Polymer fluid loss agent for well cementation sulphoaluminate cement and preparation method of polymer fluid loss agent
By using reaction monomers such as sodium methacrylate sulfaaluminate cement to form a polymer film, the excessive water loss of the cemented sulfaaluminate cement is solved and the excessive water loss of the cemented sulfaaluminate cement slurry is solved. The problem of difficult to adjust the thickening time has achieved efficient and safe cementing construction in low-temperature environments.
Patent Information
- Application Number
- CN202411268413.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-11
- Publication Date
- 2024-11-19
AI Technical Summary
The existing water loss-reducing agent has poor water loss control effect in cementing sulfa aluminate cement slurry, difficult to adjust the thickening time, and poor settlement stability, resulting in unqualified cementing quality, especially in low-temperature environments, which is difficult to meet safe construction requirements. .
Polymers prepared by aqueous radical polymerization reaction such as sodium methacrylic sulfonate, vinyl glycol ether, N-vinylformamide and acryloyloxyethyltrimethylammonium chloride are reduced by water The agent forms a polymer film on the surface of sulfoaluminate cement, controls the amount of water loss and has a retarding effect, and improves the thickening performance.
Linear water loss control of sulfur aluminate cement is achieved, the amount of retarder is reduced, the safety and quality of cementing construction is ensured, and it is suitable for cementing wells in oil and gas reservoirs in low-temperature environments.
Smart Images

Figure CN118978637A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of oil and gas well cementing, and in particular to a polymer fluid loss reducer for cementing sulphoaluminate cement and a preparation method thereof. Background Art
[0002] Sulphoaluminate cement has the advantages of fast hardening, early strength, low alkalinity, waterproofness, good frost resistance, good durability, low shrinkage, and resistance to CO2 corrosion. It is not only widely used in the construction field and road repair projects, but also has important applications in the field of oil and gas well cementing projects.
[0003] In the field of oil and gas well cementing, sulphoaluminate cement is mainly used in cementing environments with temperatures ranging from minus to 60°C, such as in cementing projects in low-temperature oil and gas reservoirs such as shallow surface, frozen layers, and deep water. In order to ensure the cementing quality of low-temperature oil and gas reservoirs and reduce waiting costs, cementing slurry needs to have the characteristics of fast hardening and early strength while meeting construction performance. Therefore, sulphoaluminate cement is often used as the main gelling material for cementing slurry. In addition, in the treatment of well leakage in oil and gas wells, the advantages of sulphoaluminate cement with fast hardening and early strength are also used to quickly plug leaks.
[0004] In the cementing environment, in order to ensure the safety of cementing construction and improve the quality of cementing, it is necessary to strictly control the thickening time and water loss of sulphoaluminate cement. For sulphoaluminate cement, the effective retarder is boric acid, but there is no special fluid loss reducer at present. In order to control the water loss of cementing sulphoaluminate cement slurry, polyacrylamide, cellulose ether and other thickening materials are often used as fluid loss reducers, but the water loss control effect is not satisfactory. The API water loss of cement slurry is still large, even up to 100mL or more, which is difficult to meet the requirements of tail pipe cementing. The existing cement cement fluid loss reducers are mainly AMPS / AM (2-acrylamide-2-methylpropanesulfonic acid / acrylamide) copolymers. This type of copolymer is developed based on the composition characteristics of silicate cement and is mainly suitable for G-grade, D-grade and other oil well cements. Therefore, it is not applicable to cementing sulphoaluminate cement. This is because the cement mineral composition of sulphoaluminate cement and silicate cement is quite different. AMPS / AM copolymers have many adverse effects when used in cementing sulphoaluminate cement. Specifically, AMPS / AM polymer fluid loss reducers for oil well cement have a strong dispersing effect on sulphoaluminate cement, causing the cement slurry to become very thin, with an increase in segregated liquid, unstable density, a large amount of water loss in the cement slurry, and poor sedimentation stability. This cannot ensure safe and effective sealing of the cement sheath, which in turn affects the quality of cementing and may even lead to unqualified cementing quality.
[0005] Aiming at the problems that the existing fluid loss reducer has poor water loss control effect in cementing sulphoaluminate cement slurry, poor adaptability to boric acid, difficult adjustment of cement slurry thickening time and poor sedimentation stability, the present invention provides a polymer fluid loss reducer suitable for cementing sulphoaluminate cement to ensure the comprehensive performance and cementing quality of sulphoaluminate cement during cementing. Summary of the invention
[0006] The object of the present invention is to provide a polymer fluid loss reducer for cementing sulphoaluminate cement and a preparation method thereof, so as to solve the problems of poor sedimentation stability and difficult adjustment of thickening time of sulphoaluminate cement slurry caused by excessive water loss, realize safe cementing construction of low-temperature oil and gas reservoirs, and thus ensure efficient and safe exploitation of low-temperature oil and gas resources such as deep water, frozen layer and shallow layer.
