Preparation method of ultrahigh-temperature fluid loss agent for well cementation

By performing polymer grafting on the surface of the slurry, a water loss reduction agent with high temperature stability and low cost was prepared, which solved the problem of loss of cement slurry in the ultra-high temperature cementing environment in the prior art, and realized the cement slurry Good suspension stability and water loss effect at high temperatures.

CN118978650AActive Publication Date: 2024-11-19CHINA UNIV OF PETROLEUM (EAST CHINA)
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202411041754.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-19
Estimated Expiration
2044-07-31

AI Technical Summary

Technical Problem

In the ultra-high temperature cementing environment above 200°C, the water loss agent has poor temperature resistance and salt resistance, and is relatively high in cost, making it difficult to effectively control the water loss amount and suspension stability of the cement slurry.

Method used

Using parathralis as the grafting core, modified by silane coupling agent, and polymer grafting is performed on its surface, using itaconic acid, 2-acrylamide-2-methylpropanesulfonic acid, and parastyrenesulfonic acid. Water-soluble monomers such as sodium acid are polymerized in aqueous solution to prepare polymer grafted particles with good dispersion properties, which significantly reduces the water loss of cement slurry at high temperatures and improves suspension stability.

Benefits of technology

The water loss of cement slurry is significantly reduced under high-temperature and ultra-high temperature environments, the suspension stability of cement slurry is improved, the temperature resistance can reach 240℃, and the good water loss reduction effect is maintained under semi-saturated brine conditions, reducing production costs .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004972557620000071
    Figure BDA0004972557620000071
  • Figure BDA0004972557620000081
    Figure BDA0004972557620000081
  • Figure BDA0004972557620000082
    Figure BDA0004972557620000082
Patent Text Reader

Abstract

The invention relates to a preparation method of an ultrahigh-temperature fluid loss agent for well cementation, and belongs to the technical field of oilfield chemistry. Palygorskite is subjected to surface modification through a silane coupling agent, so that sites are polymerized on the surface of the palygorskite, the palygorskite participates in a polymerization reaction, and non-ionic water-soluble monomers such as N, N-dimethylacrylamide and the like are used for modifying the surface of the palygorskite. According to the invention, palygorskite, anionic water-soluble monomers such as 2-acrylamide-2-methylpropanesulfonic acid, itaconic acid, sodium p-styrenesulfonate and the like, and rigid monomers such as vinyl pyrrolidone, sodium p-styrenesulfonate and the like are used as polymerization raw materials to synthesize the polymer grafted palygorskite. The fluid loss agent has excellent temperature resistance and salt tolerance, and has excellent fluid loss reduction performance in both high-temperature and ultra-high-temperature environments, and the fluid loss volume at 240 DEG C is 1t; and the filtrate reducer has no obvious influence on other basic properties of the cement paste, can effectively improve the suspension stability of the cement paste at high temperature, and is suitable for being used as a filtrate reducer of the cement paste for well cementation under severe conditions.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for preparing an ultra-high temperature fluid loss reducer for cementing, and belongs to the technical field of oilfield chemistry. Background Art

[0002] Petroleum is one of the indispensable non-renewable resources in modern society, and its exploitation and utilization play an important role in the development of the national economy. At present, with the continuous exploitation of oil and gas, it has gradually shifted from conventional oil and gas to deep oil reservoirs. As for deep oil reservoirs, there are still many problems to be solved in the exploitation process. Cementing is an indispensable and important part of oil and gas exploration and development, one of the important links in drilling engineering, and a key step to ensure the life of oil and gas wells, improve the production capacity of oil and gas wells, and promote the overall benefits of oil and gas exploration and development. For deep and ultra-deep cementing technology, it faces problems such as high temperature, high pressure, complex formation, leakage, salt-gypsum layer, and long sealing section. Compared with conventional well sections, the difficulty of cementing has increased significantly, which also requires cementing additives to have better performance to cope with this harsh environment.

[0003] Retarders, fluid loss agents and dispersants are the three main agents in oil well cementing engineering, which play a vital role in the comprehensive performance of cement slurry, the safety of cementing process and the quality of cementing. Among them, fluid loss agents can effectively control the filtration loss of cement slurry to the formation. In deep well and ultra-deep well environment, especially after 200℃, conventional fluid loss agents are very easy to hydrolyze, break chains and fail in such environment, thus making the filtration loss of cement slurry out of control. The loss of control of filtration loss will not only cause adverse effects such as oil and gas layer pollution, formation damage and channeling, but also affect the quality of cementing, and in severe cases, it will cause cementing accidents and cementing failure. Since conventional linear polymers of 2-acrylamido-2-methylpropanesulfonic acid (AMPS) cannot be used in high temperature environment, current research mainly focuses on particle grafting and the introduction of temperature-resistant monomers to improve the temperature resistance of fluid loss agents.

