Phase-change cooling organic reinforcing material as well as preparation formula and preparation method thereof

By adding small-particle-size powdered phase change material EAA and calcium oxide to organic reinforcement materials, combined with catalysts and flame retardants, the high-temperature problem during the reaction of organic reinforcement materials was solved, achieving temperature control and strength improvement, and reducing the risk of spontaneous combustion of coal seams.

CN118978662APending Publication Date: 2024-11-19SHANXI JUYI NEW BUILDING MATERIALS TECH RES INST
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411082137.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-08
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

Existing organic polymer polyurethane reinforcement materials release a large amount of heat during the reaction, which increases the risk of spontaneous combustion of coal seams, and traditional reinforcement materials are difficult to effectively reduce the reaction temperature.

Method used

The formulation of phase change cooling organic reinforcement material is adopted. By uniformly dispersing small-particle-size powdered phase change material EAA and reinforcing agent calcium oxide in component A, the reaction temperature is reduced by the endothermic melting of EAA, and the reaction rate is reduced by the synergistic catalysis of catalyst and flame retardant, thereby enhancing the strength of the material.

Benefits of technology

It effectively absorbs the heat of reaction, reduces the reaction temperature to below 100℃, and ensures that coal seam grouting reinforcement improves the strength and density of the material while reducing the risk of spontaneous combustion.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention aims to provide a phase-change cooling organic reinforcing material as well as a preparation formula and a preparation method thereof. The invention firstly provides a preparation formula of the phase-change cooling organic reinforcing material. The invention further provides a preparation method of the phase-change cooling organic reinforcing material, and the preparation method comprises the following steps: 1) while stirring, sequentially adding the polyether polyol, the catalyst, the phase-change material and the reinforcing agent into a mixing kettle A in parts by weight, and uniformly stirring at normal temperature; 2) vacuumizing and defoaming the mixing kettle A, barreling and sealing to obtain a component A; 3) under stirring, sequentially adding the isocyanate and the flame retardant into a mixing kettle B in parts by weight, and uniformly stirring at normal temperature; 4) vacuumizing and defoaming the mixing kettle B, barreling and sealing to obtain a component B; and 5) mixing the component A and the component B according to a weight ratio of 1: 1 to prepare the phase-change cooling organic reinforcing material. According to the invention, heat released by reaction can be effectively absorbed, the temperature during reaction is reduced, and effective grouting reinforcement of the coal seam is realized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of coal mine reinforcement materials, and in particular to a phase change cooling organic reinforcement material and a preparation formula and a preparation method thereof. Background Art

[0002] During the coal mining process, coal mines are often troubled by dangerous accidents such as roof falls and slab spalling caused by fault fracture zones and unstable strata, which not only affect the coal mining efficiency of coal mines, but more importantly, the lives of miners are always threatened. Therefore, reinforcement materials are generally used for grouting reinforcement during the coal mining process. Currently, the most widely used are organic polymer polyurethane reinforcement materials and silicate modified polyurethane reinforcement materials. One of the main disadvantages of organic polymer polyurethane reinforcement materials is the large reaction exotherm. The reaction temperature can usually exceed 120°C, or even as high as more than 140 degrees Celsius, releasing a large amount of heat in the coal seam. The continuous accumulation of heat will increase the risk of spontaneous combustion of the coal seam. Therefore, how to reduce the temperature of the organic reinforcement material during the reaction is a technical difficulty.

[0003] The present invention attempts to provide a phase-change cooling organic reinforcement material and a preparation formula and method thereof, which can effectively absorb reaction heat, reduce the temperature during the reaction, and achieve effective grouting reinforcement for coal seams. Summary of the invention

[0004] The present invention attempts to provide a phase-change cooling organic reinforcement material and a preparation formula and method thereof, which can effectively absorb reaction heat, reduce the temperature during the reaction, and achieve effective grouting reinforcement for coal seams.

[0005] The first aspect of the present invention provides a preparation formula of a phase change cooling organic reinforcement material, the preparation formula comprises component A and component B, wherein component A comprises polyether polyol, phase change material, reinforcing agent and catalyst, and component B comprises isocyanate and flame retardant.

[0006] Furthermore, component A includes, by weight, 90-92 parts of polyether polyol, 5-8 parts of phase change material, 0.3-0.4 parts of reinforcing agent and 0.75-1.0 parts of catalyst; component B includes, by weight, 73-75 parts of isocyanate and 25-27 parts of flame retardant.