[0007] To achieve the above purpose, the technical solution adopted by the present invention is as follows:
[0008] The present invention discloses a polymer fluid loss reducer for cementing sulphoaluminate cement, which comprises, by weight:
[0009]
[0010] The present invention uses sodium methyl propylene sulfonate, vinyl glycol ether, N-vinyl formamide and acryloyloxyethyl trimethyl ammonium chloride as reaction monomers, adds initiator and chain transfer agent, and prepares polymer fluid loss reducer for cementing sulphoaluminate cement through free radical polymerization of aqueous solution. The polymer fluid loss reducer not only contains a large number of polar groups such as -OH, -CO-NH2, -O-, but also contains a large number of -SO3 - Anionic groups and quaternary ammonium cationic groups. Polymers containing functional groups such as -OH, -CO-NH2 and -O- have good film-forming properties and can be effectively adsorbed on the surface of sulphoaluminate cement particles to form a thin and tough polymer film, which plays a good role in controlling water loss. In addition, -SO3 - Anion and -R4N + The quaternary ammonium cationic group has a good affinity for sulphoaluminate cement particles and can be adsorbed on the surface of sulphoaluminate cement particles through complexation, further increasing the toughness and strength of the polymer film, thereby improving the water loss control effect of the polymer film. The polymer film formed on the surface of sulphoaluminate cement will break under the action of the osmotic pressure difference between the inside and the outside as the hydration reaction proceeds, allowing the hydration reaction of sulphoaluminate cement to proceed normally, so it does not affect its early strength. Furthermore, the polymer contains -O- and -OH groups that have a certain retarding effect on sulphoaluminate, which can react with Ca in the liquid phase. 2+The complex is formed by complexation, so that a thick and amorphous complex film is formed on the surface of sulphoaluminate cement, which can delay the hydration of sulphoaluminate cement to a certain extent, so that the polymer fluid loss reducer has a certain retarding effect and can reduce the dosage of the retarder to a certain extent.
[0011] In the present invention, the amount of sodium methacrylate sulfonate is 25 to 45 parts; for example, 20 parts, 21 parts, 22 parts, 23 parts, 24 parts, 25 parts, 26 parts, 27 parts, 28 parts, 29 parts, 30 parts, 31 parts, 32 parts, 33 parts, 34 parts, 35 parts, 36 parts, 37 parts, 38 parts, 39 parts, 40 parts, 41 parts, 42 parts, 43 parts, 44 parts, and 45 parts.
[0012] In the present invention, the amount of vinyl glycol ether is 20 to 35 parts; for example, 20 parts, 21 parts, 22 parts, 23 parts, 24 parts, 25 parts, 26 parts, 27 parts, 28 parts, 29 parts, 30 parts, 31 parts, 32 parts, 33 parts, 34 parts, and 35 parts.
[0013] In the present invention, the amount of N-vinylformamide is 20 to 30 parts; for example, 20 parts, 21 parts, 22 parts, 23 parts, 24 parts, 25 parts, 26 parts, 27 parts, 28 parts, 29 parts, and 30 parts.
[0014] In the present invention, the amount of acryloyloxyethyltrimethylammonium chloride is 5 to 10 parts; for example, 5 parts, 6 parts, 7 parts, 8 parts, 9 parts, and 10 parts.
[0015] In the present invention, the initiator is 2 to 3 parts; for example, 2 parts, 2.5 parts, 3 parts.
[0016] In the present invention, the chain transfer agent is 3 to 5 parts; for example, 3 parts, 3.5 parts, 4 parts, 4.5 parts, 5 parts.
[0017] In some implementations of the present invention, the structural unit composition of the polymer fluid loss additive comprises a random copolymer of formula I, formula II, formula III and formula IV and a number average molecular weight of 20,000 to 40,000.
[0018] In some implementations of the present invention, in the structural units of the polymer fluid loss additive, the mass percentages of general formula I, general formula II, general formula III and general formula IV are: I = 25-45%, II = 25-35%, III = 20-30%, IV = 5-10%, respectively.
[0019] In the present invention, the mass percentage of the random copolymer of general formula I is 25-45%, for example, 25%, 26%, 27%, 28%, 29%, 30%, 31%, 32%, 33%, 34%, 35%, 36%, 37%, 38%, 39%, 40%, 41%, 42%, 43%, 44%, 45%.
[0020] In the present invention, the mass percentage of the random copolymer of formula II is 25-35%, for example, 25%, 26%, 27%, 28%, 29%, 30%, 31%, 32%, 33%, 34%, 35%.