[0004] Chinese patent document CN 113651931A discloses a method for preparing an ultra-high temperature modified polymer cementing fluid loss reducer. The preparation method is as follows: firstly, graphene oxide is ultrasonically dispersed, and then reacted with azobisisobutylamidine hydrochloride in an alkaline environment. Then, 2-acrylamido-2-methylpropanesulfonic acid, N,N-dimethylacrylamide and itaconic acid are used as polymerization monomers to react with the treated graphene solution to synthesize an ultra-high temperature modified polymer cementing fluid loss reducer. The ultra-high temperature modified polymer cementing fluid loss reducer has the advantages of stable performance, strong temperature resistance (30-240°C), saturated salt resistance, excellent fluid loss reduction performance, strong adaptability and significant improvement in the mechanical properties of cement stone. However, due to the high price of graphene oxide and the difficulty in dispersing the modified product, it is difficult to promote it in oil fields.

[0005] Chinese patent document CN 115404061A discloses a method for preparing a high temperature and salt resistant fluid loss reducer composition, wherein an intermediate polymer is formed by a basic monomer and a neutral monomer, wherein the basic monomer is mainly one or more of para-, ortho- and meta-olefin sulfonates containing a benzene ring, and the neutral monomer is a mixture of acrylamide and lauryl methacrylate in any proportion, and ammonium persulfate is used as an initiator. After the reaction is completed, an acidic monomer solution such as acrylic acid is slowly dripped into the mixture to continue the reaction to form a block polymer. The obtained polymer can effectively reduce the water loss of cement slurry and has no significant effect on the rheological properties of cement slurry, but the water loss performance after the temperature is higher than 120°C has not yet been disclosed.

[0006] Although the existing technology represented by the above patents has made breakthroughs in the temperature resistance and salt resistance of polymer cementing fluid loss reducers, there are still problems in the application and promotion of ultra-high temperature cementing operations above 200°C. Summary of the invention

[0007] In view of the shortcomings of the prior art such as poor temperature resistance and salt resistance and high cost of granular materials, the present invention provides a method for preparing an ultra-high temperature fluid loss reducer for cementing. The palygorskite with stable performance at high temperature and low cost is used as a grafting core. After a polymer is grafted on its surface, the heat and salt resistance of the polymer can be effectively improved, the water loss of cement slurry under high temperature and ultra-high temperature environments can be reduced, and the suspension stability of the cement slurry can be improved. SUMMARY OF THE INVENTION

[0009] The present invention utilizes the advantages of palygorskite's stable structural performance and low price at high temperature, and modifies palygorskite with a silane coupling agent to form unsaturated groups on its surface as reaction sites for grafted polymers. Itaconic acid, 2-acrylamido-2-methylpropanesulfonic acid, sodium p-styrenesulfonate and N,N-dimethylacrylamide and other water-soluble monomers are used as raw materials to prepare polymer-grafted palygorskite through aqueous solution polymerization. After testing, the product has good dispersibility in the solution. After being added to cement slurry, it can significantly reduce the water loss in high temperature and ultra-high temperature environments, and improve the suspension stability of cement slurry in high temperature environments. The temperature resistance can reach 240°C, the water loss is 38mL, and the salt resistance can resist semi-saturated salt water. DETAILED DESCRIPTION OF THE INVENTION

[0011] The technical solution of the present invention is as follows:

[0012] A preparation method of an ultra-high temperature fluid loss reducer for cementing:

[0013] (1) Surface modification of palygorskite

[0014] 200-1200 mesh palygorskite and hydrochloric acid are placed in a three-necked flask equipped with a stirrer and a thermometer, wherein the palygorskite accounts for 1-10% of the total mass, and the concentration of hydrochloric acid is 1-4 mol / L. After heating to 50-80°C, stirring for 1-2 hours, the surface hydroxyl groups of the palygorskite are activated, the product is taken out, washed with distilled water until neutral, dried and crushed. The activated palygorskite is dispersed in toluene, wherein the mass fraction of palygorskite is 1-5%, and a certain amount of silane coupling agent KH570 is added. After reacting for 3-6 hours, when the reaction is completed, the product is filtered, washed with anhydrous ethanol, and then dried at 105°C and crushed to obtain modified palygorskite. The mass ratio of palygorskite to KH570 is 1: (0.5-10).

