of ethylene and the polar monomer.

10. The use of a heterometallic binuclear catalyst based on a Schiff base ligand according to claim 9, characterized in that: The polar monomer is one of 6-chloro-1-hexene, 10-undecene-1-ol, and 10-undecenoic acid methyl ester, the co-catalyst is diethylaluminum chloride, the polymerization is carried out in a toluene solution, the molar ratio of the heterometallic binuclear catalyst based on the Schiff base ligand to the polar monomer is 1:500-1500, the reaction temperature is 25-60°C, and the stirring reaction time is 5-10 minutes.

Citation Information

Patent Citations

  • Binuclear vanadium catalyst as well as preparation method and application thereof

    CN114395058A

  • Trivalent vanadium complex catalyst containing bidentate ligand as well as preparation method and application of trivalent vanadium complex catalyst

    CN116874648A

  • Double-center Schiff base catalyst, preparation method thereof and preparation method of polyglycolic acid

    CN117343304A

  • Transition metal complexes in the controlled synthesis of polyolefins substituted with functional groups