[0021] In the present invention, the mass percentage of the random copolymer of formula III is 20-30%, for example, 20%, 21%, 22%, 23%, 24%, 25%, 26%, 27%, 28%, 29%, 30%.
[0022] In the present invention, the mass percentage of the random copolymer of formula IV is 5-10%, for example, 5%, 6%, 7%, 8%, 9%, 10%.
[0023] In some implementations of the present invention, the purity of the sodium methyl methacrylate sulfonate and the N-vinyl formamide are both analytically pure.
[0024] In some implementations of the present invention, the active ingredient content of the vinyl glycol ether is 99%.
[0025] In some implementations of the present invention, the acryloyloxyethyltrimethylammonium chloride is an aqueous solution with a mass fraction of 80%.
[0026] In some implementations of the present invention, the initiator is a peroxide or a mixture of several peroxides, and the peroxide includes potassium persulfate, sodium persulfate, and ammonium persulfate. Preferably, the purity of the peroxide is analytical grade.
[0027] In some implementations of the present invention, the chain transfer agent is one or a mixture of lignin xanthate, isopropanol, and sodium hypophosphite. Preferably, the purity of the lignin xanthate, isopropanol, and sodium hypophosphite is analytically pure.
[0028] The present invention also discloses a method for preparing a polymer fluid loss reducer for cementing sulphoaluminate cement, comprising the following steps:
[0029] S1. At room temperature, 25 to 45 parts of sodium methacrylate sulfonate and 25 to 35 parts of vinyl glycol ether are uniformly dispersed in 25 to 50 parts of water to obtain a first mixed solution;
[0030] S2. At room temperature, 20 to 30 parts by weight of N-vinyl formamide and 5 to 10 parts by weight of acryloyloxyethyl trimethyl ammonium chloride are uniformly dispersed in 70 to 85 parts of water to obtain a second mixed solution;
[0031] S3. At room temperature, 2 to 3 parts of the initiator are uniformly dispersed in 20 to 22 parts of water by weight to obtain a third mixed solution; 3 to 5 parts of the chain transfer agent are uniformly dispersed in 20 to 22 parts of water to obtain a fourth mixed solution;
[0032] S4, uniformly mixing the first mixed liquid and the second mixed liquid to obtain a fifth mixed liquid; introducing nitrogen into a reactor with a stirring device to remove oxygen in the reactor, and maintaining a nitrogen atmosphere, transferring the fifth mixed liquid to the reactor, heating and stirring the fifth mixed liquid to 65° C.; sequentially adding the third mixed liquid and the fourth mixed liquid dropwise to the fifth mixed liquid at a constant pressure to obtain a sixth mixed liquid;
[0033] S5, stirring and keeping the sixth mixed solution at 65° C. for 2-3 hours, then naturally cooling to 50° C., stirring and keeping the solution at 50° C. for 1-2 hours, and then taking the solution out of the reactor to obtain a seventh mixed solution;
[0034] S6, adding 100 parts of anhydrous ethanol to the seventh mixed solution, washing and purifying for multiple times and filtering out the anhydrous ethanol to obtain a white viscous substance, and vacuum freeze-drying the white viscous substance to obtain the polymer fluid loss reducer.
[0035] In some implementations of the present invention, in S3, the dripping speed of the third mixed liquid and the fourth mixed liquid is 30 drops / min; in S4, a 20% by mass NaOH solution is used to adjust the pH of the fifth mixed liquid to 6-7; in S5, the stirring speed at 65°C is 600r / min, and the stirring speed at 50°C is 300r / min; in S6, the temperature of vacuum freeze drying is -10°C and the time is 8h.
[0036] Compared with the prior art, the present invention has the following beneficial effects:
[0037] 1. Compared with the existing fluid loss reducers, the polymer fluid loss reducer provided by the present invention has a good linear water loss control effect on sulphoaluminate cement, that is, with the increase of the dosage, the API water loss of the sulphoaluminate cement slurry for cementing shows a linear decrease, and there is no problem of dosage inversion and dosage sensitivity.
[0038] 2. The polymer fluid loss reducer of the present invention has a simple preparation process and a wide range of raw material sources, and can have a good water loss control effect on sulphoaluminate cement with a small amount of addition. In addition, the polymer fluid loss reducer provided by the present invention has good low-temperature solubility, can be quickly dissolved in low-temperature cementing environments such as frozen layers and deep water, and can quickly exert its good water loss control effect in cementing sulphoaluminate cement slurry.