[0015] (2) Preparation of polymer-grafted palygorskite

[0016] Adding modified palygorskite, nonionic water-soluble monomer, anionic water-soluble monomer and rigid monomer into a three-necked glass bottle equipped with a stirrer, a nitrogen tube and a thermometer, stirring at high speed, stirring until all raw materials are evenly dispersed, controlling the pH at 5-11, passing nitrogen for 30 minutes, adding an initiator, controlling the temperature at 40-70°C, reacting for 2-10 hours, drying and crushing the product to obtain the desired target product; the monomer accounts for 10-30% of the total mass, the mass ratio of modified palygorskite, nonionic water-soluble monomer, anionic water-soluble monomer and rigid monomer is 1:(1-16):(1-10):(0-5), and the initiator accounts for 0.1-2% of the total mass of the monomer;

[0017] According to the present invention, preferably, the nonionic water-soluble monomer is one of acrylamide, N,N-dimethylacrylamide, N-isopropylacrylamide, and N-ethylacrylamide;

[0018] Preferably, the anionic water-soluble monomer is one of itaconic acid, acrylic acid, methacrylic acid, maleic acid, 2-acrylamido-2-methylpropanesulfonic acid, and sodium vinyl sulfonate;

[0019] Preferably, the rigid monomer is one of vinyl pyrrolidone, sodium p-styrene sulfonate, styrene, and N-vinyl pyridine;

[0020] Preferably, the initiator is one or more of potassium persulfate, sodium persulfate, ammonium persulfate, azobisisobutylamidine hydrochloride, azobisisobutylonitrile, and azobisisobutylimidazoline hydrochloride;

[0021] Preferably, the mesh number of palygorskite is 300 to 1000 mesh;

[0022] Preferably, the mass ratio of kaolinite to KH570 is 1:(1-8);

[0023] Preferably, the monomer accounts for 10-25% of the total mass, and the mass ratio of the modified palygorskite, the nonionic water-soluble monomer, the anionic water-soluble monomer and the rigid monomer is 1:(1-12):(2-8):(0-4);

[0024] Preferably, the persulfate accounts for 0.5 to 1.5% of the total weight of the monomer;

[0025] Preferably, during the polymerization process, the pH is 5 to 9 and the temperature is controlled at 50 to 65°C;

[0026] Preferably, the polymerization reaction time is 3 to 6 hours.

[0027] The excellent effects of the present invention are as follows:

[0028] 1. The present invention is a polymer grafted particle, and palygorskite has good high temperature stability, can effectively maintain structural stability under high temperature environment, and provide a rigid core for the polymer. After optimizing the monomer type and synthesis method, the tolerance of the polymer itself under high temperature conditions is enhanced, and under the joint action with the particles, the molecular volume changes less under high temperature or high salt. At the same time, the introduced carboxyl group also allows the product to be well adsorbed on the surface of cement particles, and the product itself can also fill the gaps in the mud cake to a certain extent. After the combination of the two, a thin and tough filter cake can be formed during high temperature and ultra-high temperature water loss process, thereby playing a good water loss reduction effect under high temperature and ultra-high temperature environment, and due to its own structural heat-resistant design, it can also improve the sedimentation stability of cement slurry under high temperature environment.

[0029] 2. The present invention uses conventional monomers as polymerization raw materials, and the molecular weight of the product is controllable. Compared with graphene and nano-silicon dioxide modified products, palygorskite is low in cost and has good hydrophilicity and dispersibility, and its own performance is less affected by temperature and alkaline environment.

[0030] 3. The product prepared by the present invention has good compatibility with conventional cement slurry systems. DETAILED DESCRIPTION

[0031] Unless otherwise specified, the experimental methods used in the following examples are conventional methods.

[0032] Unless otherwise specified, the materials and reagents used in the following examples can be obtained from commercial sources, including:

[0033] In the present invention, N,N-dimethylacrylamide can be obtained commercially, for example, it can be purchased from Jiangsu Bosite Chemical Technology Co., Ltd., industrial grade; vinyl pyrrolidone can be obtained commercially, for example, it can be purchased from Shanghai Aladdin Biochemical Technology Co., Ltd., chemically pure; sodium p-styrene sulfonate can be obtained commercially, for example, it can be purchased from Shanghai Aladdin Biochemical Technology Co., Ltd., chemically pure; itaconic acid can be obtained commercially, for example, it can be purchased from Sinopharm Chemical Reagent Co., Ltd., chemically pure; palygorskite can be obtained commercially, for example, it can be purchased from Shijiazhuang Borui Building Materials Co., Ltd.