[0007] Furthermore, the polyether polyol is prepared by mixing polyether polyol A and polyether polyol B in a weight ratio of 3:1, wherein polyether polyol A has a hydroxyl value (mgKOH / g) of 330-340 and an average molecular weight of 500, and polyether polyol B has a hydroxyl value (mgKOH / g) of 165-170 and an average molecular weight of 1000.

[0008] Furthermore, the phase change material is ethylene acrylic acid copolymer (EAA), which has a melting point of 85-90° C. and a fineness of more than 400 meshes.

[0009] Furthermore, the reinforcing agent is calcium oxide, and the fineness is ≥2000 mesh.

[0010] Furthermore, the catalyst comprises dibutyltin dilaurate and N,N-dimethylbenzylamine, and component A comprises 0.15 to 0.20 parts of dibutyltin dilaurate and 0.6 to 0.8 parts of N,N-dimethylbenzylamine by weight.

[0011] Furthermore, the isocyanate is polymethylene polyphenyl polyisocyanate (PAPI), and the flame retardant is trichloroethyl phosphate (TCEP).

[0012] The second aspect of the present invention provides a preparation method of a phase-change cooling organic reinforcement material, which uses the preparation formula of the phase-change cooling organic reinforcement material according to the first aspect, and is characterized in that the preparation method comprises the following steps: 1) adding polyether polyol, catalyst, phase change material and reinforcing agent to a mixing kettle A in parts by weight under stirring, and stirring evenly at room temperature; 2) vacuuming and degassing the mixing kettle A, and sealing the barrel to obtain component A; 3) adding isocyanate and flame retardant to a mixing kettle B in parts by weight under stirring, and stirring evenly at room temperature; 4) vacuuming and degassing the mixing kettle B, and sealing the barrel to obtain component B; 5) mixing component A and component B in a ratio of 1:1 by weight to obtain the phase-change cooling organic reinforcement material.

[0013] The third aspect of the present invention provides a phase-change cooling organic reinforcement material, which is prepared by using the preparation method of the phase-change cooling organic reinforcement material according to the second aspect.

[0014] The present invention coordinates the intensity of the reaction between the hydroxyl group and the isocyanate group by combining high (330-340) and low (165-170) hydroxyl value and different molecular weight polyether polyols, thereby ensuring the strength and reducing the temperature during the reaction; by adding small-particle powder phase change material EAA to make it uniformly dispersed in component A, when the polyether polyol and isocyanate react and release heat to reach the EAA phase change temperature, it absorbs heat and melts, slowing down the heating rate of the system and reducing the temperature during the reaction.

[0015] Compared with the prior art, the advantages of the present invention are:

[0016] (1) The small-particle powder phase change material EAA is innovatively evenly dispersed in component A. When the exothermic reaction of polyether polyol and isocyanate reaches the EAA phase change temperature, EAA absorbs heat and melts, slowing down the heating rate of the system and reducing the reaction temperature. (2) Calcium oxide is innovatively dispersed in component A to absorb the carbon dioxide gas produced by the side reaction, eliminate pores, make the solid body dense, and increase its strength. DETAILED DESCRIPTION

[0017] In order to provide a further understanding of the purpose, structure, features, and functions of the present invention, the following detailed description is given in conjunction with the embodiments.

[0018] The first aspect of the present invention provides a preparation formula of a phase change cooling organic reinforcement material, the preparation formula comprises component A and component B, wherein component A comprises polyether polyol, phase change material, reinforcing agent and catalyst, and component B comprises isocyanate and flame retardant. Component A comprises: by weight, 90-92 parts of polyether polyol, 5-8 parts of phase change material, 0.3-0.4 parts of reinforcing agent and 0.75-1.0 parts of catalyst; component B comprises: by weight, 73-75 parts of isocyanate and 25-27 parts of flame retardant.

[0019] The polyether polyol is prepared by mixing polyether polyol A and polyether polyol B in a weight ratio of 3:1, wherein polyether polyol A has a hydroxyl value (mgKOH / g) of 330-340 and an average molecular weight of 500, and polyether polyol B has a hydroxyl value (mgKOH / g) of 165-170 and an average molecular weight of 1000. By combining high (330-340) and low (165-170) hydroxyl value and different molecular weight polyether polyols, the intensity of the reaction between the hydroxyl group and the isocyanate group is balanced, which ensures the strength and reduces the temperature during the reaction.