[0039] 3. The polymer fluid loss reducer of the present invention has a retarding effect, which can reduce the dosage of the sulphoaluminate cement retarder and reduce the cost of cementing materials. In addition, the fluid loss reducer has basically no adverse effect on the early strength and late strength of sulphoaluminate cement.
[0040] 4. The polymer fluid loss reducer of the present invention has good compatibility with boric acid, a special retarder for sulphoaluminate cement. The use of these additives can form a cementing sulphoaluminate cement slurry with excellent comprehensive properties such as no free liquid, good rheological properties, small water loss, adjustable thickening time, and high early strength, thereby improving the cementing quality of low-temperature oil and gas reservoirs, thereby ensuring the efficient and safe exploitation of oil and gas resources in low-temperature reservoirs such as deep water, frozen layers, and shallow layers. BRIEF DESCRIPTION OF THE DRAWINGS
[0041] Figure 1 It is a structural formula diagram of the polymer fluid loss reducer for cementing sulphoaluminate cement of the present invention.
[0042] Figure 2 The infrared spectrum of the polymer fluid loss reducer for cementing sulphoaluminate cement of the present invention.
[0043] Figure 3 The thickening curve of the cementing sulphoaluminate cement slurry mixed with the polymer fluid loss reducer for cementing sulphoaluminate cement of the present invention is shown in FIG.
[0044] Figure 4 The thickening curve of the cementing sulphoaluminate cement slurry mixed with the prior art fluid loss reducer is shown in FIG.
[0045] Figure 5 This is the thickening curve of the cementing sulphoaluminate cement slurry without any fluid loss additive. DETAILED DESCRIPTION
[0046] In order to make the purpose, technical scheme and advantages of the present invention clearer, the present invention is further described in detail below in conjunction with the embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in the field without making creative work are within the scope of protection of the present invention. The terms "first", "second", etc. in the present invention are used to distinguish different objects, rather than to describe a specific order.
[0047] In the embodiment of the present invention, the structural unit composition of the polymer fluid loss additive comprises a random copolymer of general formulas Ⅰ, Ⅱ, Ⅲ and Ⅳ and a number average molecular weight of 20,000 to 40,000.
[0048] In the embodiment of the present invention, in the structural unit of the polymer fluid loss additive, the mass percentages of general formulas Ⅰ, Ⅱ, Ⅲ and Ⅳ are respectively: Ⅰ=25-45%, Ⅱ=25-35%, Ⅲ=20-30%, Ⅳ=5-10%.
[0049] In the embodiment of the present invention, the purity of the sodium methyl methacrylate sulfonate and the N-vinyl formamide are both analytically pure.
[0050] In the embodiment of the present invention, the effective component content of the vinyl glycol ether is 99%.
[0051] In the embodiment of the present invention, the acryloyloxyethyltrimethylammonium chloride is an aqueous solution with a mass fraction of 80%.
[0052] In the embodiment of the present invention, the initiator is a peroxide or a mixture of several peroxides, and the peroxide includes potassium persulfate, sodium persulfate, and ammonium persulfate.
[0053] In the embodiment of the present invention, the chain transfer agent is one or a mixture of lignin xanthate, isopropyl alcohol, and sodium hypophosphite.
[0054] Example 1
[0055] As a preferred embodiment of the present invention, the sulphoaluminate cement polymer fluid loss reducer for well cementing disclosed in this embodiment has the components shown in Table 1.
[0056] Table 1 Specific components of polymer fluid loss reducer in Example 1
[0057] Raw material name Weight parts / parts Sodium Methylpropene Sulfonate 45 Vinyl glycol ether 25 N-vinyl formamide 20 Acryloyloxyethyltrimethylammonium chloride 5 Initiator 2 Chain transfer agent 3
[0058] In this embodiment, a sulphoaluminate cement polymer fluid loss reducer for cementing is prepared according to the components in Table 1:
[0059] S1. At room temperature, 45 parts of sodium methacrylate sulfonate and 25 parts of vinyl glycol ether are uniformly dispersed in 30 parts of water by ultrasonication to obtain a first mixed solution;
[0060] S2. At room temperature, 20 parts of N-vinyl formamide and 5 parts of acryloyloxyethyl trimethyl ammonium chloride are uniformly dispersed in 75 parts of water by ultrasonication to obtain a second mixed solution;
[0061] S3. At room temperature, 2 parts of the initiator are uniformly dispersed in 22 parts of water to obtain a third mixed solution; 3 parts of the chain transfer agent are uniformly dispersed in 22 parts of water to obtain a fourth mixed solution;
[0062] S4, after uniformly mixing the first mixed liquid and the second mixed liquid, a fifth mixed liquid is obtained, and a 20% by mass NaOH solution is used to adjust the pH of the fifth mixed liquid to 6-7; nitrogen is introduced into a reactor with a stirring device to remove oxygen in the reactor, and the nitrogen atmosphere is maintained, the fifth mixed liquid is transferred to the reactor, and the fifth mixed liquid is heated and stirred to 65° C. The stirring speed is set to 600 r / min; the third mixed liquid and the fourth mixed liquid are sequentially added dropwise to the fifth mixed liquid at a constant pressure to obtain a sixth mixed liquid, and the dropping speed of the third mixed liquid and the fourth mixed liquid is 30 drops / min;
[0063] S5, stirring and keeping the sixth mixed solution at 65° C. for 2-3 hours, with the stirring speed set to 600 r / min, then naturally cooling to 50° C., with the stirring speed set to 300 r / min, and stirring and keeping the solution at 50° C. for 1-2 hours, then taking it out from the reactor to obtain a seventh mixed solution;
[0064] S6. Add 100 parts of anhydrous ethanol to the seventh mixed solution, wash and purify for multiple times and filter out the anhydrous ethanol to obtain a white viscous substance. The white viscous substance is vacuum freeze-dried to obtain a polymer fluid loss reducer. The vacuum freeze-drying temperature is -10°C and the time is 8 hours.