[0034] The present invention is further described below in conjunction with specific embodiments, but the protection scope of the present invention is not limited thereto.

[0035] Embodiment 1:

[0036] A method for preparing an ultra-high temperature fluid loss additive for cementing comprises the following steps:

[0037] 1000 mesh palygorskite and hydrochloric acid were placed in a three-necked flask equipped with a stirrer and a thermometer, wherein the palygorskite accounted for 2% of the total mass and the hydrochloric acid concentration was 2 mol / L. Stirring was carried out for 0.8 hours to activate the surface hydroxyl groups of the palygorskite, and then the product was taken out, washed with distilled water until neutral, dried and crushed. 1 part of the activated palygorskite was added to 94 parts of toluene solution, and 5 parts of silane coupling agent KH570 were added. After the reaction was completed for 4 hours, the product was filtered, washed with anhydrous ethanol, and then dried at 105°C and crushed. 1 part of modified palygorskite, 6 parts of N,N-dimethylacrylamide, 2 parts of 2-acrylamido-2-methylpropanesulfonic acid, 2 parts of itaconic acid, 2 parts of sodium p-styrenesulfonate and 85 parts of deionized water were added into a three-necked glass bottle equipped with a stirrer, a nitrogen tube and a thermometer, and stirred at high speed. After all the raw materials were evenly dispersed, the pH was controlled at 6, nitrogen was introduced for 30 minutes, 1.5 parts of ammonium persulfate were added, and the reaction was carried out for 4 hours. The product was dried and crushed to obtain.

[0038] Embodiment 2:

[0039] 1000 mesh palygorskite and hydrochloric acid were placed in a three-necked flask equipped with a stirrer and a thermometer, wherein the palygorskite accounted for 2% of the total mass and the hydrochloric acid concentration was 2 mol / L. After heating to 80°C, stirred for 2 hours to activate the surface hydroxyl groups of the palygorskite, the product was taken out, washed with distilled water until neutral, dried and crushed. 1 part of the activated palygorskite was added to 94 parts of toluene solution, and 5 parts of silane coupling agent KH570 were added. After the reaction was completed for 4 hours, the product was filtered, washed with anhydrous ethanol, and then dried at 105°C and crushed. 1 part of modified palygorskite, 10 parts of N,N-dimethylacrylamide, 2 parts of itaconic acid, 2 parts of 2-acrylamido-2-methylpropanesulfonic acid and 85 parts of deionized water were added into a three-necked glass bottle equipped with a stirrer, a nitrogen tube and a thermometer, and stirred at high speed. After all the raw materials were evenly dispersed, the pH was controlled at 6, nitrogen was introduced for 30 minutes, 1.5 parts of ammonium persulfate were added, and the reaction was carried out for 4 hours. The product was dried and crushed to obtain.

[0040] Embodiment 3:

[0041] As described in Example 1, except that the concentration of hydrochloric acid is 3 mol / L.

[0042] Embodiment 4:

[0043] 1000 mesh palygorskite and hydrochloric acid were placed in a three-necked flask equipped with a stirrer and a thermometer, wherein the palygorskite accounted for 2% of the total mass and the hydrochloric acid concentration was 2 mol / L. After heating to 80°C, stirred for 1 hour to activate the surface hydroxyl groups of the palygorskite, the product was taken out, washed with distilled water until neutral, dried and crushed. 1 part of the activated palygorskite was added to 94 parts of toluene solution, and 8 parts of silane coupling agent KH570 were added. After the reaction was completed for 6 hours, the product was filtered, washed with anhydrous ethanol, and then dried at 105°C and crushed. 1 part of modified palygorskite, 8 parts of N,N-dimethylacrylamide, 2 parts of itaconic acid, 2 parts of 2-acrylamido-2-methylpropanesulfonic acid and 85 parts of deionized water were added into a three-necked glass bottle equipped with a stirrer, a nitrogen tube and a thermometer, and stirred at high speed. After all the raw materials were evenly dispersed, the pH was controlled at 6, nitrogen was introduced for 30 minutes, 1.7 parts of ammonium persulfate were added, and the reaction was carried out for 4 hours. The product was dried and crushed to obtain.

[0044] Embodiment 5:

[0045] As described in Example 1, except that the nonionic water-soluble monomer is 10 parts of acrylamide.