[0020] The phase change material is ethylene acrylic acid copolymer (EAA), which has a melting point of 85-90°C and a fineness of >400 mesh. Small-particle powder phase change material EAA is added to be evenly dispersed in component A. When the exothermic reaction of polyether polyol and isocyanate reaches the EAA phase change temperature, EAA absorbs heat and melts, slowing down the system heating rate and reducing the temperature during the reaction; at the same time, the carboxylic acid group exposed after EAA melts can react with isocyanate to enhance the strength.

[0021] The reinforcing agent is calcium oxide, with a fineness of ≥2000 mesh. A small amount of water is inevitably present in organic reinforcing materials, and the carbon dioxide gas produced by the side reaction causes pores in the solid body, and in severe cases even causes expansion, which significantly reduces the strength of the solid body. The reinforcing agent calcium oxide can absorb carbon dioxide, eliminate pores, make the solid body dense, and increase its strength.

[0022] The catalyst includes dibutyltin dilaurate and N,N-dimethylbenzylamine, and component A includes 0.15-0.20 parts of dibutyltin dilaurate and 0.6-0.8 parts of N,N-dimethylbenzylamine by weight. The catalyst dibutyltin dilaurate and N,N-dimethylbenzylamine synergistically catalyze, which has the effect of easing the reaction, reducing the reaction exothermic rate, and lowering the temperature during the reaction.

[0023] The isocyanate is polymethylene polyphenyl polyisocyanate (PAPI), and the flame retardant is trichloroethyl phosphate (TCEP). The flame retardant TCEP has flame retardant and cooling effects.

[0024] The second aspect of the present invention provides a method for preparing a phase-change cooling organic reinforcement material. The preparation method uses the preparation formula of the phase-change cooling organic reinforcement material according to the first aspect of the embodiment, and the preparation method comprises the following steps: 1) adding polyether polyol, catalyst, phase change material and reinforcing agent to mixing kettle A in parts by weight under stirring, and stirring evenly at room temperature; 2) vacuuming and degassing the mixing kettle A, and sealing the barrel to obtain component A; 3) adding isocyanate and flame retardant to mixing kettle B in parts by weight under stirring, and stirring evenly at room temperature; 4) vacuuming and degassing the mixing kettle B, and sealing the barrel to obtain component B; 5) mixing component A and component B in a ratio of 1:1 by weight to obtain the phase-change cooling organic reinforcement material.

[0025] The third aspect of the present invention provides a phase-change cooling organic reinforcement material, which is prepared by using the preparation method of the phase-change cooling organic reinforcement material according to the second aspect of the present invention.

[0026] The embodiment of the present invention coordinates the intensity of the reaction between hydroxyl and isocyanate by combining high (330-340) and low (165-170) hydroxyl value and different molecular weight polyether polyols, thereby ensuring strength and reducing the reaction temperature. By adding small-particle powder phase change material EAA to evenly disperse it in component A, when the exothermic reaction of polyether polyol and isocyanate reaches the EAA phase change temperature, EAA absorbs heat and melts, slowing down the heating rate of the system and reducing the reaction temperature. At the same time, the carboxylic acid group exposed after EAA melts can react with isocyanate to enhance the strength. A small amount of moisture is inevitably present in the organic reinforcement material, and the carbon dioxide gas produced by the side reaction causes pores in the solid body, and even causes expansion in severe cases, which significantly reduces the strength of the solid body. The reinforcing agent calcium oxide can absorb carbon dioxide, eliminate pores, make the solid body dense, and increase its strength. The catalyst dibutyltin dilaurate and N,N-dimethylbenzylamine synergistically catalyze and have the effect of reducing the reaction temperature. The flame retardant TCEP has flame retardant and cooling effects.

[0027] The present invention innovatively disperses the small-particle powder phase change material EAA evenly in component A. When the polyether polyol and isocyanate react to release heat and reach the EAA phase change temperature, EAA absorbs heat and melts, slowing down the temperature rise rate of the system and reducing the reaction temperature. Calcium oxide is innovatively dispersed in component A to absorb carbon dioxide gas produced by the side reaction, eliminate pores, make the solid body dense, and increase its strength. Specific embodiments

[0029] Embodiment 1:

[0030] Component A: 90 parts of polyether polyol; 8 parts of phase change material; 0.3 parts of reinforcing agent; 0.15 parts of dibutyltin dilaurate; and 0.8 parts of N,N-dimethylbenzylamine.

[0031] Component B: 73 parts of isocyanate; 27 parts of flame retardant.