[0065] Example 2
[0066] As a preferred embodiment of the present invention, the sulphoaluminate cement polymer fluid loss reducer for cementing disclosed in this embodiment has the components shown in Table 2.
[0067] Table 2 Specific components of polymer fluid loss additive in Example 2
[0068] Raw material name Weight parts / parts Sodium Methylpropene Sulfonate 33 Vinyl glycol ether 28 N-vinyl formamide 25 Acryloyloxyethyltrimethylammonium chloride 7.5 Initiator 2.5 Chain transfer agent 4
[0069] In this embodiment, a sulphoaluminate cement polymer fluid loss reducer for cementing was prepared according to the components in Table 2:
[0070] S1. At room temperature, 33 parts of sodium methacrylate sulfonate and 28 parts of vinyl glycol ether are uniformly dispersed in 39 parts of water by ultrasonication to obtain a first mixed solution;
[0071] S2. At room temperature, 25 parts of N-vinyl formamide and 7.5 parts of acryloyloxyethyl trimethyl ammonium chloride are uniformly dispersed in 70 parts of water by ultrasonication to obtain a second mixed solution;
[0072] S3. At room temperature, 2.5 parts of the initiator are uniformly dispersed in 21.5 parts of water to obtain a third mixed solution; 4 parts of the chain transfer agent are uniformly dispersed in 21 parts of water to obtain a fourth mixed solution;
[0073] S4, after uniformly mixing the first mixed liquid and the second mixed liquid, a fifth mixed liquid is obtained, and a 20% by mass NaOH solution is used to adjust the pH of the fifth mixed liquid to 6-7; nitrogen is introduced into a reactor with a stirring device to remove oxygen in the reactor, and the nitrogen atmosphere is maintained, the fifth mixed liquid is transferred to the reactor, and the fifth mixed liquid is heated and stirred to 65° C. The stirring speed is set to 300 r / min; the third mixed liquid and the fourth mixed liquid are sequentially added dropwise to the fifth mixed liquid at a constant pressure to obtain a sixth mixed liquid, and the dropping speed of the third mixed liquid and the fourth mixed liquid is 30 drops / min;
[0074] S5, stirring and keeping the sixth mixed solution at 65° C. for 2-3 hours, with the stirring speed set to 600 r / min, then naturally cooling to 50° C., with the stirring speed set to 300 r / min, and stirring and keeping the solution at 50° C. for 1-2 hours, then taking it out from the reactor to obtain a seventh mixed solution;
[0075] S6. Add 100 parts of anhydrous ethanol to the seventh mixed solution, wash and purify for multiple times and filter out the anhydrous ethanol to obtain a white viscous substance. The white viscous substance is vacuum freeze-dried to obtain a polymer fluid loss reducer. The vacuum freeze-drying temperature is -10°C and the time is 8 hours.
[0076] Example 3
[0077] As a preferred embodiment of the present invention, the sulphoaluminate cement polymer fluid loss reducer for cementing disclosed in this embodiment has the components shown in Table 3.