[0046] Embodiment 6:

[0047] As described in Example 1, the difference is that the added monomers are 1 part of modified palygorskite, 6 parts of N,N-dimethylacrylamide, 4 parts of vinyl pyrrolidone, 2 parts of 2-acrylamido-2-methylpropanesulfonic acid, and the initiator is azobisisobutylimidazoline hydrochloride.

[0048] Embodiment 7:

[0049] 500 mesh palygorskite and hydrochloric acid were placed in a three-necked flask equipped with a stirrer and a thermometer, wherein the palygorskite accounted for 2% of the total mass and the hydrochloric acid concentration was 3 mol / L. After heating to 80°C, stirred for 1 hour to activate the surface hydroxyl groups of the palygorskite, the product was taken out, washed with distilled water until neutral, dried and crushed. 1 part of the activated palygorskite was added to 94 parts of toluene solution, and 5 parts of silane coupling agent KH570 were added. After the reaction was completed for 4 hours, the product was filtered, washed with anhydrous ethanol, and then dried at 105°C and crushed. 1 part of modified palygorskite, 10 parts of N,N-dimethylacrylamide, 2 parts of acrylic acid, 2 parts of 2-acrylamido-2-methylpropanesulfonic acid and 85 parts of deionized water were added into a three-necked glass bottle equipped with a stirrer, a nitrogen tube and a thermometer, and stirred at high speed. After all the raw materials were evenly dispersed, the pH was controlled at 6, nitrogen was introduced for 30 minutes, 1.3 parts of ammonium persulfate were added, and the reaction was carried out for 4 hours. The product was dried and crushed to obtain.

[0050] Embodiment 8:

[0051] 1000 mesh palygorskite and hydrochloric acid were placed in a three-necked flask equipped with a stirrer and a thermometer, wherein the palygorskite accounted for 2% of the total mass and the hydrochloric acid concentration was 2 mol / L. After heating to 80°C, stirred for 1 hour to activate the surface hydroxyl groups of the palygorskite, the product was taken out, washed with distilled water until neutral, dried and crushed. 1 part of the activated palygorskite was added to 94 parts of toluene solution, and 5 parts of silane coupling agent KH570 were added. After the reaction was completed for 4 hours, the product was filtered, washed with anhydrous ethanol, and then dried at 105°C and crushed. 1 part of modified palygorskite, 10 parts of N,N-dimethylacrylamide, 2 parts of maleic acid, 2 parts of sodium p-styrene sulfonate and 85 parts of deionized water were added into a three-necked glass bottle equipped with a stirrer, a nitrogen tube and a thermometer, and stirred at high speed. After all the raw materials were evenly dispersed, the pH was controlled at 6, nitrogen was introduced for 30 minutes, 1.5 parts of ammonium persulfate were added, and the reaction was carried out for 4 hours. The product was dried and crushed to obtain.

[0052] Embodiment 9:

[0053] As described in Example 1, except that the anionic water-soluble monomer is 4 parts of maleic acid.

[0054] Embodiment 10:

[0055] As described in Example 1, except that the amount of deionized water is 35 parts.

[0056] Embodiment 11:

[0057] As described in Example 1, except that the amount of ammonium persulfate was 0.75 parts.

[0058] Embodiment 12:

[0059] 1000 mesh palygorskite and hydrochloric acid were placed in a three-necked flask equipped with a stirrer and a thermometer, wherein the palygorskite accounted for 1.5% of the total mass and the hydrochloric acid concentration was 2 mol / L. After heating to 80°C, stirred for 1 hour to activate the surface hydroxyl groups of the palygorskite, the product was taken out, washed with distilled water until neutral, dried and crushed. 1 part of the activated palygorskite was added to 89 parts of toluene solution, and 10 parts of silane coupling agent KH570 were added. After the reaction was completed for 4 hours, the product was filtered, washed with anhydrous ethanol, and then dried at 105°C and crushed. 1 part of modified palygorskite, 10 parts of N,N-dimethylacrylamide, 2 parts of itaconic acid, 2 parts of sodium p-styrene sulfonate and 85 parts of deionized water were added into a three-necked glass bottle equipped with a stirrer, a nitrogen tube and a thermometer, and stirred at high speed. After all the raw materials were evenly dispersed, the pH was controlled at 8, nitrogen was introduced for 30 minutes, 1.5 parts of ammonium persulfate were added, and the reaction was carried out for 6 hours. The product was dried and crushed to obtain.