[0032] The polyether polyol is a mixture of polyether polyol A and polyether polyol B in a weight ratio of 3:1, polyether polyol A is a polyether polyol with a hydroxyl value (mgKOH / g) of 330-340 and an average molecular weight of 500, and polyether polyol B is a polyether polyol with a hydroxyl value (mgKOH / g) of 165-170 and an average molecular weight of 1000. The phase change material is ethylene acrylic acid copolymer (EAA), which has a melting point of 85-90°C and a fineness of >400 mesh. The reinforcing agent is calcium oxide with a fineness of ≥2000 mesh. The isocyanate is polymethylene polyphenyl polyisocyanate (PAPI), and the flame retardant is trichloroethyl phosphate (TCEP).

[0033] Preparation method:

[0034] 1) Add polyether polyol, catalyst, phase change material and reinforcing agent to a mixing kettle A in order by weight under stirring, and stir evenly at room temperature;

[0035] 2) Vacuum the mixing kettle A to degas, and seal the barrel to obtain component A;

[0036] 3) Add isocyanate and flame retardant to mixing kettle B in order by weight under stirring, and stir evenly at room temperature;

[0037] 4) Vacuum the mixing kettle B to degas, and seal the barrel to obtain component B;

[0038] 5) Component A and component B are mixed in a weight ratio of 1:1 to obtain the phase change cooling organic reinforcement material.

[0039] Embodiment 2:

[0040] Component A: 91 parts of polyether polyol; 7 parts of phase change material; 0.4 parts of reinforcing agent; 0.18 parts of dibutyltin dilaurate; and 0.7 parts of N,N-dimethylbenzylamine.

[0041] Component B: 74 parts of isocyanate; 26 parts of flame retardant.

[0042] The polyether polyol is a mixture of polyether polyol A and polyether polyol B in a weight ratio of 3:1, polyether polyol A is a polyether polyol with a hydroxyl value (mgKOH / g) of 330-340 and an average molecular weight of 500, and polyether polyol B is a polyether polyol with a hydroxyl value (mgKOH / g) of 165-170 and an average molecular weight of 1000. The phase change material is ethylene acrylic acid copolymer (EAA), which has a melting point of 85-90°C and a fineness of >400 mesh. The reinforcing agent is calcium oxide with a fineness of ≥2000 mesh. The isocyanate is polymethylene polyphenyl polyisocyanate (PAPI), and the flame retardant is trichloroethyl phosphate (TCEP).

[0043] Preparation method:

[0044] 1) Add polyether polyol, catalyst, phase change material and reinforcing agent to a mixing kettle A in order by weight under stirring, and stir evenly at room temperature;

[0045] 2) Vacuum the mixing kettle A to degas, and seal the barrel to obtain component A;

[0046] 3) Add isocyanate and flame retardant to mixing kettle B in order by weight under stirring, and stir evenly at room temperature;

[0047] 4) Vacuum the mixing kettle B to degas, and seal the barrel to obtain component B;

[0048] 5) Component A and component B are mixed in a weight ratio of 1:1 to obtain the phase change cooling organic reinforcement material.

[0049] Embodiment 3:

[0050] Component A: 92 parts of polyether polyol; 5 parts of phase change material; 0.3 parts of reinforcing agent; 0.20 parts of dibutyltin dilaurate; and 0.6 parts of N,N-dimethylbenzylamine.

[0051] Component B: 75 parts of isocyanate; 25 parts of flame retardant.

[0052] The polyether polyol is a mixture of polyether polyol A and polyether polyol B in a weight ratio of 3:1, polyether polyol A is a polyether polyol with a hydroxyl value (mgKOH / g) of 330-340 and an average molecular weight of 500, and polyether polyol B is a polyether polyol with a hydroxyl value (mgKOH / g) of 165-170 and an average molecular weight of 1000. The phase change material is ethylene acrylic acid copolymer (EAA), which has a melting point of 85-90°C and a fineness of >400 mesh. The reinforcing agent is calcium oxide with a fineness of ≥2000 mesh. The isocyanate is polymethylene polyphenyl polyisocyanate (PAPI), and the flame retardant is trichloroethyl phosphate (TCEP).

[0053] Preparation method:

[0054] 1) Add polyether polyol, catalyst, phase change material and reinforcing agent to a mixing kettle A in order by weight under stirring, and stir evenly at room temperature;

[0055] 2) Vacuum the mixing kettle A to degas, and seal the barrel to obtain component A;

[0056] 3) Add isocyanate and flame retardant to mixing kettle B in order by weight under stirring, and stir evenly at room temperature;

[0057] 4) Vacuum the mixing kettle B to degas, and seal the barrel to obtain component B;

[0058] 5) Component A and component B are mixed in a weight ratio of 1:1 to obtain the phase change cooling organic reinforcement material.