[0078] Table 3 Specific components of polymer fluid loss additive in Example 3
[0079] Raw material name Weight parts / parts Sodium Methylpropene Sulfonate 25 Vinyl glycol ether 35 N-vinyl formamide 30 Acryloyloxyethyltrimethylammonium chloride 10 Initiator 3 Chain transfer agent 5
[0080] In this embodiment, a sulphoaluminate cement polymer fluid loss reducer for cementing was prepared according to the components in Table 3:
[0081] S1. At room temperature, 25 parts of sodium methacrylate sulfonate and 35 parts of vinyl glycol ether are uniformly dispersed in 40 parts of water by ultrasonication to obtain a first mixed solution;
[0082] S2. At room temperature, 30 parts of N-vinyl formamide and 10 parts of acryloyloxyethyl trimethyl ammonium chloride are uniformly dispersed in 80 parts of water by ultrasonication to obtain a second mixed solution;
[0083] S3. At room temperature, 3 parts of the initiator are uniformly dispersed in 22 parts of water to obtain a third mixed solution; 5 parts of the chain transfer agent are uniformly dispersed in 20 parts of water to obtain a fourth mixed solution;
[0084] S4, after uniformly mixing the first mixed liquid and the second mixed liquid, a fifth mixed liquid is obtained, and a 20% by mass NaOH solution is used to adjust the pH of the fifth mixed liquid to 6-7; nitrogen is introduced into a reactor with a stirring device to remove oxygen in the reactor, and the nitrogen atmosphere is maintained, the fifth mixed liquid is transferred to the reactor, and the fifth mixed liquid is heated and stirred to 65° C. The stirring speed is set to 600 r / min; the third mixed liquid and the fourth mixed liquid are sequentially added dropwise to the fifth mixed liquid at a constant pressure to obtain a sixth mixed liquid, and the dropping speed of the third mixed liquid and the fourth mixed liquid is 30 drops / min;
[0085] S5, stirring and keeping the sixth mixed solution at 65° C. for 2-3 hours, with the stirring speed set to 600 r / min, then naturally cooling to 50° C., with the stirring speed set to 300 r / min, and stirring and keeping the solution at 50° C. for 1-2 hours, then taking it out from the reactor to obtain a seventh mixed solution;
[0086] S6. Add 100 parts of anhydrous ethanol to the seventh mixed solution, wash and purify for multiple times and filter out the anhydrous ethanol to obtain a white viscous substance. The white viscous substance is vacuum freeze-dried to obtain a polymer fluid loss reducer. The vacuum freeze-drying temperature is -10°C and the time is 8 hours.
[0087] After testing, the number average molecular weight of the random multi-polymer in the polymer fluid loss additive obtained in Examples 1 to 3 is 20,000 to 80,000. And after infrared spectroscopy, the structural units in the random multi-polymer are as follows Figure 1 As shown, it includes general formula I, general formula II, general formula III and general formula IV. The infrared spectra of the random copolymers of each general formula are shown Figure 2 shown.
[0088] The random copolymer of general formula I is characterized by infrared spectroscopy as follows: In the infrared spectrum, 2927 and 2829 cm -1 It is the stretching vibration absorption peak of C-H bond in -CH3 or -CH2, 1324cm -1 The bending vibration absorption peak of C-H bond is 1037cm -1 The characteristic absorption peak of the stretching vibration of sulfonic acid group-SO3M, 684cm -1 The weak peak at is the stretching vibration absorption peak of O—S bond.
[0089] The random copolymer of general formula II is characterized by infrared spectroscopy as follows: 3446 cm -1 The peaks at 2927 and 2859 cm-1 can be attributed to the stretching vibration absorption peaks of -OH in vinyl glycol ether. -1 It is the stretching vibration absorption peak of the C-H bond in -CH2-, 1324cm -1 The bending vibration absorption peak of C-H bond is 1407cm in the infrared spectrum.-1 The C—O—C stretching vibration absorption peak in 3-vinyl glycol ether is 873 cm -1 It is the bending vibration absorption peak of C—O—C.
[0090] The random copolymer of formula III is characterized by infrared spectroscopy as follows: In the infrared spectrum, 2927 and 2859 cm -1 It is the stretching vibration absorption peak of C—H bond in N-vinylformamide, 1670cm -1 The stretching vibration absorption peaks at 1650-1565cm -1 The absorption peaks are at 1002-1193 cm-1, which are the C-N bond stretching vibration absorption peak and N-H bending vibration absorption peak in N-vinyl formamide. -1 The absorption peaks between them should be attributed to the stretching vibration absorption peaks of C—N bonds.
[0091] The random copolymer of formula IV is characterized by infrared spectroscopy as follows: -1 It is the stretching vibration absorption peak of C-H in -CH3 or -CH2-, 1670cm -1 The stretching vibration absorption peak at 1407 cm-1 is attributed to the C=O bond of acryloyloxyethyltrimethylammonium chloride. -1 The absorption peak at 1324 cm-1 is attributed to the antisymmetric deformation vibration of -CH3. -1 The C—N + The stretching vibration absorption peak of the bond, and 1002cm -1 C-N + Bond stretching vibration absorption peak.