[0060] Comparative Example 1:

[0061] This comparative example provides a cementing slurry fluid loss reducer, which is prepared by the following specific steps:

[0062] Add 10 parts of N,N-dimethylacrylamide, 2 parts of itaconic acid, 2 parts of 2-acrylamido-2-methylpropanesulfonic acid and 86 parts of deionized water into a three-necked glass bottle equipped with a stirrer, a nitrogen tube and a thermometer, and stir at high speed. After all the raw materials are evenly dispersed, the pH is controlled at 6, nitrogen is introduced for 30 minutes, 1.5 parts of ammonium persulfate are added, and the reaction is carried out for 4 hours. The product is dried and crushed to obtain.

[0063] Comparative Example 2:

[0064] This comparative example provides a cementing slurry fluid loss reducer, which is prepared by the following specific steps:

[0065] Add 10 parts of N,N-dimethylacrylamide, 2 parts of itaconic acid, 2 parts of sodium p-styrene sulfonate and 86 parts of deionized water into a three-necked glass bottle equipped with a stirrer, a nitrogen tube and a thermometer, and stir at high speed. After all the raw materials are evenly dispersed, the pH is controlled at 6, nitrogen is introduced for 30 minutes, 1.5 parts of ammonium persulfate are added, and the reaction is carried out for 6 hours. The product is dried and crushed to obtain.

[0066] Comparative Example 3:

[0067] This comparative example provides a cementing slurry fluid loss reducer, which is prepared by the following specific steps:

[0068] Add 10 parts of N,N-dimethylacrylamide, 4 parts of itaconic acid, 2 parts of sodium p-styrene sulfonate and 84 parts of deionized water into a three-necked glass bottle equipped with a stirrer, a nitrogen tube and a thermometer, and stir at high speed. After all the raw materials are evenly dispersed, the pH is controlled at 6, nitrogen is introduced for 30 minutes, 1.5 parts of ammonium persulfate are added, and the reaction is carried out for 6 hours. The product is dried and crushed to obtain.

[0069] Comparative Example 4:

[0070] This comparative example provides a cementing slurry fluid loss reducer, which is prepared by the following specific steps:

[0071] Add 10 parts of N,N-dimethylacrylamide, 2 parts of maleic acid, 2 parts of 2-acrylamido-2-methylpropanesulfonic acid and 86 parts of deionized water into a three-necked glass bottle equipped with a stirrer, a nitrogen tube and a thermometer, and stir at high speed. After all the raw materials are evenly dispersed, the pH is controlled at 6, nitrogen is introduced for 30 minutes, 1.5 parts of ammonium persulfate are added, and the reaction is carried out for 6 hours. The product is dried and crushed to obtain.

[0072] Comparative Example 5:

[0073] This comparative example provides a cementing slurry fluid loss reducer, which is prepared by the following specific steps:

[0074] Add 10 parts of N,N-dimethylacrylamide, 4 parts of acrylic acid, 2 parts of 2-acrylamido-2-methylpropanesulfonic acid and 84 parts of deionized water into a three-necked glass bottle equipped with a stirrer, a nitrogen tube and a thermometer, and stir at high speed. After all the raw materials are evenly dispersed, the pH is controlled at 5, nitrogen is introduced for 30 minutes, 1 part of ammonium persulfate is added, and the reaction is carried out for 6 hours. The product is dried and crushed to obtain. BRIEF DESCRIPTION OF THE DRAWINGS

[0075] The accompanying drawings are used to provide a further understanding of the present invention and constitute a part of the specification. Together with the following specific embodiments, they are used to explain the present invention but do not constitute a limitation of the present invention. In the accompanying drawings:

[0076] Figure 1 is a thickening curve of cement slurry at 240°C×120MPa in Test Example 1 of the present invention to which the fluid loss reducer provided in Example 1 (the addition amount is 1% of the cement dry ash weight) is added,

[0077] Figure 2This is a graph showing the influence of Example 1 (dosage is 1% of the dry cement ash weight), Comparative Example 1 (dosage is 1% of the dry cement ash weight) and no fluid loss additive added on the sedimentation stability of cement slurry at 240°C in Test Example 4 of the present invention.

[0078] Performance Evaluation

[0079] Test Example 1:

[0080] For the provided ultra-high temperature fluid loss reducer Example 1 for cementing (the addition amount is 1% of the dry ash weight of cement), its thickening time under 240°C×120Mpa environment was tested. The test was carried out in accordance with the national standard GB / T19139-2012 "Test Method for Oil Well Cement". The obtained thickening curve is as follows: Figure 1 shown.