[0059] Phase change cooling organic reinforcement material performance test

[0060] project Maximum temperature during reaction / ℃ Compressive strength / MPa AQ / T1089-2020 ≤100 ≥40 Example 1 94.8 46 Example 2 95.5 48 Example 3 96.1 49

[0061] AQ / T 1089-2020 is the national standard for polymer materials used to reinforce coal and rock mass in coal mines. From the above data, it can be seen that the three embodiments can meet the standard requirements.

[0062] The embodiments described above are only specific embodiments of the technical solutions of the present invention and are not intended to limit the present invention. Any modifications, supplements or similar substitutions made within the scope of the principles of the present invention should be included in the protection scope of the present invention.

[0063] In the description of the present invention, it should be understood that the terms "longitudinal", "lateral", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside" and "outside" orientations or positional relationships are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the referred device or element must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as limiting the present invention.

[0064] The present invention has been described by the above-mentioned relevant embodiments, however, the above-mentioned embodiments are only examples for implementing the present invention. It must be pointed out that the disclosed embodiments do not limit the scope of the present invention. On the contrary, changes and modifications made without departing from the spirit and scope of the present invention are all within the scope of patent protection of the present invention.

Claims

1. A preparation formula for phase change cooling organic reinforcement material, It is characterized in that The preparation formula comprises component A and component B, wherein component A comprises polyether polyol, phase change material, reinforcing agent and catalyst, and component B comprises isocyanate and flame retardant.

2. The preparation formula of the phase change cooling organic reinforcement material according to claim 1, It is characterized in that Component A includes: by weight, 90-92 parts of polyether polyol, 5-8 parts of phase change material, 0.3-0.4 parts of reinforcing agent and 0.75-1.0 parts of catalyst; Component B comprises: by weight, 73-75 parts of isocyanate and 25-27 parts of flame retardant.

3. The preparation formula of the phase change cooling organic reinforcement material according to claim 2, It is characterized in that The polyether polyol is prepared by mixing polyether polyol A and polyether polyol B in a weight ratio of 3:1, wherein polyether polyol A has a hydroxyl value (mgKOH / g) of 330-340 and an average molecular weight of 500, and polyether polyol B has a hydroxyl value (mgKOH / g) of 165-170 and an average molecular weight of 1000.

4. The preparation formula of the phase change cooling organic reinforcement material according to claim 3, It is characterized in that The phase change material is ethylene acrylic acid copolymer (EAA), which has a melting point of 85-90° C. and a fineness of more than 400 meshes.

5. The preparation formula of the phase change cooling organic reinforcement material according to claim 4, It is characterized in that The reinforcing agent is calcium oxide, and the fineness is ≥2000 mesh.

6. The preparation formula of the phase change cooling organic reinforcement material according to claim 5, It is characterized in that The catalyst comprises dibutyltin dilaurate and N,N-dimethylbenzylamine. Component A comprises 0.15-0.20 parts of dibutyltin dilaurate and 0.6-0.8 parts of N,N-dimethylbenzylamine by weight.

7. The preparation formula of the phase change cooling organic reinforcement material according to claim 6, It is characterized in that The isocyanate is polymethylene polyphenyl polyisocyanate (PAPI), and the flame retardant is trichloroethyl phosphate (TCEP).

8. A method for preparing a phase-change cooling organic reinforcement material, the method using the preparation formula of the phase-change cooling organic reinforcement material according to claim 7, It is characterized in that The preparation method comprises the following steps: 1) Add polyether polyol, catalyst, phase change material and reinforcing agent to a mixing kettle A in order by weight under stirring, and stir evenly at room temperature; 2) Vacuum the mixing kettle A to degas, and seal the barrel to obtain component A; 3) Add isocyanate and flame retardant to mixing kettle B in order by weight under stirring, and stir evenly at room temperature; 4) Vacuum the mixing kettle B to degas, and seal the barrel to obtain component B; 5) Component A and component B are mixed in a weight ratio of 1:1 to obtain the phase change cooling organic reinforcement material.

9. A phase change cooling organic reinforcement material, It is characterized in that It is prepared by using the preparation method of the variable temperature organic reinforcement material according to claim 8.

Citation Information

Cited By

  • Polyurethane composition and composite material containing same

    CN119591827A