[0092] Comparative Example 1
[0093] Commercially available silicate cement fluid loss reducers are used, mainly AMPS / AM copolymers.
[0094] Comparative Example 2
[0095] The blank group was not added with any fluid loss additive.
[0096] Test Case
[0097] The sulphoaluminate polymer fluid loss reducer for cementing obtained in Examples 1 to 3 was added to the cement slurry, and the experiment was conducted according to the following formula: sulphoaluminate cement (based on 100% by weight of sulphoaluminate cement) + 0.3% of boric acid + 0.3-0.9% of sulphoaluminate polymer fluid loss reducer for cementing + 44% of water. (The cement slurry formula for cementing is not limited to the above-mentioned cement admixtures for cementing).
[0098] Comparative Example 1 and Comparative Example 2 (blank group) were set up at the same time. The comparative example used a commercially available common high-temperature suspension stabilizer to replace the polymer fluid loss additive of the present invention, and the blank group did not add any fluid loss additive. The other ratios and conditions were the same as the above configuration.
[0099] The cementing sulphoaluminate cement slurry was prepared according to GB / T19139-2012 Test Method for Oil Well Cement, and the thickening performance and engineering performance of the cementing sulphoaluminate cement slurry in the embodiment and the comparative example were tested according to SY / T6544-2017 Performance Requirements for Oil Well Cement Slurry. The experimental results are shown in Table 4.
[0100] Table 4 Experimental results of examples and control examples
[0101]
[0102]
[0103] From the results of Table 4, it can be seen that when no fluid loss reducer is added (Comparative Example 2), the water loss of cementing sulphoaluminate cement is large, and the water loss is as high as 93mL, which cannot meet the cementing requirements of the tail pipe cementing cement slurry. When the prior art fluid loss reducer for oil well cement is added (Comparative Example 1), the water loss of cementing sulphoaluminate cement slurry does not decrease but increases, and there is free liquid, which shows that the prior art fluid loss reducer is not suitable for cementing sulphoaluminate cement system. After adding the polymer fluid loss reducer of the present invention, the API water loss of cementing sulphoaluminate cement is effectively controlled, and the API water loss is basically less than 50mL, and with the increase of the amount added, the API water loss is also gradually reduced, which shows that the polymer fluid loss reducer of the present invention has a good water loss control effect on cementing sulphoaluminate cement slurry, and can effectively ensure the safe construction of cementing sulphoaluminate cement.
[0104] from Figure 3 It can be seen that compared with the existing fluid loss reducers, the polymer fluid loss reducer of the present invention has better compatibility with boric acid, and the fluid loss reducer has a slight retarding effect on the cementing sulphoaluminate cement slurry, slightly prolongs the thickening time of the sulphoaluminate cement, can reduce the amount of retarder, and reduce the cost of cementing materials, and has better thickening performance, and the cement slurry does not show abnormal gelling phenomenon, which is manifested by a stable thickening curve.
[0105] from Figure 4 and Figure 5It can be seen that the thickening curve of the sulphoaluminate cementing slurry without the addition of a fluid loss reducer fluctuates to a certain extent, which may be caused by the instability of the slurry, while the thickening curve of the sulphoaluminate cement slurry added with the fluid loss reducer of the prior art fluctuates significantly, which indicates that the sulphoaluminate cement slurry has abnormal gelation. This is because the fluid loss reducer of the prior art is not suitable for the sulphoaluminate cement for cementing and has a strong dispersing effect, resulting in poor sedimentation stability of the cement slurry, which leads to abnormal gelation of the cement slurry, showing obvious fluctuations in the thickening curve.
[0106] It can also be seen from the fluidity test results in Table 4 that the prior art fluid loss reducer has a strong dispersing effect on sulphoaluminate cement and there is free liquid. In addition, it can also be seen from Table 4 that the polymer fluid loss reducer of the present invention has no adverse effect on the early strength of sulphoaluminate cement paste.
[0107] The above experimental results show that the polymer fluid loss reducer prepared by the present invention has an excellent linear water loss control effect on sulphoaluminate cement, and has good adaptability in cementing sulphoaluminate cement slurry, has no adverse effect on the rheological properties, thickening properties, early strength and other working properties of sulphoaluminate cement, and can effectively ensure the cementing quality of low-temperature oil and gas layers such as shallow surface, frozen layer, and deep water.
[0108] Finally, it should be noted that the above embodiments are only preferred embodiments of the present invention to illustrate the technical solutions of the present invention, rather than limiting them, and certainly not limiting the patent scope of the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions recorded in the aforementioned embodiments, or replace some or all of the technical features therein by equivalents. These modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present invention. In other words, any changes or modifications made to the main design concept and spirit of the present invention that have no substantive significance, and the technical problems they solve are still consistent with the present invention, should be included in the protection scope of the present invention. In addition, the direct or indirect application of the technical solutions of the present invention in other related technical fields is also included in the patent protection scope of the present invention.