[0081] Depend on Figure 1 It can be seen that after adding Example 1, the cement slurry thickening curve is overall stable, without obvious "bulges" and abnormal conditions such as rapid decrease in consistency, indicating that Example 1 provided by the present invention has good temperature resistance, good compatibility with the retarder, and has little effect on the cement slurry thickening process. In addition, the cement slurry can still be maintained at about 20Bc under ultra-high temperature environment, which indirectly reflects that it has good sedimentation stability. It can be seen that the present invention can effectively improve the temperature resistance of the polymer and has good compatibility by grafting the polymer on palygorskite.

[0082] Test Example 2:

[0083] For Examples 1 to 12 and Comparative Examples 1 to 5, according to the relevant provisions of the petroleum and natural gas industry standard SY / T5504.2-2013 "Evaluation Methods for Oil Well Cement Admixtures Part 2: Fluid Loss Additives" and the national standard GB / T19139-2012 "Test Methods for Oil Well Cement", the performance parameters such as the initial consistency and API water loss of the cement slurry were tested at different experimental temperatures and fluid loss additive dosages, and the results are shown in Table 1.

[0084] The cement slurry formula is: 500g Jiahua G grade cement + 50% 200 mesh silica sand + 4% retarder + X% fluid loss reducer + water-cement ratio of 0.57.

[0085] Among them, the retarder is homemade in the laboratory, which is a carboxylic acid retarder with a temperature resistance of up to 260°C.

[0086] Table 1 Water loss reduction performance of different water loss reducers under different conditions

[0087]

[0088]

[0089] Note: NaCl concentration is the mass ratio in water.

[0090] From Table 1, it can be seen that the fluid loss reducing agents prepared by Examples 1-12 of the present invention have good fluid loss reducing performance at 240°C, and the initial consistency of the cement slurry after addition is low, all less than 30BC. At the same time, as the temperature increases, although the water loss of Example 1 increases, it remains good overall. At the same time, as the amount added increases, a good water loss reducing effect can be achieved at a dosage of 1.2%. Comparison of different embodiments also found that the polymer monomer has a certain influence on the performance of the product, but the overall API water loss is less than 50mL. Compared with the comparative example, it can be seen that the polymer grafted palygorskite can effectively improve the heat resistance of the polymer and maintain a low water loss under ultra-high temperature environment. At the same time, it can effectively reduce the demand for polymer molecular weight for water loss and reduce the impact of the product on the fluidity of cement slurry. At the same time, under the condition of semi-saturated salt water, it still has good water loss reducing performance.

[0091] Test Example 3:

[0092] For Examples 1 to 12 and Comparative Examples 1 to 5, the compressive strength test, thickening time and other test standards in the national standard GB / T19139-2012 "Test Methods for Oil Well Cement" were used to investigate their effects on cement slurry performance and compatibility, and the results are shown in Table 2. The compressive strength of the cement slurry system without the addition of a fluid loss agent was 48.7 MPa, and the thickening time was 420 min.

[0093] The cement slurry formula is: 500g Jiahua G grade cement + 50% 200 mesh silica sand + 4% retarder + X% fluid loss reducer + water-cement ratio of 0.57.

[0094] Among them, the retarder is homemade in the laboratory and is a carboxylic acid retarder with a temperature resistance of up to 260°C.

[0095] Table 2 Effect of different fluid loss reducers on cement compressive strength and thickening time

[0096]

[0097]

[0098] From Table 2, it can be seen that the fluid loss reducers prepared in Examples 1-12 provided by the present invention have no obvious effect on the compressive properties and thickening time of cement slurry, and palygorskite can also participate in the strength development of cement paste, and increase the mechanical strength of cement paste to a certain extent. Compared with the comparative example, after the polymer is grafted on palygorskite, the adverse effect of the fluid loss reducer on other properties of cement slurry can be effectively reduced, and the performance requirements of cement slurry in ultra-high temperature environment can be guaranteed.

[0099] Test example 4:

[0100] For the provided ultra-high temperature fluid loss reducer Example 1 (dosage is 1% of the dry ash weight of cement) and Comparative Example 1 (dosage is 1% of the dry ash weight of cement), a cement slurry stability test was conducted in accordance with the national standard GB / T19139-2012 "Test Methods for Oil Well Cement", and the test temperature was 240°C. The sedimentation stability of Example 1 and Comparative Example 1 was compared with that of the cement sample without adding the fluid loss reducer. Figure 2 shown.