Claims
1. A polymer fluid loss reducer for cementing sulphoaluminate cement, characterized in that: The parts by weight include: 25-45 parts of sodium methyl methacrylate sulfonate; 25-35 parts of vinyl glycol ether; 20-30 parts of N-vinyl formamide; 5-10 parts of acryloyloxyethyl trimethyl ammonium chloride; 2-3 parts of initiator; 3 to 5 parts of chain transfer agent.
2. The polymer fluid loss reducer for cementing sulphoaluminate cement according to claim 1, characterized in that: The structural unit composition of the polymer fluid loss reducer comprises a random copolymer of general formula I, general formula II, general formula III and general formula IV and a number average molecular weight of 20,000 to 40,000.
3. The polymer fluid loss reducer for cementing sulphoaluminate cement according to claim 2, characterized in that: In the structural unit of the polymer fluid loss reducer, the mass percentages of general formula I, general formula II, general formula III and general formula IV are respectively: I = 25-45%, II = 25-35%, III = 20-30%, IV = 5-10%.
4. The polymer fluid loss reducer for cementing sulphoaluminate cement according to claim 1, characterized in that: The purity of the sodium methyl methacrylate sulfonate and the N-vinyl formamide are both analytically pure.
5. The polymer fluid loss reducer for cementing sulphoaluminate cement according to claim, characterized in that: The effective component content of the vinyl glycol ether is 99%.
6. The polymer fluid loss reducer for cementing sulphoaluminate cement according to claim 1, characterized in that: The acryloyloxyethyl trimethyl ammonium chloride is an aqueous solution with a mass fraction of 80%.
7. The polymer fluid loss reducer for cementing sulphoaluminate cement according to claim 1, characterized in that: The initiator is a peroxide or a mixture of several peroxides, and the peroxide includes potassium persulfate, sodium persulfate, and ammonium persulfate.
8. The polymer fluid loss reducer for cementing sulphoaluminate cement according to claim 1, characterized in that: The chain transfer agent is one or a mixture of lignin xanthate, isopropyl alcohol, and sodium hypophosphite.
9. The method for preparing a polymer fluid loss reducer for cementing sulphoaluminate cement according to any one of claims 1 to 8, characterized in that: The following steps are involved: S1. At room temperature, 25 to 45 parts of sodium methacrylate sulfonate and 25 to 35 parts of vinyl glycol ether are uniformly dispersed in 25 to 50 parts of water to obtain a first mixed solution; S2. At room temperature, 20 to 30 parts by weight of N-vinyl formamide and 5 to 10 parts by weight of acryloyloxyethyl trimethyl ammonium chloride are uniformly dispersed in 70 to 85 parts of water to obtain a second mixed solution; S3. At room temperature, 2 to 3 parts of the initiator are uniformly dispersed in 20 to 22 parts of water by weight to obtain a third mixed solution; 3 to 5 parts of the chain transfer agent are uniformly dispersed in 20 to 22 parts of water to obtain a fourth mixed solution; S4, uniformly mixing the first mixed liquid and the second mixed liquid to obtain a fifth mixed liquid; introducing nitrogen into a reactor with a stirring device to remove oxygen in the reactor, and maintaining a nitrogen atmosphere, transferring the fifth mixed liquid to the reactor, heating and stirring the fifth mixed liquid to 65° C.; sequentially adding the third mixed liquid and the fourth mixed liquid dropwise to the fifth mixed liquid at a constant pressure to obtain a sixth mixed liquid; S5, stirring and keeping the sixth mixed solution at 65° C. for 2-3 hours, then naturally cooling to 50° C., stirring and keeping the solution at 50° C. for 1-2 hours, and then taking the solution out of the reactor to obtain a seventh mixed solution; S6, adding 100 parts of anhydrous ethanol to the seventh mixed solution, washing and purifying for multiple times and filtering out the anhydrous ethanol to obtain a white viscous substance, and vacuum freeze-drying the white viscous substance to obtain the polymer fluid loss reducer.
10. The method for preparing a polymer fluid loss reducer for cementing sulphoaluminate cement according to claim 9, characterized in that: In S3, the dropping speed of the third mixed liquid and the fourth mixed liquid is 30 drops / min; in S4, a 20% by mass NaOH solution is used to adjust the pH of the fifth mixed liquid to 6-7; in S5, the stirring speed at 65°C is 600r / min, and the stirring speed at 50°C is 300r / min; in S6, the temperature of vacuum freeze drying is -10°C and the time is 8h.