[0101] Depend on Figure 2 It can be seen that after treatment at 240°C, the density difference between the free liquid and cement paste of the sample without adding fluid loss agent is relatively large, while in Example 1, the free liquid amount is reduced from 11.3 mL to 1.5 mL, and the density difference between the upper and lower cement pastes is significantly reduced to 0.042 g / cm 3 It can be seen that the polymer grafted palygorskite provided by the present invention can effectively improve the sedimentation stability of cement slurry in an ultra-high temperature environment. Compared with the comparative example, after the introduction of palygorskite, due to the stability and rigidity of the particle nature, the overall temperature resistance of the polymer can be significantly improved, the polymer grid structure in the cement slurry is maintained, the viscosity of the cement slurry is maintained, and the sedimentation stability of the cement slurry in an ultra-high temperature environment is improved.

[0102] Although the embodiments disclosed in this application are as above, the contents described are only embodiments adopted to facilitate understanding of this application and are not intended to limit this application. Any technician in the field to which this application belongs can make any modifications and changes in the form and details of implementation without departing from the spirit and scope disclosed in this application, but the scope of patent protection of this application shall still be based on the scope defined in the attached claims.

Claims

1. A method for preparing an ultra-high temperature fluid loss reducer for cementing, comprising the following steps: (1) Surface modification of palygorskite Put a certain amount of palygorskite and hydrochloric acid into a three-necked flask equipped with a stirrer and a thermometer, wherein the palygorskite accounts for 1-10% of the total mass, and the concentration of hydrochloric acid is 1-4 mol / L. After heating to 50-80°C, stir for 1-2 hours to activate the surface hydroxyl groups of the palygorskite, take out the product, wash it with distilled water until it is neutral, and then grind it after drying. Disperse the activated product in toluene, wherein the mass fraction of palygorskite is 1-5%, add a certain amount of silane coupling agent KH570, react for 3-6 hours, wait for the reaction to end, filter the product by suction, wash it with anhydrous ethanol, and then dry it at 105°C and grind it to obtain the modified palygorskite; (2) Preparation of polymer-grafted palygorskite Add the modified palygorskite, nonionic water-soluble monomer, anionic water-soluble monomer and rigid monomer into a three-necked glass bottle equipped with a stirrer, a nitrogen tube and a thermometer, stir at high speed until all the raw materials are evenly dispersed, adjust the pH, pass nitrogen for 30 minutes, add persulfate, maintain a certain temperature, react for a period of time, dry and crush the product to obtain the desired target product; The nonionic water-soluble monomer is one of acrylamide, N,N-dimethylacrylamide, N-isopropylacrylamide and N-ethylacrylamide; The anionic water-soluble monomer is one of itaconic acid, acrylic acid, methacrylic acid, maleic acid, 2-acrylamido-2-methylpropanesulfonic acid, and sodium vinyl sulfonate; The rigid monomer is one of vinyl pyrrolidone, sodium p-styrene sulfonate, styrene and N-vinyl pyridine; The persulfate is one of potassium persulfate, sodium persulfate and ammonium persulfate.

2. The method for preparing the ultra-high temperature fluid loss additive for cementing according to claim 1, characterized in that: In step (1), the mesh number of palygorskite is 300 to 1000 meshes.

3. The method for preparing the ultra-high temperature fluid loss additive for cementing according to claim 1, characterized in that: In step (1), the mass ratio of palygorskite to KH570 is 1:(1-8).

4. The method for preparing the ultra-high temperature fluid loss additive for cementing according to claim 1, characterized in that: In step (2), the monomer accounts for 10-25% of the total mass, and the mass ratio of the modified palygorskite, the nonionic water-soluble monomer, the anionic water-soluble monomer and the rigid monomer is 1:(1-12):(2-8):(0-4).

5. The method for preparing the ultra-high temperature fluid loss additive for cementing according to claim 1, characterized in that: In step (2), the persulfate accounts for 0.5-1.5% of the total mass of the monomers.

6. The method for preparing the ultra-high temperature fluid loss additive for cementing according to claim 1, characterized in that: During the polymerization process in step (2), the pH is 5 to 9, the temperature is controlled at 50 to 65° C., and the polymerization reaction time is 3 to 6 hours.

Citation Information

Patent Citations

  • High-temperature-resistant and salt-resistant fluid loss agent and preparation method therefor

    CN105441040A

  • Inorganic-organic polymer oil well cement filtrate loss reduction additive, and preparation method and application thereof

    CN109503782A

  • Fluid loss agent and preparation method thereof

    CN112391153A

  • Temperature-resistant and salt-resistant fluid loss agent for well cementation as well as preparation method and application of temperature-resistant and salt-resistant fluid loss agent

    CN114835848A

  • Ultrahigh-temperature well cementation cement slurry fluid loss agent as well as preparation method and application thereof

    CN115725030A